Polyester copolymer for heat-shrink labels, composition comprising same, and product

By developing specific polyester copolymers, the problems of insufficient heat resistance and heat shrinkability of heat shrinkable film label materials are solved, and the efficient removal of label paper and the effect of containers are achieved.

CN118922467APending Publication Date: 2024-11-08SK CHEMICALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029656.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing heat shrink film label materials such as polystyrene and oriented polystyrene have shortcomings in terms of heat resistance and heat shrinkage properties, making it difficult to effectively remove label paper from containers, and lacks resins with high shrinkage properties and easy separation.

Method used

A polyester copolymer has been developed, which is polymerized with ethylene glycol by dicarboxylic acid or its derivatives, with specific linear diol monomer and cyclic monomer residues, satisfying specific A-value and physical property factors. Range to achieve suitable tear strength and shrinkage stress, ensuring that the label paper does not deform when removed.

Benefits of technology

The polyester copolymer has low shrinkage stress and excellent shrinkage properties on the container, making it easy to remove without causing the container to deform, and at the same time has appropriate tear strength for easy separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005055338100000221
    Figure BDA0005055338100000221
  • Figure BDA0005055338100000222
    Figure BDA0005055338100000222
  • Figure BDA0005055338100000231
    Figure BDA0005055338100000231
Patent Text Reader

Abstract

In the present disclosure, a polyester copolymer having excellent shrinkage properties and removability is provided. In particular, the present disclosure provides a polyester copolymer having a tear strength in a range suitable for removal from a container and a shrinkage stress in a range that does not deform the container.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0036015 filed on March 23, 2022, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety.

[0003] The present disclosure relates to a polyester copolymer that can be used for heat shrink labels and has excellent shrinking properties and removability and a composition comprising the polyester copolymer. The present disclosure also relates to a product comprising the polyester copolymer. Background Art

[0004] In recent years, the use of plastic packaging containers has increased rapidly, and international environmental regulations for them have been strengthened. Therefore, the industry is more interested in sustainable packaging. In addition, there is a need to remove label paper from beverage containers according to the recycling method of waste. Therefore, there is a need to develop a resin for labels that can be easily removed from the container and has a high shrinkage rate.

[0005] However, polystyrene and oriented polystyrene (OPS), which are widely used as materials for heat shrinkable film labels, have problems of insufficient heat resistance and heat shrinking performance. Therefore, by solving these problems, the development of polyester-based resins for heat shrinkable films has been actively pursued.

[0006] However, since there is still no resin having both shrinkage properties such as shrinkage stress and shrinkage ratio and ease of label separation, there is a need for developing a resin. DETAILED DESCRIPTION OF THE INVENTION

[0008] Technical issues

[0009] In the present disclosure, a polyester copolymer having excellent shrinkage properties and removability is provided. Specifically, the present disclosure provides a polyester copolymer having a tear strength within a range suitable for removal from a container and a shrinkage stress within a range not to deform the container.

[0010] Technical Solutions

[0011] In order to solve the above problems, the following polyester copolymer is provided:

[0012] The polyester copolymer has a structure in which an acid portion derived from a dicarboxylic acid or a derivative thereof and a diol portion derived from a diol including ethylene glycol are repeated,

[0013] wherein the polyester copolymer comprises residues of linear diol monomers and residues of cyclic monomers;

[0014] The value of A in the following equation 1 is 2.0 or more and 6.5 or less, and

[0015] The physical property factor value of the following Equation 2 is greater than 0 and 42.5 or less.

[0016] [Equation 1]

[0017] A value = (residue content of linear diol monomers other than ethylene glycol (mol%)) * 20 / ((residue content of cyclic monomers (mol%)) * 2-99)

[0018] [Equation 2]

[0019] Physical property factor = (A value) * 8.4-11.13

[0020] In Equation 1, the content is based on 100 mol% of the total residues.

[0021] Hereinafter, the polyester copolymer will be described in more detail.

[0022] In the present disclosure, the term 'residue' refers to a portion or unit derived from a specific compound contained in a product of a chemical reaction when the specific compound participates in a chemical reaction. Specifically, each of the "residue" of a dicarboxylic acid component and the "residue" of a diol component refers to a portion derived from the dicarboxylic acid component or a portion derived from the diol component in a polyester copolymer formed by an esterification reaction or a polycondensation reaction.

[0023] Polyester copolymer

[0024] The polyester copolymer according to one embodiment of the present disclosure is prepared by polymerizing a dicarboxylic acid or a derivative thereof with a diol, and has a structure in which an acid moiety derived from a dicarboxylic acid or a derivative thereof and a diol moiety derived from a diol containing ethylene glycol are repeated. In the present disclosure, the acid moiety and the diol moiety refer to the residue remaining after removing hydrogen, a hydroxyl group or an alkoxy group from the polymerization of a dicarboxylic acid or a derivative thereof with a diol. The dicarboxylic acid or a derivative thereof and the diol will be described in more detail below. For example, the dicarboxylic acid or a derivative thereof may be mainly terephthalic acid or a derivative thereof, and the diol includes ethylene glycol and may also include a derivative of ethylene glycol.

[0025] Polyester copolymers generally have higher tear strength in the machine direction than in the vertical direction. However, when used as a label paper on a container, low tear strength in the machine direction is advantageous for removal because it is easy to tear. In addition, if the shrinkage stress of the polyester copolymer when used as a label paper on a container is too high, deformation of the container such as crushing may occur. Therefore, the present disclosure is intended to provide a polyester copolymer having a tear strength and shrinkage stress in the machine direction within a range suitable for use as a label paper for containers and the like.

[0026] The polyester copolymer may include residues of linear diol monomers and residues of cyclic monomers.

[0027] In addition, the polyester copolymer may have a value of the following Equation 1 of 2.0 or more and 6.5 or less, and a value of a physical property factor of the following Equation 2 of greater than 0 and 42.5 or less.

[0028] [Equation 1]

[0029] A value = (residue content of linear diol monomers other than ethylene glycol (mol%)) * 20 / ((residue content of cyclic monomers (mol%)) * 2-99)

[0030] [Equation 2]

[0031] Physical property factor = (A value) * 8.4-11.13

[0032] In Equation 1, the content is based on 100 mol% of the total residues.

[0033] 100 mol% of the total residues means the sum of the residue content of the cyclic monomer and the residue content of the linear diol monomer. That is, 100 mol% of the total residues in the present disclosure means the sum of the residue content derived from the dicarboxylic acid or its derivative constituting the polyester copolymer and the residue content derived from the diol component. In addition, the dicarboxylic acid or its derivative may be cyclic or linear, and the diol component may also be cyclic or linear.

[0034] Specifically, the value of Equation 1 may be 2.0 or more, 2.5 or more, 3.0 or more, 3.5 or more, or 4.0 or more and 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, or 4.5 or less.

[0035] In addition, the physical property factor value of Equation 2 can be greater than 0, greater than 5.0, greater than 10.0, greater than 15.0 or greater than 20.0 and 42.5 or less, 42.0 or less, 40.0 or less, 35.0 or less, 30.0 or less or 25.0 or less.

[0036] The physical property factor value of equation 2 represents the tear strength of the polyester copolymer in the machine direction. That is, the tear strength of the resin can be evaluated only by the composition ratio of the monomers without the steps of stretching the resin and measuring the physical properties, and there is no prior art that expresses the tear strength as the composition ratio of the monomers. In actual industry, resins are manufactured in batches, and after checking the physical properties during the manufacturing process, it is actually impossible to readjust the composition ratio of the input monomers. Therefore, it is very important to easily check the physical property factor to be achieved using only the composition ratio of the monomers.

[0037] When the A value of equation 1 is less than 2.0, the physical property factor value of equation 2 and the tear strength in the machine direction (MD direction) have a large difference, and there may be a problem that the physical property factor is useless. In addition, when the A value of equation 1 exceeds 6.5, the tear strength exceeds 42.5 N / mm, making it difficult to tear and remove the label from the container when applied to the container.

[0038] The physical property factor value of Equation 2 represents tear strength in the machine direction, and may be greater than 0 and 42.5 or less in consideration of easy tear properties to be achieved in the present disclosure when the polyester copolymer is applied to a label for a container.

[0039] In equation 1, the residue of the cyclic monomer may be derived from a dicarboxylic acid or a derivative thereof, or a diol other than ethylene glycol. There are no restrictions on dicarboxylic acids or derivatives thereof and diols other than ethylene glycol, as long as they are used for polyester copolymers and are monomers having an aliphatic ring structure or an aromatic ring structure in the molecular structure. For example, they may be at least one selected from the group consisting of 1,4-cyclohexanedimethanol, 1,4-cyclohexanedicarboxylic acid, terephthalic acid or a derivative thereof, recycled 1,4-cyclohexanedimethanol, recycled 1,4-cyclohexanedicarboxylic acid, and recycled terephthalic acid or a derivative thereof. Terephthalic acid or a derivative thereof may be at least one selected from the group consisting of terephthalic acid, dimethyl terephthalic acid, hydroxyethyl terephthalic acid, recycled terephthalic acid, recycled dimethyl terephthalic acid, and recycled hydroxyethyl terephthalic acid. In addition, based on 100 mol% of the total residue, the residue content of the cyclic monomer can be 56.5 mol% or more and 67.5 mol% or less. Specifically, based on 100 mol% of the total residue, the residue content of the cyclic monomer can be 56.5 mol% or more, 60.0 mol% or more, 60.5 mol% or more, 61.0 mol% or more, 61.5 mol% or more, 62.0 mol% or more, 62.5 mol% or more, 63.0 mol% or more, 63.5 mol% or more, 64.0 mol% or more, 64.5 mol% or more, 65.0 mol% or more, 65.5 mol% or more, or 66.0 mol% or more and 67.5 mol% or less, 67.0 mol% or less, or 66.5 mol% or less.

[0040] In Equation 1, the residue of the linear diol monomer may be derived from diol. The diol is not limited as long as it is used for the polyester copolymer and the molecular structure is a linear structure. For example, the residue of the linear diol monomer may be derived from at least one selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, recycled ethylene glycol, recycled diethylene glycol, and recycled neopentyl glycol.

[0041] In Equation 1, the residue content of the linear glycol monomer other than ethylene glycol is used as a variable. In this case, the residue content of the linear glycol monomer other than ethylene glycol in Equation 1 may be 12.5 mol% or less based on 100 mol% of the total residue. Specifically, the residue content of the linear glycol monomer other than ethylene glycol in Equation 1 may be 2.5 mol% or more, 3.0 mol% or more, 3.5 mol% or more, 4.0 mol% or more, 4.5 mol% or more, 5.0 mol% or more, 5.5 mol% or more, or 6.0 mol% or more and 12.5 mol% or less, 10.0 mol% or less, 8.0 mol% or less, 7.5 mol% or less, 7.0 mol% or less, or 6.5 mol% or less based on 100 mol% of the total residue.

[0042] In addition to the above equation 1, the diol of the polyester copolymer of one embodiment of the present disclosure includes ethylene glycol. In the absence of ethylene glycol, even if the A value and the physical property factor meet the above range, the tear strength in the machine direction exceeds 42.5 N / mm. Therefore, when applied to a container as a label, the label is difficult to tear, which is not conducive to separation, or the shrinkage stress is high, which may be different from the characteristics of the low shrinkage stress label to be achieved in the present disclosure. Based on 100 mol% of the total residue, the residue of the ethylene glycol monomer may be 27.5 mol% to 39.0 mol%.

[0043] The polyester copolymer satisfying Equation 1 and Equation 2 may have a tear strength in the machine direction (MD direction) of 7.0 N / mm or more and 42.5 N / mm or less at 90° C. Specifically, the tear strength in the machine direction (MD direction) at 90° C. may be 7.0 N / mm or more, 7.5 N / mm or more, 8.0 N / mm or more, 8.5 N / mm or more, 9.0 N / mm or more, 10.0 N / mm or more, 15.0 N / mm or more, 20.0 N / mm or more, or 25.0 N / mm or more and 42.5 N / mm or less, 40.0 N / mm or less, 35.0 N / mm or less, or 30.0 N / mm or less.

[0044] When used as label paper for containers, etc., when the tear strength in the machine direction is less than 7.0 N / mm, there may be a problem in not being able to tear in the desired direction, and when used as label paper, when the tear strength in the machine direction exceeds 42.5 N / mm, there may be problems in removal.

[0045] In addition, the polyester copolymer satisfying Equation 1 and Equation 2 may have a shrinkage stress of 12.0 MPa or less at 85° C. Specifically, the polyester copolymer may have a shrinkage stress of 3.1 MPa or more and 12.0 MPa or less at 85° C. Specifically, the shrinkage stress at 85° C. may be 3.1 MPa or more, 3.4 MPa or more, 4.0 MPa or more, 4.5 MPa or more, 5.0 MPa or more, 5.5 MPa or more, 6.0 MPa or more, or 6.5 MPa or more and 12.0 MPa or less, 11.0 MPa or less, 10.0 MPa or less, 9.0 MPa or less, 8.5 MPa or less, 8.0 MPa or less, or 7.0 MPa or less.

[0046] If the shrinkage stress exceeds 12.0 MPa, there may be a problem of deformation of the container when used as a label paper for a container, and if the shrinkage stress is too low, there may be a problem of non-adhesion to the container when used as a label paper for a container.

[0047] In addition, the polyester copolymer satisfying Equation 1 and Equation 2 may have a glass transition temperature of 69.0° C. or more and 74.8° C. or less. When the glass transition temperature is too low, there is a possibility of cracking during heat treatment during processing and film formation, and when the glass transition temperature is high, sufficient stretching required for label application may not be possible.

[0048] Preparation of polyester copolymers

[0049] The polyester copolymer may be prepared by a step including subjecting a dicarboxylic acid or a derivative thereof and a diol to an esterification reaction or an ester exchange reaction, and subjecting a product obtained by the esterification reaction or the ester exchange reaction to a polycondensation reaction.

[0050] In the esterification reaction or transesterification reaction, a catalyst may be used. The catalyst may be a methanolate of sodium and magnesium; an acetate, borate, fatty acid salt or carbonate of Zn, Cd, Mn, Co, Ca, Ba and the like; a metal such as Mg; or an oxide of Pb, Zn, Sb, Ge and the like.

[0051] The esterification reaction or transesterification reaction may be carried out in a batch, semi-continuous or continuous manner.Each raw material may be added individually, but it may be preferably added in the form of a slurry in which the dicarboxylic acid or its derivative is mixed in the diol.

[0052] Polycondensation catalysts, stabilizers, colorants, crystallization agents, antioxidants, branching agents, and the like may be added to the slurry before the esterification reaction or transesterification reaction or added to the product after the reaction is completed.

[0053] However, the input time of the additive described above is not limited thereto, and the additive described above can be added at any time during the preparation of the polyester copolymer. As a polycondensation catalyst, conventional titanium-based compounds, germanium-based compounds, antimony-based compounds, aluminum-based compounds, and tin-based compounds can be appropriately selected and used. Preferred examples of titanium-based catalysts include tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, titanate octanediol, lactic acid titanate, triethanolamine titanate, titanate acetylacetonate, ethyl acetoacetate titanate, isostearyl titanate, titanium dioxide, titanium dioxide / silicon dioxide copolymer, titanium dioxide / zirconium dioxide copolymer, and the like. In addition, preferred examples of germanium-based catalysts include germanium dioxide and copolymers thereof. As a stabilizer, a phosphorus-based compound such as phosphoric acid, trimethyl phosphate and triethyl phosphate can be generally used, and the content of the phosphorus-based compound added based on phosphorus atoms can be 10ppm to 200ppm relative to the weight of the final polymer (polyester copolymer). When the content of the stabilizer is less than 10ppm, it may not be fully stabilized, and the color of the polymer may turn yellow. When the content exceeds 200ppm, a polymer with a high degree of polymerization may not be obtained.

[0054] In addition, the example of the colorant added in order to improve the color of the polymer can include conventional colorants, such as cobalt acetate, cobalt propionate and the like. Relative to the weight of the final polymer (polyester copolymer), the content of the addition based on cobalt atoms of conventional colorants can be 10ppm to 200ppm. If necessary, compounds based on anthraquinone, compounds based on pyrenone, compounds based on azo, compounds based on methine and the like can be used as organic colorants, and commercially available products include toners such as Polysynthren Blue RLS (manufactured by Clarient) and Solvaperm Red BB (manufactured by Clarient). Relative to the weight of the final polymer, the content of the addition of organic colorants can be 0ppm to 50ppm. When colorants are used with a content exceeding the scope described above, the yellowness of polyester copolymers may not be fully covered, or physical properties may be reduced.

[0055] Examples of the crystallizing agent may include crystal nucleating agents, ultraviolet absorbers, polyolefin-based resins, polyamide resins, and the like. Examples of the antioxidant may include hindered phenol-based antioxidants, phosphite-based antioxidants, thioether-based antioxidants, and mixtures thereof.

[0056] In addition, the esterification reaction may be carried out at a temperature of 200°C to 300°C or 230°C to 280°C and at 0 kgf / cm 2Up to 10.0kgf / cm 2 (0mmHg to 7355.6mmHg), 0kgf / cm 2 Up to 5.0kgf / cm 2 (0mmHg to 3677.8mmHg) or 0.1kgf / cm 2 Up to 3.0kgf / cm 2 (73.6 mmHg to 2206.7 mmHg) pressure. In addition, the transesterification reaction can be carried out at a temperature of 150°C to 270°C or 180°C to 260°C and at 0 kgf / cm 2 Up to 5.0kgf / cm 2 (0mmHg to 3677.8mmHg) or 0.1kgf / cm 2 Up to 3.0kgf / cm 2 The pressure outside the brackets refers to the gauge pressure (in kgf / cm 2 ), and the pressure in brackets refers to the absolute pressure (expressed in mmHg).

[0057] When the reaction temperature and pressure exceed the above range, the physical properties of the polyester copolymer may be reduced. The reaction time (average residence time) is generally 1 to 24 hours or 2 to 8 hours, and can vary according to the reaction temperature, pressure, and the molar ratio of the diol to the dicarboxylic acid or its derivative used.

[0058] The product obtained by esterification or transesterification can undergo polycondensation to prepare a polyester copolymer with a high degree of polymerization. Typically, the polycondensation reaction is carried out at a temperature of 150°C to 300°C, 200°C to 290°C or 260°C to 290°C and under a reduced pressure of 400mmHg to 0.01mmHg, 100mmHg to 0.05mmHg or 10mmHg to 0.1mmHg. Here, pressure refers to absolute pressure. The reduced pressure of 400mmHg to 0.01mmHg is to remove by-products such as glycols and unreacted materials of the polycondensation reaction. Therefore, when the pressure exceeds the above range, the removal of by-products and unreacted materials may be insufficient. In addition, when the temperature of the polycondensation reaction exceeds the above range, the physical properties of the polyester copolymer may be reduced. The polycondensation reaction can be carried out for a desired time until the desired intrinsic viscosity is reached, for example, an average residence time of 1 hour to 24 hours.

[0059] In order to reduce the content of unreacted materials remaining in the polyester copolymer, the unreacted raw materials can be discharged from the system by intentionally maintaining the vacuum reaction for a long period of time at the end of the esterification reaction or the transesterification reaction or at the beginning of the polycondensation reaction, that is, when the viscosity of the resin is not high enough. When the viscosity of the resin is high, it is difficult for the raw materials remaining in the reactor to flow out of the system. For example, the unreacted materials remaining in the polyester copolymer can be effectively removed by retaining the reaction product obtained by the esterification reaction or the transesterification reaction under a reduced pressure of about 400mmHg to 1mmHg or about 200mmHg to 3mmHg for about 0.2 hours to 3 hours before the polycondensation reaction. Here, the temperature of the product can be controlled to be equal to the temperature of the esterification reaction or the transesterification reaction, or the temperature of the polycondensation reaction, or the temperature between them.

[0060] Suitably, the intrinsic viscosity of the polymer obtained after the polycondensation reaction is 0.30 dl / g to 1.0 dl / g. When the intrinsic viscosity is less than 0.30 dl / g, the reaction rate in the solid phase reaction can be significantly reduced. When the intrinsic viscosity exceeds 1.0 dl / g, the viscosity of the molten material may increase during melt polymerization, and therefore, the possibility of polymer discoloration may increase through the shear stress between the agitator and the reactor, producing by-products such as acetaldehyde.

[0061] If necessary, the polyester copolymer according to one embodiment may have a higher degree of polymerization by further performing a solid phase reaction after the polycondensation reaction.

[0062] Specifically, the polymer obtained by polycondensation reaction is discharged from the reactor to be granulated. Granulation can be carried out by strand cutting method or underwater cutting method, in which the polymer is extruded into strand shape, solidified in cooling liquid and cut with a cutter, and in the underwater cutting method, the die hole is immersed in the cooling liquid, the polymer is directly extruded into the cooling liquid and cut with a cutter. Usually, the temperature of the cooling liquid should be kept low in the strand cutting method, so that the strand is well solidified, so that there is no cutting problem. In the underwater cutting method, it is preferred to keep the temperature of the cooling liquid according to the polymer, so that the shape of the polymer is uniform. However, in the case of crystalline polymers, the temperature of the cooling liquid can be intentionally kept high, so as to induce crystallization during discharge.

[0063] The water-soluble materials in the unreacted raw materials can be removed by washing the granular polymer. The smaller the particle size, the wider the surface area relative to the weight of the particles. Therefore, a small particle size is advantageous. To achieve this purpose, the particles can be prepared to have an average weight of about 15 mg or less. For example, the granular polymer can be washed by leaving it in water at a temperature equal to the glass transition temperature of the polymer or at a temperature of about 50°C to 100°C for 5 minutes to 10 hours.

[0064] The granular polymer is subjected to a crystallization step to prevent fusion during the solid phase reaction. The crystallization step may be performed in an atmosphere, an inert gas, water vapor, or an inert gas containing water vapor, or in a solution, and may be performed at 110° C. to 210° C. or 120° C. to 210° C. When the temperature is low, the speed of crystal formation of the particles may be too slow. When the temperature is high, the rate at which the surface of the particles melts may be faster than the rate at which crystals are formed, so that the particles may adhere to each other to cause fusion. Since the heat resistance of the particles increases as the particles crystallize, the particles may also be crystallized by dividing the crystallization into several steps and gradually increasing the temperature.

[0065] The solid phase reaction can be carried out for an average residence time of 1 hour to 150 hours under an inert gas atmosphere such as nitrogen, carbon dioxide, argon and the like or under a reduced pressure of 400 mmHg to 0.01 mmHg and at a temperature of 180° C. to 220° C. By carrying out the solid phase reaction, the molecular weight can be additionally increased, and the raw materials that do not react in the melt reaction but only remain, as well as cyclic oligomers, acetaldehyde and the like generated during the reaction can be removed.

[0066] The solid phase reaction may be performed until the intrinsic viscosity of the crystallized polymer reaches 0.65 dl / g or more, 0.70 dl / g or more, 0.75 dl / g or more, or 0.80 dl / g or more, wherein the intrinsic viscosity is measured at 35° C. after dissolving the polymer at a concentration of 0.12 wt % in o-chlorophenol at 150° C.

[0067] In the extrusion blow molding (EBM) process, shear thinning properties are required, wherein the shear thinning properties maintain low viscosity in a high shear stress region inside the screw of the molding machine and exhibit high viscosity in a region where a parison with low shear stress is formed. Such shear thinning properties minimize the heat generated by shear stress friction inside the screw and reduce the temperature of the parison itself, thereby preventing friction heat from being generated at a temperature higher than the molding temperature set in the molding machine.

[0068] In case of multi-head extrusion blow molding with higher shear stress, several parisons are made by one screw, which leads to higher shear stress because the screw RPM becomes higher for more extrusion volume. Therefore, better shear thinning properties are required.

[0069] Dicarboxylic acid or its derivatives

[0070] The dicarboxylic acid component used in the present disclosure refers to the main monomer that constitutes the polyester copolymer together with the diol component. The term "dicarboxylic acid or its derivative" of the present disclosure means at least one compound selected from dicarboxylic acids and derivatives of dicarboxylic acids. In addition, the term 'derivative of dicarboxylic acid' means an alkyl ester of dicarboxylic acid (C1 to C4 lower alkyl ester, such as monomethyl ester, monoethyl ester, dimethyl ester, diethyl ester, dibutyl ester or the like) or a dicarboxylic anhydride. Thus, for example, terephthalic acid or its derivatives generally include compounds that react with a diol to form a terephthaloyl moiety, such as terephthalic acid; monoalkyl terephthalate or dialkyl terephthalate; and terephthalic anhydride.

[0071] Specifically, the residue of the dicarboxylic acid component of the present disclosure may include one or more residues selected from the group consisting of terephthalic acid, dimethyl terephthalic acid, hydroxyethyl terephthalic acid, and derivatives thereof. Specifically, terephthalic acid or its derivatives may be at least one selected from the group consisting of terephthalic acid, dimethyl terephthalic acid, hydroxyethyl terephthalic acid, recycled terephthalic acid, recycled dimethyl terephthalic acid, and recycled hydroxyethyl terephthalic acid.

[0072] In addition, the polyester copolymer may include an acid moiety derived from a comonomer other than terephthalic acid or its derivatives. Specifically, the comonomer may be at least one selected from the group consisting of an aromatic dicarboxylic acid or its derivatives having 8 to 14 carbon atoms and an aliphatic dicarboxylic acid or its derivatives having 4 to 12 carbon atoms. Examples of aromatic dicarboxylic acids or their derivatives having 8 to 14 carbon atoms include isophthalic acid, naphthalene dicarboxylic acids such as 2,6-naphthalene dicarboxylic acid, diphenyl dicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 2,5-furan dicarboxylic acid, 2,5-thiophene dicarboxylic acid and the like, but are not limited thereto. Examples of aliphatic dicarboxylic acids or derivatives thereof having 4 to 12 carbon atoms include linear aliphatic dicarboxylic acid components, branched aliphatic dicarboxylic acid components, or cyclic aliphatic dicarboxylic acid components, including cyclohexanedicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid, phthalic acid, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, fumaric acid, adipic acid, glutaric acid, and azelaic acid, but are not limited thereto. Specifically, the comonomer other than terephthalic acid or a derivative thereof may be at least one selected from the group consisting of isophthalic acid, 2,6-naphthalene dicarboxylic acid, adipic acid, azelaic acid, succinic acid, and 1,4-cyclohexanedicarboxylic acid.

[0073] The dicarboxylic acid or its derivatives may include terephthalic acid or its derivatives in an amount of greater than 70 mol % based on 100 mol % of the total dicarboxylic acids or their derivatives; and at least one selected from the group consisting of aromatic dicarboxylic acids or their derivatives having 8 to 14 carbon atoms and aliphatic dicarboxylic acids or their derivatives having 4 to 12 carbon atoms in an amount of 30 mol % or less based on 100 mol % of the total dicarboxylic acids or their derivatives.

[0074] Diol component

[0075] The diol component used in the present disclosure refers to the main monomer that constitutes the polyester copolymer together with the dicarboxylic acid component described above. In particular, in addition to ethylene glycol, the diol component may include diethylene glycol, neopentyl glycol or cyclohexanedimethanol as comonomers. In addition, recycled ethylene glycol, recycled diethylene glycol, recycled neopentyl glycol or recycled cyclohexanedimethanol may be used as monomers of the diol component.

[0076] Ethylene glycol is a component that helps improve transparency and impact strength of the polyester copolymer. Preferably, the residue of ethylene glycol may be included in an amount of 27.5 mol % to 39.0 mol % based on 100 mol % of the total residues.

[0077] Diethylene glycol is a component that helps improve the color of the polyester copolymer. Preferably, the amount of diethylene glycol may be 2.5 mol% to 6.5 mol% based on 100 mol% of the total residue.

[0078] Cyclohexanedimethanol (e.g., 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol or 1,4-cyclohexanedimethanol) is a component that helps improve the transparency and impact strength of the polyester copolymer to be prepared. Preferably, the diol moiety derived from cyclohexanedimethanol is contained in an amount of 6.5 mol% to 16.5 mol% based on the total diol moiety of the polyester copolymer.

[0079] Products containing polyester copolymers

[0080] According to one embodiment of the present disclosure, a product including a polyester copolymer may be provided.

[0081] Blend compositions comprising polyester copolymers

[0082] According to one embodiment of the present disclosure, a polyester copolymer blend composition including 5 wt % to 95 wt % of the polyester copolymer may be provided.

[0083] The blend composition may include a multi-layer structure.

[0084] Additionally, one embodiment of the present disclosure may provide a product including the polyester copolymer blend composition.

[0085] Beneficial Effects

[0086] The polyester copolymer of one embodiment of the present disclosure has low shrinkage stress and excellent shrinkage properties so as not to cause deformation of the container when applied to the container.

[0087] Furthermore, the polyester copolymer of one embodiment of the present disclosure may have a tear strength within an appropriate range, and thus may be easily removed from a container. DETAILED DESCRIPTION

[0088] Hereinafter, preferred embodiments are provided to help understand the present invention. However, the following embodiments are provided only for easier understanding of the present invention, and the present invention is not limited thereto.

[0089] Example 1

[0090] Step 1) Esterification reaction

[0091] TPA (terephthalic acid, 2300 g), EG (ethylene glycol, 810 g), CHDM (1,4-cyclohexanedimethanol, 650 g) and DEG (diethylene glycol, 170 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (0.1 g) was added thereto as a catalyst.

[0092] Then, nitrogen gas was injected into the reactor to form a pressurized state in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0093] Step 2) Polycondensation

[0094] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0095] Example 2

[0096] Step 1) Esterification reaction

[0097] TPA (terephthalic acid, 2300 g), EG (ethylene glycol, 1000 g), CHDM (1,4-cyclohexanedimethanol, 700 g) and DEG (diethylene glycol, 172 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (0.1 g) was added thereto as a catalyst.

[0098] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0099] Step 2) Polycondensation

[0100] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.68 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0101] Example 3

[0102] Step 1) Esterification reaction

[0103] TPA (terephthalic acid, 2300 g), EG (ethylene glycol, 805 g), CHDM (1,4-cyclohexanedimethanol, 654 g) and DEG (diethylene glycol, 190 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0104] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0105] Step 2) Polycondensation

[0106] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.75 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0107] Example 4

[0108] Step 1) Esterification reaction

[0109] TPA (terephthalic acid, 2400 g), EG (ethylene glycol, 880 g), CHDM (1,4-cyclohexanedimethanol, 360 g), CHDA (1,4-cyclohexanedicarboxylic acid, 300 g) and DEG (diethylene glycol, 170 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0110] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0111] Step 2) Polycondensation

[0112] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.75 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0113] Example 5

[0114] Step 1) Esterification reaction

[0115] TPA (terephthalic acid, 2200 g), EG (ethylene glycol, 760 g), CHDM (1,4-cyclohexanedimethanol, 710 g) and DEG (diethylene glycol, 200 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0116] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0117] Step 2) Polycondensation

[0118] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.72 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0119] Example 6

[0120] Step 1) Esterification reaction

[0121] TPA (terephthalic acid, 2220 g), EG (ethylene glycol, 730 g), CHDM (1,4-cyclohexanedimethanol, 750 g), NPG (neopentyl glycol, 50 g) and DEG (diethylene glycol, 150 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0122] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0123] Step 2) Polycondensation

[0124] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.72 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0125] Example 7

[0126] Step 1) Esterification reaction

[0127] TPA (terephthalic acid, 2260 g), EG (ethylene glycol, 790 g), CHDM (1,4-cyclohexanedimethanol, 670 g) and DEG (diethylene glycol, 150 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0128] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0129] Step 2) Polycondensation

[0130] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0131] Example 8

[0132] Step 1) Esterification reaction

[0133] TPA (terephthalic acid, 2300 g), EG (ethylene glycol, 870 g), CHDM (1,4-cyclohexanedimethanol, 570 g) and DEG (diethylene glycol, 140 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0134] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0135] Step 2) Polycondensation

[0136] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.72 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0137] Example 9

[0138] Step 1) Esterification reaction

[0139] TPA (terephthalic acid, 3000 g), EG (ethylene glycol, 1020 g), CHDM (1,4-cyclohexanedimethanol, 1000 g) and DEG (diethylene glycol, 230 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1 g) was added thereto as a catalyst.

[0140] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0141] Step 2) Polycondensation

[0142] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.73 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0143] Comparative Example 1

[0144] Step 1) Esterification reaction

[0145] TPA (terephthalic acid, 2500 g), EG (ethylene glycol, 1000 g), CHDM (1,4-cyclohexanedimethanol, 200 g) and DEG (diethylene glycol, 40 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1 g) was added thereto as a catalyst.

[0146] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0147] Step 2) Polycondensation

[0148] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.72 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0149] Comparative Example 2

[0150] Step 1) Esterification reaction

[0151] TPA (terephthalic acid, 2300 g), EG (ethylene glycol, 860 g), CHDM (1,4-cyclohexanedimethanol, 620 g) and DEG (diethylene glycol, 80 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0152] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0153] Step 2) Polycondensation

[0154] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.72 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0155] Comparative Example 3

[0156] Step 1) Esterification reaction

[0157] TPA (terephthalic acid, 2000 g), EG (ethylene glycol, 520 g), CHDM (1,4-cyclohexanedimethanol, 1230 g) and DEG (diethylene glycol, 130 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1 g) was added thereto as a catalyst.

[0158] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0159] Step 2) Polycondensation

[0160] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.74 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0161] Comparative Example 4

[0162] Step 1) Esterification reaction

[0163] TPA (terephthalic acid, 2000 g), EG (ethylene glycol, 830 g), CHDM (1,4-cyclohexanedimethanol, 300 g) and DEG (diethylene glycol, 150 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1 g) was added thereto as a catalyst.

[0164] Then, nitrogen is injected into the reactor to form a pressurized state, wherein the pressure of the reactor is 1.0 kgf / cm2 higher than normal pressure. Then, the temperature of the reactor is raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 260°C over 2 hours. Thereafter, esterification is carried out while the temperature of the reactor is maintained at 260°C until the mixture in the reactor becomes transparent to the naked eye. In the process, by-products flow through the column and condenser. When the esterification is completed, the nitrogen in the pressurized reactor is discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor is transferred to a 7L reactor capable of vacuum reaction.

[0165] Step 2) Polycondensation

[0166] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.75 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0167] Comparative Example 5

[0168] As Comparative Example 6, commercially available oriented polystyrene was used.

[0169] Comparative Example 6

[0170] Step 1) Esterification reaction

[0171] TPA (terephthalic acid, 2400 g), EG (ethylene glycol, 980 g), CHDM (1,4-cyclohexanedimethanol, 290 g), NPG (neopentyl glycol, 160 g) and DEG (diethylene glycol, 150 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0172] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0173] Step 2) Polycondensation

[0174] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0175] Comparative Example 7

[0176] Step 1) Esterification reaction

[0177] TPA (terephthalic acid, 2500 g), EG (ethylene glycol, 1010 g), CHDM (1,4-cyclohexanedimethanol, 170 g), NPG (neopentyl glycol, 260 g) and DEG (diethylene glycol, 90 g) were placed in a 10 L reactor connected to a column and a condenser capable of being cooled by water, and TiO2 (1.0 g) was added thereto as a catalyst.

[0178] Then, nitrogen gas was injected into the reactor to form a pressurized state, in which the pressure of the reactor was 1.0 kgf / cm higher than the normal pressure. 2 . Then, the temperature of the reactor was increased to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then increased to 260°C over 2 hours. Thereafter, the esterification reaction was carried out while maintaining the temperature of the reactor at 260°C until the mixture in the reactor became transparent to the naked eye. In the process, by-products flowed through the column and the condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside to reduce the pressure of the reactor to normal pressure, and then the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.

[0179] Step 2) Polycondensation

[0180] Then, the pressure of the 7L reactor is reduced from normal pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and the temperature of the reactor is increased to 280°C over 1 hour to carry out the polycondensation reaction, while the pressure of the reactor is maintained at 1 Torr (absolute pressure: 1 mmHg) or lower. In the initial stage of the polycondensation reaction, the stirring rate is set to high, but when the stirring force is weakened due to the increase in the viscosity of the reactants as the polycondensation reaction proceeds, or when the temperature of the reactants is increased to above the set temperature, the stirring rate can be appropriately adjusted. The polycondensation reaction is carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor becomes 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reaches the desired level, the polycondensation mixture is discharged from the reactor and made into strands. It is solidified and granulated with a cooling liquid to have an average weight of about 12 mg to 14 mg, thereby preparing a polyester copolymer.

[0181] The physical properties of the polyester copolymers of Examples 1 to 10 and Comparative Examples 1 to 9 were measured by the following methods and are shown in the following table.

[0182] Residue composition (method for determining the molar ratio of residues of linear diol monomers to residues of cyclic monomers)

[0183] After the sample was dissolved in a CDCl3 solvent at a concentration of 3 mg / mL, the residue composition (mol%) of the diol monomer and the residue composition (mol%) of the cyclic monomer in the polyester copolymer were confirmed by 1H-NMR spectrum obtained at 25°C using a nuclear magnetic resonance device (JEOL, 600MHz FT-NMR). In addition, the residue of TMA was confirmed by quantitative analysis of the spectrum, wherein the content of benzene-1,2,4-triethylcarboxylate produced by the reaction of ethanol with TMA by ethanolysis was measured at 250°C using gas chromatography (Agilent Technologies, 7890B). In addition, it was confirmed as the content (mol%) based on the total number of moles of carboxylic acid and diol parts.

[0184] Intrinsic viscosity (IV)

[0185] After the polyester copolymer was dissolved in o-chlorophenol (OCP, o-chlorophenol) at a concentration of 0.12% at 150° C., the intrinsic viscosity was measured using an Ubbelohde viscometer in a constant temperature bath at 35° C. Specifically, the time required for the solvent to pass between certain internal sections of the viscometer (outflow time; t0) and the time required for the solution to pass through the viscometer (t) were measured. Subsequently, the specific viscosity was calculated by substituting t0 and t into Equation 1, and the intrinsic viscosity was calculated by substituting the calculated specific viscosity into Equation 2.

[0186] [Equation 1]

[0187]

[0188] [Equation 2]

[0189]

[0190] Glass transition temperature (Tg)

[0191] The glass transition temperature of the prepared polyester copolymer was measured while heating the resin sample at 10 K / min in the range of 25° C. to 150° C.

[0192] Shrinkage stress

[0193] The shrinkage stress of the prepared polyester copolymer was obtained by inducing shrinkage in the vertical direction with hot air at 85°C, fixing both ends of the film, and measuring the final shrinkage stress (unit: mPa) in the vertical direction (TD direction) at 30°C.

[0194] Tear strength in machine direction

[0195] The tear strength of the prepared polyester copolymer is obtained by extruding the polyester copolymer prepared according to ASTM D1922 into a sheet having a thickness of 200 μm to 400 μm, stretching the sheet by 500% at 600 mm / min in a direction perpendicular to the machine direction at a temperature of 88° C., and dividing the measured value (k / gf) measured using a TGT-01 tear tester from Leading Instruments with a weight of 800 g by the measured film thickness (mm), thereby eliminating the influence factor by the film thickness.

[0196] [Table 1]

[0197]

[0198] [Table 2]

[0199]

[0200] [Table 3]

[0201]

[0202]

[0203] *A value = (residue of linear diol monomers other than ethylene glycol)*20 / ((residue of cyclic monomers)*2-99)

[0204] **Physical property factor = (A value) * 8.4-11.13

[0205] Referring to Comparative Examples 2 to 3 and Comparative Examples 5 to 7 in Table 3, when the A value does not satisfy the range of 2.0 or greater and 6.5 or less, there is a difference between the physical property factor value and the tear strength in the MD direction, or the tear strength in the MD direction is too large, exceeding 42.5 N / mm.

[0206] In the case of Comparative Example 1, the A value range is not satisfied, but the physical property factor value range is satisfied. However, the measured tear strength value is different from the physical property factor, and the measured shrinkage stress is too low at 2 MPa.

[0207] In the case of Comparative Example 4 in which the value of the physical property factor slightly exceeded 42.5, the measured tear strength exceeded 42.5 N / mm, and the shrinkage stress also exceeded 12 MPa.

[0208] Therefore, it was confirmed that when the polyester copolymer satisfies the A value of 2.0 to 6.5 and the physical property factor of greater than 0 and 42.5 or less, the tear strength can be evaluated without the step of stretching the resin and measuring the physical properties. In addition, it was confirmed that the polyester copolymer satisfying the A value range and the physical property factor has the tear strength and shrinkage stress suitable for use as a film in a packaging container.

Claims

1. A polyester copolymer having a structure in which an acid portion derived from a dicarboxylic acid or a derivative thereof and a diol portion derived from a diol including ethylene glycol are repeated, wherein the polyester copolymer comprises residues of linear diol monomers and residues of cyclic monomers, The value of A of the following equation 1 is 2.0 or more and 6.5 or less, and, The physical property factor value of the following equation 2 is greater than 0 and 42.5 or less: [Equation 1] A value = (residue content of linear diol monomers other than ethylene glycol (mol%)) * 20 / ((residue content of cyclic monomers (mol%)) * 2-99) [Equation 2] Physical property factor = (A value) * 8.4-11.13 In Equation 1, the content is based on 100 mol% of the total residues.

2. The polyester copolymer according to claim 1, The residue of the cyclic monomer is derived from at least one selected from the group consisting of 1,4-cyclohexanedimethanol, 1,4-cyclohexanedicarboxylic acid, terephthalic acid or its derivatives, recycled 1,4-cyclohexanedimethanol, recycled 1,4-cyclohexanedicarboxylic acid and recycled terephthalic acid or its derivatives.

3. The polyester copolymer according to claim 1, The residue of the linear diol monomer may be derived from at least one selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, recycled ethylene glycol, recycled diethylene glycol and recycled neopentyl glycol.

4. The polyester copolymer according to claim 1, Wherein the residue content of the linear diol monomer other than ethylene glycol in Formula 1 is 12.5 mol% or less based on 100 mol% of the total residues.

5. The polyester copolymer according to claim 1, Wherein the residue content of the cyclic monomer in Formula 1 is 56.5 mol% or more and 67.5 mol% or less based on 100 mol% of the total residues.

6. The polyester copolymer according to claim 1, wherein the polyester copolymer has a tear strength in a machine direction of 7.0 N / mm or more and 42.5 N / mm or less at 90°C.

7. The polyester copolymer according to claim 1, wherein the polyester copolymer has a shrinkage stress of 12.0 MPa or less at 85°C.

8. The polyester copolymer according to claim 7, The polyester copolymer has a shrinkage stress of 8.5 MPa or less at 85°C.

9. The polyester copolymer according to claim 1, Wherein the value of Equation 1 is 3.0 or more and 6.5 or less.

10. The polyester copolymer according to claim 1, Wherein the value of Equation 2 is greater than 5.0 and 42.5 or less.

11. The polyester copolymer according to claim 2, The terephthalic acid or a derivative thereof is at least one selected from the group consisting of terephthalic acid, dimethyl terephthalic acid, hydroxyethyl terephthalic acid, recycled terephthalic acid, recycled dimethyl terephthalic acid and recycled hydroxyethyl terephthalic acid.

12. A product comprising the polyester copolymer according to any one of claims 1 to 11.

13. A polyester copolymer blend composition comprising 5 wt% to 95 wt% of the polyester copolymer according to any one of claims 1 to 11.

14. A product comprising the polyester copolymer blend composition according to claim 13.