Thermosetting resin composition, sealing agent for display device, and display device

By introducing a compound of a specific structure and a heat curing agent into the thermosetting resin composition, the flexibility and moisture resistance of the sealant are improved, and the problem of peeling the sealant under stress is solved, thereby achieving effective sealing of the display device.

CN118922465APending Publication Date: 2024-11-08MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029794.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing thermosetting resin sealant used in display devices is insufficient in softness when stress is applied, resulting in the problem of peeling the sealant from the substrate being unable to be effectively solved.

Method used

A thermosetting resin composition containing compound (A) is used, which has a total of two or more glycidyl and oxetyl functional groups, and the molecular motility and cross-linking density are improved by the structure of the general formula (1), and combined with heat The curing agent (B) is used to adjust the viscosity and moisture resistance to form a sealant with high flexibility and moisture resistance.

Benefits of technology

Effectively inhibit the peeling of the sealant when stress is applied, improves the stability and sealing performance of the display device, and ensures the stable existence of the sealant between the substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922465A_ABST
    Figure CN118922465A_ABST
Patent Text Reader

Abstract

The present invention relates to a thermosetting resin composition comprising: a compound (A) having a total of two or more functional groups of a glycidyl group and / or an oxetanyl group, and having a skeleton represented by general formula (1); and a thermosetting agent (B). The viscosity of the thermosetting resin composition measured by an E-type viscometer at 25 DEG C and 2.5 rpm is 20.0 Pa.s or less. In general formula (1), a represents an integer of 0 to 8, b represents an integer of 0 to 3, c represents an integer of 0 to 8, d represents an integer of 0 to 8, at least one of a, b and c is 1 or more, n is an integer of 1 or more, and * represents a bonding position. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermosetting resin composition, a sealant for a display device, and a display device. Background Art

[0002] In recent years, liquid crystal display devices, organic EL display devices, electrophoretic display devices, and the like have been put into practical use as display devices for various electronic devices.

[0003] For example, a liquid crystal display device includes two transparent substrates with electrodes provided on the surface, a frame-shaped sealant sandwiched between the substrates, and a liquid crystal material sealed in a region surrounded by the sealant. As a sealant for sealing the liquid crystal, for example, Patent Document 1 discloses a thermosetting resin composition (liquid crystal sealant) containing an epoxy resin and an epoxy resin curing agent.

[0004] On the other hand, as an electrophoretic display device, a display device having a microcup structure is proposed, for example, as in Patent Document 2. In the electrophoretic display device, a display element is disposed between a pair of substrates and sealed by applying a sealant.

[0005] For such an electrophoretic display device, for example, Patent Document 3 describes that a sealant containing epoxy resin or the like can be used.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-018022

[0009] Patent Document 2: Japanese Patent Application Publication No. 2004-536332

[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-142549 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Thus, sealants for various display devices are known. The cured product of the thermosetting resin composition contained in the sealant is required to have high flexibility so as to relieve the stress when external stress is applied to the display device. If the softness of the cured product is low, for example, when the display device is installed in a tablet computer terminal, the sealant cannot relieve the stress applied to the display device, and there is a problem of peeling from the substrate.

[0013] According to the research conducted by the present inventors, the sealants containing the thermosetting resin composition described in Patent Documents 1 and 3 do not improve the flexibility of the cured product and cannot suppress the sealant from peeling when stress is applied to the display device.

[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a thermosetting resin composition, a sealant for a display device, and a display device that can suppress separation of a sealant from a substrate when stress is applied to the display device.

[0015] Means for solving problems

[0016] The present invention relates to the following thermosetting resin composition, sealant for display device, and display device.

[0017] The thermosetting resin composition of the present invention comprises: a compound (A) having a total of two or more functional groups of at least one of a glycidyl group and an oxetane group and having a structure represented by the general formula (1); and a thermosetting agent (B), wherein the viscosity of the thermosetting resin composition measured by an E-type viscometer at 25° C. and 2.5 rpm is not more than 20.0 Pa·s.

[0018] [Chemistry 1]

[0019]

[0020] In the general formula (1), a represents an integer of 0 to 8, b represents an integer of 0 to 3, c represents an integer of 0 to 8, d represents an integer of 0 to 8, at least one of a, b and c is 1 or more, n is an integer of 1 or more, and * represents a bonding position. When the compound (A) has a plurality of structures represented by the general formula (1), the numbers of a, b, c, d and n in each structure may be the same or different.

[0021] The sealant for a display device of the present invention contains the above-mentioned thermosetting resin composition.

[0022] The display device of the present invention comprises a protective member, a substrate having an image display portion, and the above-mentioned sealant for a display device disposed between the protective member and the substrate.

[0023] Effects of the Invention

[0024] According to the present invention, a thermosetting resin composition capable of suppressing separation of a sealant from a substrate when stress is applied to a display device, a sealant including the thermosetting resin composition, and a display device can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram showing the structure of a display device according to one embodiment of the present invention. DETAILED DESCRIPTION

[0026] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0027] 1. Thermosetting resin composition

[0028] The thermosetting resin composition of the present invention comprises: a compound (A) having a total of two or more glycidyl groups and at least one of oxetane functional groups and having a structure represented by the general formula (1); and a thermosetting agent (B), wherein the viscosity of the thermosetting resin composition measured by an E-type viscometer at 25° C. and 2.5 rpm is not more than 20.0 Pa·s.

[0029] [Chemistry 2]

[0030]

[0031] In the general formula (1), a represents an integer greater than or equal to 0 and less than or equal to 8, b represents an integer greater than or equal to 0 and less than or equal to 3, c represents an integer greater than or equal to 0 and less than or equal to 8, d represents an integer greater than or equal to 0 and less than or equal to 8, at least one of a, b and c is greater than or equal to 1, n is an integer greater than or equal to 1, and * represents a bonding position.

[0032] As described above, in the conventional sealant made of a thermosetting resin composition, the flexibility of the cured product has not been improved, and there has been a problem that the sealant is peeled off from the substrate when stress is applied to the display device.

[0033] In contrast, the present inventors have conducted intensive research and found that the above-mentioned peeling can be made less likely to occur by including a compound (A), i.e., a compound having a structure represented by the above-mentioned general formula (1) and having a total of two or more glycidyl groups and at least one of oxetane functional groups, in a thermosetting resin composition. Although the reason for this is not yet clear, it is considered to be as follows.

[0034] It is believed that the structure represented by the general formula (1) is a soft structure that can improve molecular mobility. Therefore, it is believed that by including a compound (A) having the structure in a thermosetting resin composition, the flexibility of the cured product is improved. In addition, the cured product of the thermosetting resin composition can be obtained by crosslinking the compound contained in the composition in the presence of a thermosetting agent. At this time, the compound has a skeleton represented by the general formula (1), so that the distance between the crosslinking points of the compounds can be extended, so it is believed that the crosslinking density becomes low. Thus, it is also believed that the flexibility of the cured product will be improved. In addition, by improving the flexibility of the cured product, even if the stress such as the sealant peeling is applied to the display device, the above-mentioned stress can be dispersed to the entire cured product and relieved, so it is believed that the peeling of the sealant can be suppressed.

[0035] 1-1. Compound (A)

[0036] The compound (A) in the present invention has a total of two or more functional groups of at least one of a glycidyl group and an oxetanyl group, and has a structure represented by the above general formula (1).

[0037] The compound (A) may be a compound having a total of two or more functional groups of at least one of a glycidyl group and an oxetanyl group, and preferably has two or more glycidyl groups. Specifically, the compound (A) is preferably a polyfunctional epoxy compound.

[0038] The total number of glycidyl groups and oxetanyl groups contained in one molecule of the compound (A) may be two or more, and is preferably two from the viewpoint of suppressing a decrease in flexibility of the cured product due to an increase in crosslinking density.

[0039] In the above general formula (1), a represents an integer of 0 to 8, b represents an integer of 0 to 3, c represents an integer of 0 to 8, d represents an integer of 0 to 8, at least one of a, b and d is 1 or more, and n is an integer of 1 or more. Among them, with respect to compound (A), in the above general formula (1), the value of a+b+c+d is preferably 1 to 10, more preferably 2 to 5. The more the number of carbon atoms in the structure represented by the general formula (1) is increased, the more the crosslinking points and the softness of the cured product can be improved. On the other hand, by reducing the number of carbon atoms in the structure represented by the general formula (1), the decrease in moisture resistance of the cured product caused by the elongation of the distance between the crosslinking points can be suppressed, and the increase in the molecular weight of the compound (A) can be suppressed, and the viscosity of the composition can be easily adjusted to a suitable range. More specifically, it preferably satisfies (a=3, b=0, c=0, d=0), (a=1, b=1, c=0, d=0) or (a=0, b=1, c=0, d=1), and more preferably satisfies (a=3, b=0, c=0, d=0). In addition, compound (A) is preferably a bifunctional epoxy compound that satisfies these conditions.

[0040] In the above general formula (1), n ​​is an integer greater than or equal to 1, preferably greater than or equal to 1 and less than or equal to 10, more preferably greater than or equal to 3 and less than or equal to 7, and further preferably greater than or equal to 3 and less than or equal to 5. When n is less than or equal to 10, the molecular weight of the compound (A) can be appropriately adjusted to make it easier to adjust the viscosity of the thermosetting resin composition within the above range. In addition, when n is less than or equal to 5, the moisture resistance of the cured product can be easily maintained.

[0041] Compound (A) may have only one structure represented by the general formula (1) in the skeleton, or may have multiple structures represented by the general formula (1) in which the values ​​of a, b, c, d and n are the same or different. In addition, multiple structures represented by the general formula (1) with different values ​​of a, b, c and d may be continuous. When compound (A) has structures represented by the general formula (1) at multiple positions, the numbers of a, b, c, d and n in each structure may be the same or different.

[0042] In addition, compound (A) may further have other structures other than the structure represented by general formula (1). Examples of the above-mentioned other structures include the structure represented by the following general formula (2), the structure represented by the general formula (3), etc. Among them, from the viewpoint of further improving the moisture resistance of the cured product, the structure represented by the following general formula (2) is preferred.

[0043] [Chemistry 3]

[0044]

[0045] [Chemistry 4]

[0046]

[0047] In the general formula (2) and the general formula (3), R1 is a single bond, an alkylene group having 1 to 4 carbon atoms, an alkylidene group having 2 to 4 carbon atoms, a sulfonyl group, an oxygen atom and a sulfur atom; R2 is a hydrogen atom or an alkylene group having 1 to 4 carbon atoms; m is an integer of 1 to 4; and * represents a bonding position.

[0048] According to the knowledge of the inventors, in conventional sealants, when a thermosetting resin composition includes a compound having a structure represented by the general formula (2), moisture resistance can be improved, but on the other hand, the flexibility of the cured product cannot be improved, and thus peeling of the sealant cannot be suppressed when stress is applied to the display device. On the other hand, even if the compound (A) included in the thermosetting resin composition of the present invention includes a structure represented by the general formula (2) in order to improve moisture resistance, since it has a structure represented by the general formula (1), it can improve the flexibility of the cured product and suppress peeling of the sealant when stress is applied to the display device.

[0049] In the general formula (2), R1 is preferably an alkylene group having 1 to 4 carbon atoms or an alkylidene group having 2 to 4 carbon atoms, and more preferably an alkylidene group having 2 to 4 carbon atoms.

[0050] Examples of the alkylene group having 1 to 4 carbon atoms include methylene, ethylene, propylene, butylene, and isobutylene.

[0051] Examples of the alkylidene group having 2 to 4 carbon atoms include methylene (methylidene), ethylidene, propylidene, isopropylidene, butylidene, isobutylidene, etc. Among them, isopropylidene is preferred.

[0052] In the general formula (2), R2 is a hydrogen atom or an alkylene group having 1 to 4 carbon atoms, and m is an integer of 1 to 4. A plurality of R2 may be the same or different, and preferably all are hydrogen atoms. In addition, m is preferably 1.

[0053] When R2 is an alkylene group having 1 to 4 carbon atoms, the carbon number is preferably 2 to 4.

[0054] Compound (A) may have only one structure represented by general formula (2), or R1 and R2 may have multiple structures represented by general formula (2) that are the same or different. When compound (A) has structures represented by general formula (2) at multiple positions, R1 and R2 in each structure may be the same or different.

[0055] It should be noted that in the general formula (2), when R1 is a single bond, the general formula (2) becomes a biphenyl structure. In this case, in the present specification, a compound having a total of two or more glycidyl groups and at least one of oxetanyl groups and having a structure represented by the general formula (1) and a biphenyl structure is referred to as compound (A).

[0056] R1, R2 and m in the general formula (3) can be the same as those in the general formula (2), and thus detailed description thereof will be omitted.

[0057] The compound (A) may be in a solid state at room temperature, but is preferably in a liquid state from the viewpoint of easily adjusting the viscosity of the thermosetting resin composition to the above range.

[0058] When compound (A) is an epoxy compound, the epoxy equivalent of compound (A) is preferably 300 g / eq or more, more preferably 350 g / eq or more, more preferably 350 g / eq or more and 750 g / eq or less, and further preferably 350 g / eq or more and 500 g / eq or less. If the epoxy equivalent is 300 g / eq or more, the flexibility of the cured product can be further improved. In addition, by having an epoxy equivalent of 750 g / eq or less, moisture resistance can be more easily maintained. The above-mentioned epoxy equivalent can be measured by a method in accordance with JIS K7236:2009.

[0059] Regarding compound (A), the glass transition temperature (Tg) of the cured product obtained by the following method is preferably 100°C or less, more preferably 80°C or less, and further preferably 70°C or less. If the glass transition temperature is 100°C or less, the flexibility of the cured product can be further improved. The lower limit of the glass transition temperature is not particularly limited, and is, for example, 0°C or more.

[0060] The cured product of the compound (A) can be obtained by mixing 100 parts by mass of the compound (A), a chemically equivalent amount of methylhexahydrophthalic anhydride to 100 parts by mass of the compound (A), and 1 part by mass of dimethylbenzylamine, heating the mixture at 110° C. for 3 hours, and then heating the mixture at 165° C. for 2 hours.

[0061] The glass transition temperature can be measured, for example, using a dynamic viscoelasticity measurement (DMA: Dynamic Mechanical Analysis) apparatus (DMS7100, manufactured by Hitachi High-Tech Science Co., Ltd.).

[0062] Examples of commercially available products of the compound (A) include EP-4010S and EP-4010L (both manufactured by ADEKA Corporation), etc. The thermosetting resin composition may contain only one type of the compound (A), or may contain two or more types of the compound (A).

[0063] Relative to the gross mass of the thermosetting resin composition, the content of compound (A) is preferably 1.5% by mass or more and 20% by mass or less, more preferably 2.5% by mass or more and 15% by mass or less. If the above content is more than 1.5% by mass, the flexibility of the thermosetting resin composition can be further improved. Thus, even if stress is applied to the display device, it is possible to further suppress the sealant from peeling off the substrate. In addition, if the above content is less than 20% by mass, it is easier to adjust the viscosity of the thermosetting resin composition to the above range.

[0064] 1-2. Compounds having a biphenyl structure (a)

[0065] The thermosetting resin composition of the present invention may further include a compound (a) having a functional group of at least one of a glycidyl group and an oxetanyl group, and a biphenyl structure. By including the compound (a) in the thermosetting resin composition, the moisture resistance of the thermosetting resin composition is further improved by the biphenyl structure of the compound (a). Furthermore, by including the compound (a), the viscosity of the thermosetting resin composition can be further reduced and easily adjusted to the above range.

[0066] According to the findings of the present inventors, in conventional sealants, when a compound (a) having a biphenyl structure is included in a thermosetting resin composition, moisture resistance can be improved, but on the other hand, the flexibility of the cured product cannot be improved, and peeling of the sealant cannot be suppressed when stress is applied to the display device. In contrast, the compound (A) included in the thermosetting resin composition of the present invention includes a compound (a) having a biphenyl structure in order to improve moisture resistance, but since it has a structure represented by the general formula (1), it can improve the flexibility of the cured product and suppress peeling of the sealant when stress is applied to the display device.

[0067] It should be noted that, as described above, in this specification, a compound having a functional group of at least one of a glycidyl group and an oxetanyl group and a biphenyl structure and further having a structure represented by the general formula (1) is compound (A). That is, compound (a) does not include a compound having a structure represented by the general formula (1).

[0068] The compound (a) may be a compound having at least one of a glycidyl group and an oxetanyl group and a biphenyl structure, and preferably has a glycidyl group among the functional groups. Specifically, the compound (a) is preferably an epoxy compound having a biphenyl structure.

[0069] The number of glycidyl groups and oxetanyl groups contained in one molecule of the compound (a) is preferably 1.

[0070] The compound (a) may be in a solid state at room temperature, but is preferably in a liquid state from the viewpoint of easily adjusting the viscosity of the thermosetting resin composition to the above range.

[0071] When compound (a) is an epoxy compound, the epoxy equivalent of compound (a) is preferably 226 g / eq or more and 260 g / eq or less. If the epoxy equivalent is 226 g / eq or more, the flexibility of the cured product can be further improved. In addition, by having an epoxy equivalent of 260 g / eq or less, the reduction in moisture resistance can be further suppressed. The above-mentioned epoxy equivalent can be measured using the same method as described in compound (A).

[0072] Specific examples of the compound (a) include o-phenylphenol glycidyl ether, m-phenylphenol glycidyl ether, p-phenylphenol glycidyl ether, and derivatives thereof. The thermosetting resin composition of the present application may contain only one compound (a), or may contain two or more compounds (a).

[0073] Examples of commercially available products of the compound (a) include OPP-EP (manufactured by Yokkaichi Kogyo Co., Ltd.) and the like.

[0074] The content of compound (a) is preferably 10% by mass or more and 30% by mass or less, more preferably 15% by mass or more and 25% by mass or less relative to the total mass of the thermosetting resin composition. If the above content is 10% by mass or more, the moisture resistance of the thermosetting resin composition can be further improved. In addition, if the above content is 30% by mass or less, the softness of the cured product can be further maintained.

[0075] In addition, the compound (a) may contain a functional group other than the glycidyl group and the oxetanyl group, and a structure other than the biphenyl structure in part.

[0076] 1-3. Other compounds

[0077] The thermosetting resin composition of the present invention may contain other curable compounds other than compound (A) and compound (a). Examples of other curable compounds include polyfunctional epoxy compounds that do not have the structure represented by general formula (1) and biphenyl structure.

[0078] The total content of other curable compounds is preferably 30% by mass or more and 40% by mass or less relative to the total mass of the thermosetting resin composition. When the content is within the above range, the viscosity of the thermosetting resin composition can be easily adjusted to the above range.

[0079] 1-4. Thermosetting agent (B)

[0080] The thermosetting resin composition of the present invention contains a thermosetting agent (B).

[0081] The thermosetting agent (B) may be any thermosetting agent that can react with a compound contained in the thermosetting resin composition such as the compound (A) to cure the compound, and examples thereof include dihydrazide thermosetting agents, amine adduct thermosetting agents, and polyamine thermosetting agents. Among them, polyamine thermosetting agents are preferred from the viewpoint of improving the viscosity stability of the thermosetting resin composition.

[0082] The thermosetting agent (B) is preferably a latent thermosetting agent. The latent thermosetting agent is a curing agent that does not cure compounds such as the compound (A) under normal storage conditions (room temperature), but cures these compounds when heated.

[0083] Examples of the latent thermosetting agent include dihydrazide-based latent thermosetting agents, amine adduct-based latent thermosetting agents, and polyamine-based latent thermosetting agents, etc. Among them, polyamine-based latent thermosetting agents are preferred from the viewpoint of improving the viscosity stability of the thermosetting resin composition.

[0084] Examples of dihydrazide latent heat curing agents include adipic acid dihydrazide (melting point 181° C.), 1,3-bis(hydrazinocarboxyethyl)-5-isopropylhydantoin (melting point 120° C.), 7,11-octadecadiene-1,18-dicarbohydrazide (melting point 160° C.), dodecanedioic acid dihydrazide (melting point 190° C.), and sebacic acid dihydrazide (melting point 189° C.).

[0085] Amine addition latent heat curing agent is a latent heat curing agent containing an addition compound obtained by reacting an amine compound having catalytic activity with an arbitrary compound. Examples of amine addition latent heat curing agents include Amicure PN-40 (melting point 110°C), Amicure PN-50 (melting point 120°C), Amicure PN-23 (melting point 100°C), Amicure PN-31 (melting point 115°C), Amicure PN-H (melting point 115°C), Amicure MY-24 (melting point 120°C), and Amicure MY-H (melting point 131°C) (all manufactured by Ajinomoto Fine-Techno Co., Ltd.).

[0086] Examples of the polyamine-based latent thermosetting agent include ADEKA HARDENER EH5015S (melting point 85° C. to 105° C.), ADEKA HARDENER EH4357S (melting point 75° C. to 85° C.), and ADEKA HARDENER EH5030S (melting point 70° C. to 80° C.) (all manufactured by ADEKA Corporation).

[0087] The melting point of the thermosetting agent is preferably 60°C to 190°C, more preferably 60°C to 110°C, and even more preferably 65°C to 100°C. If the melting point is 60°C or higher, the thermosetting agent (B) can be prevented from reacting with the compound (A) or the like at room temperature to cure. If the melting point is 110°C or lower, the compound (A) or the like can be cured even without excessive heating.

[0088] Relative to the gross mass of the thermosetting resin composition, the content of the thermosetting agent (B) is preferably 25% by mass or more and 40% by mass or less, more preferably 30% by mass or more and 35% by mass or less. If the above content is 25% by mass or more, the curability of the cured product can be further improved. Thus, for example, the cured product of the sealant comprising the thermosetting resin composition can fully seal the display device. In addition, if the above content is 40% by mass or less, the viscosity of the thermosetting resin composition can be easily adjusted to the above range.

[0089] 1-5. Inorganic filler (C)

[0090] The thermosetting resin composition of the present invention may contain an inorganic filler (C). When the thermosetting resin composition contains an inorganic filler (C), the moisture resistance of the cured product is more easily improved.

[0091] Examples of the inorganic filler (C) include calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, zirconium silicate, iron oxide, titanium oxide, aluminum oxide (alumina), zinc oxide, silicon dioxide, potassium titanate, kaolin, talc, glass beads, sericite, activated clay, bentonite, aluminum nitride, silicon nitride, etc. The thermosetting resin composition may contain only one inorganic filler (C), or may contain two or more.

[0092] The shape of the inorganic filler (C) may be a fixed shape such as a sphere, a plate, or a needle, or may be amorphous. When the inorganic filler (C) is spherical, the average primary particle size of the inorganic filler (C) is preferably 0.1 μm or more and 20 μm or less, more preferably 0.1 μm or more and 10 μm or less, and further preferably 0.5 μm or more and 5.0 μm or less. If the above average primary particle size is within the above range, the viscosity of the thermosetting resin composition can be more easily adjusted. The average primary particle size of the inorganic filler (C) can be measured by a laser diffraction method according to JIS Z8825-1:2013.

[0093] The mass average particle size d of the inorganic filler (C) 50 It is preferably 0.05 μm or more and 5.0 μm or less, and more preferably less than 25.0 μm. 50 When the particle size is within the above range, the viscosity stability of the thermosetting resin composition becomes high. In addition, from the viewpoint of improving the moisture resistance of the cured product, the mass average particle size d of the filler is preferably 50 The particle size is preferably 0.05 μm or more, more preferably 0.1 μm or more, further preferably 0.2 μm or more, and may exceed 1.0 μm. 50 It can be determined by a laser diffraction method in accordance with JIS Z8825-1: 2013. Specifically, the particle size represented by the 50% by mass value on the mass cumulative curve obtained in the above measurement can be defined as the mass average particle size d. 50 .

[0094] The content of the inorganic filler (C) is preferably 0% by mass or more and 10% by mass or less, more preferably 0% by mass or more and 5% by mass or less, relative to the total mass of the thermosetting resin composition. In addition, if the above content is 10% by mass or less, the viscosity of the thermosetting resin composition can be suppressed from being excessively increased, and the above viscosity can be easily adjusted.

[0095] 1-6. Others

[0096] The thermosetting resin composition of the present invention may also contain additives such as silane coupling agents, rubber agents, ion scavengers, ion exchangers, leveling agents, pigments, dyes, plasticizers, defoamers, etc. The thermosetting resin composition may contain only one additive or two or more additives.

[0097] Examples of the silane coupling agent include vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane.

[0098] The content of the silane coupling agent is preferably 0.01% by mass or more and 5.0% by mass or less relative to the total mass of the thermosetting resin composition. When the content of the silane coupling agent is within the above range, the bonding strength between the cured product and the substrate can be further improved.

[0099] 1-7. Preparation method of thermosetting resin composition

[0100] The preparation method of the above-mentioned thermosetting resin composition is not particularly limited, and the composition can be prepared by mixing the components using a known method. The method for mixing the components is not particularly limited, and for example, a double-arm mixer, a roller mixer, a twin-screw extruder, a ball mill mixer, and a planetary mixer can be used. After the components are mixed, they can be filtered using a filter to remove impurities, thereby obtaining a thermosetting resin composition, or they can be further subjected to vacuum degassing treatment to obtain the composition.

[0101] 1-8. Physical properties of thermosetting resin composition

[0102] The viscosity of the thermosetting resin composition of the present invention measured by an E-type viscometer at 25°C and 2.5rpm is 20.0Pa·s or less, preferably 10.0Pa·s or less, and more preferably 5.0Pa·s or less. If the above viscosity is 20.0Pa·s or less, when a sealant containing a thermosetting resin composition is used to make various display devices, it will enter into a small gap, and the display device can be more reliably sealed. The lower limit of the above viscosity is not particularly limited, and is preferably 0.5Pa·s or more. The viscosity of the thermosetting resin composition can be set to the above range by adjusting the composition of the thermosetting resin composition.

[0103] 2. Sealant for display devices

[0104] The sealant for a display device of the present invention (hereinafter simply referred to as “sealant”) contains the above-mentioned thermosetting resin composition.

[0105] The sealant may be the above-mentioned thermosetting resin composition as it is or a mixture of the above-mentioned thermosetting resin composition and additives and the like may be used as the sealant.

[0106] The sealant of the present invention can be used in various display devices. Regarding the sealant, it is particularly preferred that the cured product of the sealant is used to seal the display element in a display device having a pair of substrates and a display element disposed between the pair of substrates. Specifically, it is preferred that the sealant is used to seal the display element in various display devices having a liquid crystal component, an EL component, an LED (light emitting diode) component, an electrophoretic display element, an electrochromic display element, etc.

[0107] Since the viscosity of the sealant is within the above range, it is particularly easy to enter the gap between the substrates holding the display element, so that sealing can be performed more reliably. In a display device having an electrophoretic display element and an electrochromic display element, since it is expected that the sealant enters into a tiny gap, the sealant of the present invention can be more appropriately used in an electrophoretic display device or an electrochromic display device. Examples of electrophoretic display devices and electrochromic display devices include displays using these methods, electronic paper, etc.

[0108] The sealant can be applied to the substrate and cured to seal the display element. The sealant application method is not particularly limited, and known methods such as a dispenser and screen printing can be used. In addition, the sealant can be filled between a pair of substrates that clamp the display element and then cured. The method of filling the sealant between the substrates can be, for example, filled using a dispenser.

[0109] In addition, the sealant can be cured by heat curing. From the viewpoint of suppressing degradation of the display device, the heat curing temperature is preferably 60° C. to 80° C. The heat curing time can be appropriately adjusted according to the heat curing temperature or the amount of the sealant, for example, 30 minutes to 90 minutes.

[0110] 3. Display device

[0111] The display device of the present invention includes a pair of substrates, a cured product of the display device sealant disposed between the pair of substrates, and a display element disposed in a space between the pair of substrates surrounded by the cured product of the sealant.

[0112] Examples of the substrate include an inorganic substrate, a resin substrate, and the like.

[0113] Examples of inorganic substrates include glass substrates, etc. Examples of resin substrates include substrates made of resins such as polyethylene terephthalate, polymethyl methacrylate, polycarbonate, cyclic polyolefin (COC, Cyclo-Olefin Copolymer), polypropylene, polystyrene, polyvinyl chloride, transparent ABS resin, transparent nylon, transparent polyimide, and polyvinyl alcohol.

[0114] As described above, examples of display elements include liquid crystal elements, EL elements, LED elements, electrophoretic display elements, electrochromic display elements, and the like.

[0115] For example, a display device having an electrophoretic display element may be configured as follows: Figure 1 The structure shown.

[0116] The display device 100 includes a pair of substrates 110 , a cured product 120 of the sealant 1 for a display device disposed between the pair of substrates 110 , and a display element 130 disposed in a space between the pair of substrates 110 surrounded by the cured product 120 of the sealant.

[0117] The display element 130 includes a display layer 130 a and a transparent electrode 130 b for driving the display layer 130 a .

[0118] The display layer 130a may be configured to include charged particles such as pigments and a dispersion medium. For example, the display layer 130a may be configured to include microcapsules containing charged particles and a dispersion medium such as an alcohol solvent.

[0119] The transparent electrode 130b applies a voltage to the display layer 130a to drive the display layer 130a. A protective film may be disposed on the surface of the transparent electrode 130b.

[0120] The display device of the present invention can be manufactured, for example, through the following steps: (1) a step of forming a stacked body having a display element and a pair of substrates that clamp the display element, (2) a step of filling the above-mentioned sealant in the gap between the pair of substrates formed at the peripheral portion of the stacked body, and (3) a step of curing the above-mentioned sealant.

[0121] The method of filling the sealant is not particularly limited, and the sealant may be filled using, for example, a dispenser. The method of curing the sealant may be the same as that described for the sealant.

[0122] Example

[0123] Hereinafter, the present invention will be specifically described with reference to Examples, but the scope of the present invention is not limited to the description of the Examples.

[0124] 1. Materials of thermosetting resin composition

[0125] 1-1. Compound (A)

[0126] EP-4010S (manufactured by ADEKA Co., Ltd., a bisphenol A type difunctional epoxy compound (propylene oxide modified), in which a=3, b=0, c=0 in the general formula (1), R1 in the general formula (2) is an isopropylidene group, epoxy equivalent: 350 g / eq, and the glass transition temperature Tg of the cured product: 60°C) was used.

[0127] 1-2. Compounds having a biphenyl structure (a)

[0128] OPP-EP (manufactured by Yokkaichi Kogyo Co., Ltd., epoxy compound, epoxy equivalent: 230 g / eq) was used.

[0129] 1-3. Other compounds (A')

[0130] Any of the following polyfunctional epoxy compounds was used.

[0131] EXA-835LV (A'-1) (manufactured by DIC Corporation, bisphenol F type / bisphenol A type bifunctional epoxy compound, epoxy equivalent: 165 g / eq)

[0132] YL-983U (A'-2) (manufactured by Mitsubishi Chemical Corporation, bisphenol F type difunctional epoxy compound, epoxy equivalent: 170 g / eq)

[0133] YL-980 (A'-3) (manufactured by Mitsubishi Chemical Corporation, bisphenol A type difunctional epoxy compound, epoxy equivalent: 190 g / eq)

[0134] YX8000D (A'-4) (Mitsubishi Chemical Corporation, hydrogenated bisphenol A type difunctional epoxy compound, epoxy equivalent 205 g / eq)

[0135] The glass transition temperature of the compound (A) after curing is measured by the following method.

[0136] 100 parts by mass of the epoxy compound (compound (A)), a chemically equivalent amount of methylhexahydrophthalic anhydride to 100 parts by mass of the epoxy compound, and 1 part by mass of dimethylbenzyldiamine were mixed, heated at 110° C. for 3 hours, and then heated at 165° C. for 2 hours. The obtained cured product was processed into a film of 100 μm, and the glass transition temperature (Tg) of the cured product was measured by dynamic viscoelasticity measurement (DMA).

[0137] 1-4. Thermosetting agent (B)

[0138] EH5030S (polyamine-based thermosetting agent, manufactured by ADEKA Corporation, melting point: 70° C. to 80° C., amine equivalent: 105 g / equivalent) was used.

[0139] 1-5. Inorganic filler (C)

[0140] S-100 (silicon dioxide particles, manufactured by Nippon Shokubai Co., Ltd.) was used.

[0141] 1-6. Others

[0142] The following substances were used.

[0143] Silane coupling agent: KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0144] 2. Preparation of Thermosetting Resin Composition

[0145] (Example 1)

[0146] A thermosetting resin composition was obtained by mixing 50 parts by mass of the compound (A), 215 parts by mass of the compound (a) having a biphenyl structure, 320 parts by mass of the polyfunctional epoxy compound (A'-1), 330 parts by mass of the thermosetting agent (B), and 30 parts by mass of the silane coupling agent using a three-roll mill. In this example, this was used as a sealant.

[0147] (Example 2 to Example 7, Comparative Example 1 to Comparative Example 4)

[0148] Except having changed into the composition shown in Table 1 and Table 2, it carried out similarly to Example 1, and prepared the thermosetting resin composition.

[0149] 3. Evaluation

[0150] The obtained thermosetting resin composition and its cured product were evaluated as follows.

[0151] (Viscosity)

[0152] The viscosity of the thermosetting resin composition was measured at 25° C. using an E-type viscometer at a rotation speed of 2.5 rpm.

[0153] (Adhesion (flexibility))

[0154] The prepared thermosetting resin composition was dripped onto a screen having a mesh diameter of 1.5 mm. Then, the screen was set in a manner that the mesh portions overlapped on the central portion of a 25 mm×45 mm glass substrate (RT-DM88-PIN, manufactured by EHC Co., Ltd.) on which a transparent electrode was preformed, and the thermosetting resin composition was applied from the mesh portions using a squeegee.

[0155] Next, the glass substrate formed with the thermosetting resin composition was bonded to the glass substrate forming a pair thereof from directly above the thermosetting resin composition in such a manner that the long sides of the substrates intersected each other perpendicularly. The two bonded glass substrates were then heated at 80° C. for 1 hour to cure the thermosetting resin composition, thereby obtaining a test piece.

[0156] For the obtained test piece, a press-in tester (Model 210, manufactured by INTESCO Co., Ltd.) was used to press a portion 22.5 mm from the center of the thermosetting resin composition cured into a circular shape vertically relative to the glass substrate at a speed of 37.5 mm / min to measure the stress when the thermosetting resin composition was peeled off from the glass substrate. The bonding strength was obtained by dividing the stress by the dot width drawn using the thermosetting resin composition. The obtained bonding strength was evaluated according to the following criteria.

[0157] ○ Adhesion strength is 1.0N / mm or more

[0158] △The bonding strength is 0.5N / mm or more and less than 1.0N / mm

[0159] × Adhesion strength is less than 0.5N / mm

[0160] (moisture resistance)

[0161] A release film was placed on a glass plate, and the four sides of the glass plate were surrounded by a 100 μm PET (polyethylene terephthalate) film sheet, and then the prepared thermosetting resin composition was applied. Then, a release film and a glass plate were further placed on the applied thermosetting resin composition, and the four sides of the glass plate were fixed with a clamp. The glass sheet with the coating film of the thermosetting resin composition was kept in a hot air drying oven at 80°C for 60 minutes, then taken out and cooled. Then, the glass sheet was disassembled, and the coating film was peeled off from the release paper to obtain a film with a thickness of 100 μm.

[0162] The obtained 100 μm film was used to prepare an aluminum cup according to the method of JIS Z0208:1976, and placed in a high temperature and high humidity tank at 60°C and 90% RH for 17 hours. The weight of the film after placement was then measured. After the film was placed again for 24 hours, the weight of the film was measured, and the moisture permeability was calculated using the following calculation formula.

[0163] Moisture permeability (g / m 2 ·100μm·24h) = [weight of the aluminum cup after 24 hours (g) - weight of the aluminum cup before 24 hours (g)] / membrane area (m 2 )

[0164] Based on the calculated moisture permeation rate, moisture resistance was evaluated according to the following criteria.

[0165] ○Moisture permeability less than 50g / m 2

[0166] △Moisture permeability is 50g / m 2 Above and less than 80g / m 2

[0167] ×Moisture permeability: 80g / m 2 above

[0168] The evaluation results are shown in Tables 1 and 2. The numerical values ​​of the compositions in Tables 1 and 2 represent parts by mass.

[0169] [Table 1]

[0170]

[0171] [Table 2]

[0172]

[0173] As shown in Table 1, the thermosetting resin compositions of Examples 1 to 7 containing a compound (A) having a glycidyl group and a structure of formula (1) and a polyamine-based latent thermosetting agent (B) all have excellent bonding strength when stress is applied, and the sealant (thermosetting resin composition) is not easily peeled off from the substrate. It is believed that the reason is that the compound (A) has a structure represented by formula (1), thereby relieving stress. It can be further seen that moisture resistance can be improved in Examples 1 to 7.

[0174] On the other hand, the thermosetting resin compositions of Comparative Examples 1 to 4 not containing the compound (A) had low adhesive strength when stress was applied.

[0175] This application claims priority based on Japanese Patent Application No. 2022-049974 filed on March 25, 2022. The contents described in the specification and drawings of that application are incorporated herein by reference in their entirety.

[0176] Industrial Applicability

[0177] According to the present invention, a thermosetting resin composition can be obtained which can suppress peeling from a substrate when stress is applied to a display device. The present invention is very useful in applications to various display devices.

[0178] Explanation of symbols

[0179] 100: Display device

[0180] 110: Substrate

[0181] 120: Cured sealant

[0182] 130: Display element.

Claims

1. A thermosetting resin composition comprising: Compound (A) has a total of two or more functional groups of at least one of a glycidyl group and an oxetanyl group, and has a structure represented by the general formula (1); and Thermal curing agent (B), The thermosetting resin composition has a viscosity of 20.0 Pa·s or less as measured by an E-type viscometer at 25° C. and 2.5 rpm, [Chemistry 1] In the general formula (1), a represents an integer of 0 to 8, b represents an integer of 0 to 3, c represents an integer of 0 to 8, d represents an integer of 0 to 8, at least one of a, b and c is 1 or more, n is an integer of 1 or more, and * represents a bonding position. When compound (A) has a plurality of structures represented by the general formula (1), the numbers of a, b, c, d and n in each structure may be the same or different.

2. The thermosetting resin composition according to claim 1, in, The compound (A) further has a structure represented by the general formula (2); [Chemistry 2] In the general formula (2), R 1 is any one of an alkylene group having 1 to 4 carbon atoms, an alkylidene group having 2 to 4 carbon atoms, an oxygen atom and a sulfur atom, and * represents a bonding position; when compound (A) has a plurality of structures represented by general formula (2), R in each structure 1 Can be the same or different.

3. The thermosetting resin composition according to claim 1 or 2, in, The compound (A) is a difunctional epoxy compound wherein, in the general formula (1), a=3, b=0, c=0, d=0; a=1, b=1, c=0, d=0; or a=0, b=1, c=0, d=1.

4. The thermosetting resin composition according to any one of claims 1 to 3, in, The compound (A) is an epoxy compound having an epoxy equivalent of 300 g / eq or more, Furthermore, 100 parts by mass of the compound (A), a chemically equivalent amount of methylhexahydrophthalic anhydride relative to 100 parts by mass of the compound (A), and 1 part by mass of dimethylbenzylamine are mixed, heated at 110° C. for 3 hours, and then heated at 165° C. for 2 hours to obtain a cured product having a glass transition temperature of 100° C. or less.

5. The thermosetting resin composition according to any one of claims 1 to 4, in, The thermosetting agent (B) is at least one selected from the group consisting of dihydrazide thermosetting agents, amine adduct thermosetting agents, and polyamine thermosetting agents.

6. The thermosetting resin composition according to any one of claims 1 to 5, in, The thermosetting agent (B) is a polyamine-based latent thermosetting agent having a melting point of 60° C. to 110° C.

7. The thermosetting resin composition according to any one of claims 1 to 6, further comprising a compound (a), The compound (a) has at least one functional group of a glycidyl group and an oxetanyl group, and a biphenyl structure. 8 . The thermosetting resin composition according to claim 1 , further comprising an inorganic filler (C). 9 . A sealant for a display device, comprising the thermosetting resin composition according to claim 1 .

10. The sealant for a display device according to claim 9, in, In a display device including a pair of substrates and a display element disposed between the pair of substrates, the cured product of the display device sealant is used to seal the display element.

11. The sealant for a display device according to claim 9 or 10, in, The display device is an electrophoretic display device or an electrochromic display device.

12. A display device comprising: a pair of base plates; The cured product of the display device sealant according to any one of claims 9 to 11, which is disposed between the pair of substrates; and The display element is arranged in a space between the pair of substrates and surrounded by the cured product of the display device sealant.