Iron casting and method of manufacturing same
By heat treatment of the austenite casting materials and adjusting the lattice arrangement of the austenite phase, the thermal expansion problem of iron castings is solved, and the low thermal expansion effect is achieved within a specific temperature range, which is suitable for a variety of applications.
Patent Information
- Application Number
- CN202380027030.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively reduce the thermal expansion coefficient of iron castings, especially within a temperature range of 50°C or more and 200°C or less.
By heat treatment of casting materials using an austenite system, the object for heat treatment is maintained at a first holding temperature of 850°C or above 1250°C and cooling it to a temperature of 150°C or above 150°C or below, the austenite is adjusted The lattice arrangement in the innoli phase reduces the linear expansion coefficient. The method includes a primary cooling and a secondary cooling process to optimize the cooling speed and termination temperature, further suppressing lattice deformation and volume changes.
The linear expansion coefficient of iron castings is significantly reduced and is suitable for a variety of uses, especially in use environments from 20°C to 100°C.
Smart Images

Figure BDA0005038463580000181 
Figure BDA0005038463580000191 
Figure BDA0005038463580000201
Abstract
Description
Technical Field
[0001] The present invention relates to an iron casting and a method for producing the same. Background Art
[0002] The abstract of Patent Document 1 states: A method for easily manufacturing a cast iron material having good castability and processability similar to general cast iron materials and having more excellent low thermal expansion characteristics is provided. In addition, the abstract of Patent Document 1 states: A casting having a cast iron composition containing carbon at a ratio of 2.5% by mass or less and nickel at a ratio of 25% by mass or more and 40% by mass or less is maintained at a temperature of 550°C to 700°C for more than 3 hours, and then subjected to annealing treatment, the annealing treatment comprising natural cooling to at least 200°C by furnace cooling, and then the casting after such annealing treatment is maintained at a temperature of 600°C to 1150°C for more than 1.5 hours, and then subjected to solution treatment including rapid cooling by fan air cooling, water cooling or oil cooling, thereby manufacturing a cast iron material having a thermal expansion coefficient of 4×10 -6 / ℃ low thermal expansion cast iron material.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-95747 Summary of the invention
[0006] Problems to be solved by the invention
[0007] Provided is an iron casting having reduced thermal expansion using an austenitic casting material.
[0008] Means for solving problems
[0009] A method in one embodiment of the present invention is a method for manufacturing an iron casting by heat treating a heat-treated object cast using an austenitic casting material. The casting material contains 26.0 mass% to 50.0 mass% Ni, 0.1 mass% to 3.5 mass% C, 0.1 mass% to 3.5 mass% Si, 0 mass% to 8.0 mass% Co, 0 mass% to 3.0 mass% Mn, and 0 mass% to 0.2 mass% Mg, with the remainder being Fe and inevitable elements. The heat treatment includes: a first holding step of holding the heat-treated object at a first holding temperature of 850°C to 1250°C; and a first cooling step of cooling the heat-treated object to a first cooling termination temperature of -150°C to 150°C after the first holding step. The first holding step includes holding the heat-treated object for a first holding time of 0.25 hours to 100 hours.
[0010] In this method, in the first holding process, the heat treatment object is maintained at a first holding temperature (850°C to 1250°C) and a first holding time (0.25 hours to 100 hours). And, in the first cooling process after the first holding process, the heat treatment object is cooled to a first cooling termination temperature (-150°C to 150°C). Through this first holding process, the solidification segregation of the solute elements in the heat treatment object can be reduced, and the relative difference (crystal orientation difference) of the crystal orientation inside each grain constituting the austenite phase can be reduced. Thus, the arrangement of the lattice in the austenite phase can be adjusted. As a result, the linear expansion coefficient of the iron casting can be reduced.
[0011] In this method, the first cooling step preferably includes cooling the heat treatment object at a first cooling rate of 0.01°C / min to 300°C / min. The first cooling rate is preferably 0.01°C / min to 20°C / min. The first holding time is preferably 2.5 hours to 25 hours. The first cooling termination temperature is preferably 0°C to 100°C.
[0012] In this method, preferably, the above-mentioned first cooling process includes: a primary cooling process, cooling the above-mentioned heat treatment object at a primary cooling rate; and a secondary cooling process, after the above-mentioned primary cooling process, cooling the above-mentioned heat treatment object at a secondary cooling rate greater than the above-mentioned primary cooling rate, the above-mentioned primary cooling process includes cooling the above-mentioned heat treatment object to a primary cooling termination temperature of not less than 250°C and not more than 950°C, and the above-mentioned secondary cooling process includes cooling the above-mentioned heat treatment object to the above-mentioned first cooling termination temperature.
[0013] In this method, the first cooling process after the first holding process includes: a primary cooling process, cooling the heat treatment object at a primary cooling rate; and a secondary cooling process, after the primary cooling process, cooling the heat treatment object at a secondary cooling rate greater than the primary cooling rate. Specifically, in the primary cooling process, the heat treatment object is cooled to a primary cooling termination temperature (above 250°C and below 950°C) at a primary cooling rate. Through this primary cooling process, the carbon in the austenite phase can be diffused to the graphite side. Therefore, the amount of solid solution carbon in the austenite phase can be reduced. Therefore, excessive deformation of the lattice in the austenite phase can be suppressed. As a result, the linear expansion coefficient of the iron casting can be further reduced. Furthermore, in the secondary cooling process after the primary cooling process, the heat treatment object is cooled to a first cooling termination temperature (above -150°C and below 150°C) at a secondary cooling rate greater than the primary cooling rate. Through this secondary cooling process, it is easy to increase the change in spontaneous volume magnetostriction associated with temperature changes below the Curie point. Therefore, in temperature changes below the Curie point, it is easy to make the volume change caused by spontaneous volume magnetostriction and the volume change caused by lattice vibration offset each other. Therefore, it is easy to suppress the volume change associated with temperature changes. As a result, it is easy to further reduce the linear expansion coefficient of the iron casting.
[0014] In this method, it is preferred that the primary cooling rate is 0.01°C / min to 20°C / min, and the secondary cooling rate is 1°C / min to 40,000°C / min. The secondary cooling rate is preferably 100°C / min to 40,000°C / min. The first holding time is preferably 2.5 hours to 25 hours. The primary cooling termination temperature is preferably 450°C to 850°C. The first cooling termination temperature is preferably 0°C to 100°C.
[0015] In the method, the heat treatment may also include: a second holding step, after the first cooling step, holding the heat treatment object at a second holding temperature of not less than 250°C and not more than 950°C; and a second cooling step, after the second holding step, cooling the heat treatment object to a second cooling termination temperature of not less than -150°C and not more than 150°C, and the second holding step includes holding the heat treatment object for a second holding time of not less than 0.25 hours and not more than 25 hours.
[0016] In this method, the first cooling step preferably includes cooling the heat-treated object at a first cooling rate of 0.01°C / min to 300°C / min. The first cooling rate is preferably 1°C / min to 50°C / min. The second cooling step preferably includes cooling the heat-treated object at a second cooling rate of 1°C / min to 40,000°C / min. The second cooling rate is preferably 100°C / min to 10,000°C / min. The first holding time is preferably 2.5 hours to 25 hours. The first cooling termination temperature is preferably 0°C to 100°C. The second holding temperature is preferably 550°C to 950°C. The second cooling termination temperature is preferably 0°C to 50°C.
[0017] In this method, the Co content of the casting material is preferably 0.1 mass% to 8.0 mass%. The Mn content of the casting material is preferably 0.01 mass% to 3.0 mass%. The Mg content of the casting material is preferably 0.01 mass% to 0.2 mass%.
[0018] Another embodiment of the present invention is a method for producing an iron casting by heat treating a heat-treated object cast using an austenitic casting material. The heat treatment includes: a first holding step of holding the heat-treated object at a first holding temperature of 850°C to 1250°C; and a first cooling step of cooling the heat-treated object to a first cooling end temperature of -150°C to 150°C after the first holding step. The first holding step includes holding the heat-treated object for a first holding time of 0.25 hours to 100 hours.
[0019] In this method, preferably, the above-mentioned first cooling process includes: a primary cooling process, cooling the above-mentioned heat treatment object at a primary cooling rate; and a secondary cooling process, after the above-mentioned primary cooling process, cooling the above-mentioned heat treatment object at a secondary cooling rate greater than the above-mentioned primary cooling rate, the above-mentioned primary cooling process includes cooling the above-mentioned heat treatment object to a primary cooling termination temperature of not less than 250°C and not more than 950°C, and the above-mentioned secondary cooling process includes cooling the above-mentioned heat treatment object to the above-mentioned first cooling termination temperature.
[0020] In the method, the heat treatment may also include: a second holding step, after the first cooling step, holding the heat treatment object at a second holding temperature of not less than 250°C and not more than 950°C; and a second cooling step, after the second holding step, cooling the heat treatment object to a second cooling termination temperature of not less than -150°C and not more than 150°C, and the second holding step holds the heat treatment object for a second holding time of not less than 0.25 hours and not more than 25 hours.
[0021] An iron casting according to one embodiment of the present invention is an iron casting produced using the method according to one embodiment of the present invention or the method according to another embodiment of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a diagram showing an example of an image obtained by observing the microstructure of a heat-treated object cast using an austenitic casting material through a microscope.
[0023] Figure 2 It is shown Figure 1 A plot of the area occupied by graphite in the images shown.
[0024] Figure 3 It is shown Figure 1 The image shown is a diagram of the region occupied by an intermetallic compound mainly composed of iron (Fe).
[0025] Figure 4 It is shown Figure 1 A diagram of the area occupied by the austenite phase in the image shown. DETAILED DESCRIPTION
[0026] Hereinafter, with reference to the accompanying drawings, an embodiment of the iron casting disclosed in the present invention will be described. The present invention is not limited to the following embodiments, including the contents specified in the claims. It should be noted that in the following description, unless otherwise specified, the terms "first", "second", etc. are used only to distinguish the constituent elements from each other, and do not indicate a specific order or sequence.
[0027] The iron casting of the embodiment of the present invention can be manufactured by subjecting a heat treatment object cast using an austenitic casting material to a heat treatment specified below. "Austenitic casting material" refers to a material in which the main structure of the parent phase (iron matrix structure other than graphite) of the cast heat treatment object at room temperature is an austenite phase. For example, the proportion of the austenite phase in the parent phase of the heat treatment object is 50% or more. The proportion of the austenite phase in the parent phase of the heat treatment object is preferably 70% or more, more preferably 80% or more, more preferably 85% or more, more preferably 90% or more, and further preferably 95% or more.
[0028] Figure 1 This is a diagram showing an example of an image obtained by observing the microstructure of a heat-treated object cast using an austenitic casting material through a microscope. Figure 2 It is shown Figure 1 A plot of the area occupied by graphite in the images shown. Figure 3 It is shown Figure 1 The image shown is a diagram of the region occupied by an intermetallic compound mainly composed of iron (Fe).
[0029] Figure 4 It is shown Figure 1 For example, the area of the parent phase of the heat-treated object can be obtained by Figure 1 The area of the entire microstructure of the heat-treated object is subtracted from Figure 2 The "area of the region occupied by graphite" shown in FIG. The "area of the austenite phase" can be calculated by subtracting the "area of the parent phase of the heat-treated object" calculated above from the "area of the parent phase of the heat-treated object" Figure 3 Therefore, the "ratio of the austenite phase in the parent phase of the heat-treated object" can be calculated by dividing the "area of the austenite phase (refer to Figure 4 )" divided by "the area of the parent phase of the heat treatment object". In this example, a general image processing software is used to calculate Figures 1 to 4 The number of pixels in the region corresponding to each area shown is 84.6% (about 85%) of the austenite phase in the parent phase of the heat-treated object. Figure 1 In the case where a region occupied by an intermetallic compound mainly composed of iron (Fe) is not formed, the ratio of the austenite phase to the parent phase of the heat-treated object is 100%.
[0030] In the present disclosure, "casting" includes casting using various casting methods such as sand casting, mold casting, die casting, lost wax casting, etc. In addition, the "mass %" of an element refers to the percentage of the mass of the element relative to the mass of the austenitic casting material. For example, the expression "an element of X mass % or more and Y mass % or less" means that the mass % of the element is X% or more and Y% or less. For example, the expression "an element of 0 mass % or less and Y mass % or less" means that the element is not included or the mass % of the element is Y% or less. "The remainder" refers to components other than the elements listed in the components constituting the austenitic casting material.
[0031] <First Form of Casting Material>
[0032] A first embodiment of an austenitic casting material (hereinafter referred to as "the present material") contains 26.0 mass % to 50.0 mass % Ni, with the remainder being Fe and inevitable elements. Hereinafter, the first embodiment of the present material may be referred to as "the first embodiment of the present material (Ni-Fe composition)".
[0033] (Ni: nickel)
[0034] The first mode of the present material comprises Ni of more than 26.0 mass % and less than 50.0 mass %. In the first mode of the present material, by making the content of Ni more than 26.0 mass % and less than 50.0 mass %, Ni is segregated around graphite. That is, by enriching Ni in the region around graphite, austenite is stabilized. By making the lower limit of the content of Ni be 26.0 mass %, austenite can be stabilized and the generation of martensite can be suppressed. Therefore, the reduction of the ductility of the iron casting can be suppressed, and the machinability of the iron casting can be improved. In addition, by making the upper limit of the content of Ni be 50.0 mass %, the increase of the linear expansion coefficient can be suppressed. The same is true in the following mode of the present material.
[0035] (Fe: Iron, an inevitable element)
[0036] The remainder in the first embodiment of the present material is Fe and inevitable elements. As the inevitable elements contained in the remainder, elements such as P (phosphorus), S (sulfur), Cu (copper), Al (aluminum), Cr (chromium), Mo (molybdenum), V (vanadium), Ti (titanium), and Zn (zinc) can be cited. The content of the inevitable elements is preferably less than 10.0 mass %, more preferably less than 5.0 mass %, more preferably less than 3.0 mass %, and further preferably less than 1.0 mass %. The same is true in the following embodiments of the present material.
[0037] In the first embodiment of the present material, the lower limit of the content of Ni is preferably 26.5 mass%, more preferably 27.0 mass%, more preferably 27.5 mass%, more preferably 28.0 mass%, more preferably 28.5 mass%, more preferably 29.0 mass%, more preferably 29.5 mass%, more preferably 30.0 mass%, more preferably 30.5 mass%, more preferably 31.0 mass%, more preferably 31.5 mass%, and more preferably 32.0 mass%. In addition, the upper limit of the content of Ni is preferably 45.0 mass%, more preferably 42.0 mass%, more preferably 41.0 mass%, more preferably 40.0 mass%, more preferably 39.5 mass%, more preferably 39.0 mass%, more preferably 38.5 mass%, more preferably 38.0 mass%, more preferably 37.5 mass%, and more preferably 37.0 mass%. The same is true in the following embodiments of the present material.
[0038] <Second Embodiment of Casting Material>
[0039] The second embodiment of the present material comprises 26.0 mass % to 50.0 mass % of Ni, 0.1 mass % to 3.5 mass % of C, and the remainder is Fe and inevitable elements. Hereinafter, the second embodiment of the present material may be referred to as "the second embodiment of the present material (Ni-C-Fe composition)".
[0040] (C: Carbon)
[0041] The second mode of the present material contains C of more than 0.1 mass % and less than 3.5 mass %. In the second mode of the present material, by making the lower limit of the content of C to 0.1 mass %, the liquidus temperature of the present material can be reduced. Therefore, the melt fluidity of the present material can be improved. In addition, by making the lower limit of the content of C to 0.1 mass %, the amount of crystallization or precipitation of graphite can be increased. Therefore, the machinability of the iron casting can be improved. In addition, by making the upper limit of the content of C to 3.5 mass %, graphite floating (carbon floatation) can be suppressed. Therefore, the reduction of the strength and ductility of the iron casting can be suppressed. In addition, by making the upper limit of the content of C to 3.5 mass % and making the upper limit of the content of Ni, which acts as a graphitization promoting element, to 50.0 mass %, the excessive graphitization of C can be suppressed. Therefore, the generation of fragmented graphite can be suppressed. Therefore, the elongation of the iron casting can be improved. The same is true in the following mode of the present material.
[0042] In the second embodiment of the present material, the lower limit of the content of C is preferably 0.15 mass%, more preferably 0.2 mass%, more preferably 0.4 mass%, more preferably 0.7 mass%, more preferably 1.0 mass%, more preferably 1.25 mass%, more preferably 1.5 mass%, and further preferably 1.75 mass%. By making the lower limit of the content of C 0.7 mass%, the tendency of the crystallized graphite to form a eutectic structure during solidification is increased, thereby increasing the expansion of graphite and suppressing the generation of shrinkage cavities. In addition, the upper limit of the content of C is preferably 3.3 mass%, more preferably 3.1 mass%, more preferably 3.0 mass%, more preferably 2.95 mass%, more preferably 2.9 mass%, more preferably 2.85 mass%, more preferably 2.8 mass%, more preferably 2.75 mass%, more preferably 2.7 mass%, more preferably 2.65 mass%, more preferably 2.6 mass%, more preferably 2.55 mass%, and further preferably 2.5 mass%. The same is true in the following embodiments of the present material.
[0043] <Third Embodiment of Casting Material>
[0044] The third embodiment of the present material comprises 26.0 mass % to 50.0 mass % of Ni, 0.1 mass % to 3.5 mass % of C, and 0.1 mass % to 3.5 mass % of Si, with the remainder being Fe and inevitable elements. Hereinafter, the third embodiment of the present material may be referred to as "the third embodiment of the present material (Ni-C-Si-Fe composition)".
[0045] (Si: Silicon)
[0046] The third mode of the present material includes Si of 0.1 mass % or more and 3.5 mass % or less. In the third mode of the present material, by making the content of Ni be 26.0 mass % or more and 50.0 mass % or less, and making the content of Si be 0.1 mass % or more and 3.5 mass % or less, Ni is segregated around the graphite, and as a result, Si is segregated in the final solidification part. That is, by enriching Ni in the area around the graphite to stabilize austenite, Si is enriched in the final solidification part as the residual liquid side. By making the lower limit of the content of Si be 0.1 mass %, it is easy to reduce the liquidus temperature of the present material. Therefore, it is easy to improve the melt fluidity of the present material. In addition, by making the lower limit of the content of Si be 0.1 mass %, the ratio of the content of Si to the content of C can be increased. Therefore, the formation of CO gas can be suppressed. Therefore, the gas defects generated on the surface of the iron casting can be reduced. In addition, by making the upper limit of the content of Si be 3.5 mass %, the solid solution amount of Si in Fe (iron matrix) can be reduced. Therefore, the increase of the linear expansion coefficient can be suppressed. In addition, by setting the upper limit of the content of Si, which acts as a graphitization promoting element, to 3.5 mass%, the excessive graphitization of C can be suppressed. Therefore, the generation of fragmented graphite can be suppressed. Therefore, the elongation of the iron casting can be improved. The same is true in the following manner of this material.
[0047] In the third embodiment of the present material, the lower limit of the content of Si is preferably 0.25 mass%, more preferably 0.5 mass%, more preferably 0.75 mass%, preferably 1.0 mass%, more preferably 1.2 mass%, more preferably 1.3 mass%, and further preferably 1.4 mass%. In addition, the upper limit of the content of Si is preferably 3.3 mass%, more preferably 3.1 mass%, more preferably 2.9 mass%, more preferably 2.7 mass%, more preferably 2.5 mass%, more preferably 2.3 mass%, and further preferably 2.1 mass%. The same is true in the following embodiments of the present material.
[0048] <Fourth Form of Casting Material>
[0049] The fourth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, and 0.1 mass % to 8.0 mass % Co, with the remainder being Fe and inevitable elements. Hereinafter, the fourth embodiment of the present material may be referred to as "the fourth embodiment of the present material (Ni-C-Si-Co-Fe composition)".
[0050] (Co: cobalt)
[0051] The fourth mode of the present material includes Co of more than 0.1 mass % and less than 8.0 mass %. In the fourth mode of the present material, by making the content of Co more than 0.1 mass % and less than 8.0 mass %, the linear expansion coefficient can be further reduced by the synergistic effect with Ni. By making the lower limit of the content of Co be 0.1 mass %, the minimum value of the linear expansion coefficient can be reduced by the synergistic effect with Ni. In addition, by making the upper limit of the content of Co be 8.0 mass %, it is possible to suppress the increase of the linear expansion coefficient after showing the minimum value with the excessive addition of Co. The same is true in the following mode of the present material.
[0052] In the fourth mode of this material, the lower limit of the content of Co is preferably 0.5 mass %, more preferably 1.0 mass %, more preferably 1.5 mass %, more preferably 2.0 mass %, more preferably 2.5 mass %, more preferably 3.0 mass %, more preferably 3.5 mass %, and more preferably 4.0 mass %. In addition, the upper limit of the content of Co is preferably 7.5 mass %, more preferably 7.0 mass %, more preferably 6.5 mass %, more preferably 6.25 mass %, and more preferably 6.0 mass %. In addition, relative to the content of Ni, it is 31.0 mass % or more and 34.0 mass % or less, and the content of Co is preferably 4.0 mass % or more and 5.5 mass % or less. In addition, when the lower limit of the content of Ni is 28.5 mass %, the content of Co is preferably 5.0 mass % or more and 8.0 mass % or less. By setting the lower limit and upper limit of the content of Co in this way, it is easy to further reduce the linear expansion coefficient by using the synergistic effect with Ni. The same is true in the following mode of this material.
[0053] <Fifth Form of Casting Material>
[0054] The fifth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, 0.1 mass % to 8.0 mass % Co, and 0.01 mass % to 3.0 mass % Mn, and the remainder is Fe and inevitable elements. Hereinafter, the fifth embodiment of the present material is sometimes referred to as "the fifth embodiment of the present material (Ni-C-Si-Co-Mn-Fe composition)".
[0055] (Mn: Manganese)
[0056] The fifth mode of this material comprises Mn of more than 0.01 mass % and less than 3.0 mass %. In the fifth mode of this material, by making the content of Mn be more than 0.01 mass % and less than 3.0 mass %, it is possible to utilize the synergistic effect with Ni to stabilize austenite and suppress the generation of martensite. Therefore, the machinability of iron castings can be improved. By making the lower limit of the content of Mn be 0.01 mass %, austenite can also be stabilized at room temperature. In addition, by making the upper limit of the content of Mn be 3.0 mass %, it is possible to reduce the solid solution amount of Mn in Fe (iron matrix). Therefore, the increase of linear expansion coefficient can be suppressed.
[0057] In the fifth embodiment of the present material, the lower limit of the content of Mn is preferably 0.05 mass%, more preferably 0.07 mass%, more preferably 0.08 mass%, more preferably 0.09 mass%, and further preferably 0.1 mass%. In addition, the upper limit of the content of Mn is preferably 2.5 mass%, more preferably 2.0 mass%, more preferably 1.5 mass%, more preferably 1.0 mass%, more preferably 0.85 mass%, and further preferably 0.7 mass%. The same is true in the following embodiments of the present material.
[0058] <Sixth Form of Casting Material>
[0059] The sixth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, 0.1 mass % to 8.0 mass % Co, and 0.01 mass % to 0.2 mass % Mg, with the remainder being Fe and inevitable elements. Hereinafter, the sixth embodiment of the present material is sometimes referred to as "the sixth embodiment of the present material (Ni-C-Si-Co-Mg-Fe composition)".
[0060] (Mg: magnesium)
[0061] The sixth embodiment of the present material contains Mg in an amount of 0.01 mass % to 0.2 mass %. In the sixth embodiment of the present material, by making the content of Mg to be 0.01 mass % to 0.2 mass %, the spheroidization of graphite can be improved, and Mg can be segregated in the final solidification portion. By making the lower limit of the content of Mg to 0.01 mass %, the spheroidization of graphite can be improved. In addition, by making the upper limit of the content of Mg to 0.2 mass %, the generation of Mg oxides or sulfides can be suppressed. Therefore, the reduction in the fluidity of the melt of the present material can be suppressed. Furthermore, the casting defects of the iron casting can be reduced.
[0062] In the sixth aspect of the present material, the lower limit of the Mg content is preferably 0.02 mass%, more preferably 0.03 mass%, and further preferably 0.04 mass%. In addition, the upper limit of the Mg content is preferably 0.15 mass%, more preferably 0.1 mass%, and further preferably 0.08 mass%. The same is true in the following aspects of the present material.
[0063] <Seventh Method of Casting Materials>
[0064] The seventh embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, 0.1 mass % to 8.0 mass % Co, 0.01 mass % to 3.0 mass % Mn, and 0.01 mass % to 0.2 mass % Mg, with the remainder being Fe and inevitable elements. Hereinafter, the seventh embodiment of the present material is sometimes referred to as "the seventh embodiment of the present material (Ni-C-Si-Co-Mn-Mg-Fe composition)".
[0065] <Eighth Form of Casting Material>
[0066] The eighth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, and 0.01 mass % to 3.0 mass % Mn, with the remainder being Fe and inevitable elements. Hereinafter, the eighth embodiment of the present material may be referred to as "the eighth embodiment of the present material (Ni-C-Si-Mn-Fe composition)".
[0067] <Ninth Form of Casting Material>
[0068] The ninth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, 0.01 mass % to 3.0 mass % Mn, and 0.01 mass % to 0.2 mass % Mg, with the remainder being Fe and inevitable elements. Hereinafter, the ninth embodiment of the present material may be referred to as "the ninth embodiment of the present material (Ni-C-Si-Mn-Mg-Fe composition)".
[0069] <Tenth Form of Casting Materials>
[0070] The tenth embodiment of the present material comprises 26.0 mass % to 50.0 mass % Ni, 0.1 mass % to 3.5 mass % C, 0.1 mass % to 3.5 mass % Si, and 0.01 mass % to 0.2 mass % Mg, with the remainder being Fe and inevitable elements. Hereinafter, the tenth embodiment of the present material may be referred to as "the tenth embodiment of the present material (Ni-C-Si-Mg-Fe composition)".
[0071] <First Method of Heat Treatment>
[0072] The first method of heat treatment of a heat treatment object cast using the present material (hereinafter referred to as "the present heat treatment") includes: a first holding step of holding the heat treatment object at a first holding temperature of 850°C to 1250°C; and a first cooling step of cooling the heat treatment object to a first cooling termination temperature of -150°C to 150°C after the first holding step. In the first method of the present heat treatment, the first holding step includes holding the heat treatment object for a first holding time of 0.25 hours to 100 hours. It should be noted that the first method of the present heat treatment may also include other heat treatment steps before and after each of the first holding step and the first cooling step. In the first method of the present heat treatment, when other heat treatment steps are not included before and after each of the above steps, by sequentially performing only the first holding step and the first cooling step on the heat treatment object cast using the present material, it is possible to prevent unexpected thermal effects on the heat treatment object. Therefore, the linear expansion coefficient of the iron casting can be more reliably reduced.
[0073] In the first mode of this heat treatment, in the first holding process, the heat treatment object is maintained at a first holding temperature (above 850°C and below 1250°C) and a first holding time (between 0.25 hours and below 100 hours). And, in the first cooling process after the first holding process, the heat treatment object is cooled to a first cooling termination temperature (above -150°C and below 150°C). Through this first holding process, the solidification segregation of the solute elements in the heat treatment object can be reduced, and the relative difference (crystal orientation difference) of the crystal orientation inside each grain constituting the austenite phase can be reduced. Thus, the arrangement of the lattice in the austenite phase can be adjusted. As a result, the linear expansion coefficient of the iron casting can be reduced.
[0074] In the first mode of the present heat treatment, the first cooling step includes cooling the heat treatment object at a first cooling rate of 0.01°C / min to 300°C / min. The first cooling rate is preferably 0.01°C / min to 20°C / min. The first holding time is preferably 2.5 hours to 25 hours. The first cooling termination temperature is preferably 0°C to 100°C.
[0075] In the first embodiment of the present heat treatment, the lower limit of the first holding temperature is preferably 875° C., more preferably 900° C., more preferably 925° C., more preferably 950° C., more preferably 975° C., more preferably 1000° C., and further preferably 1025° C. In addition, the upper limit of the first holding temperature is preferably 1225° C., more preferably 1200° C., more preferably 1175° C., more preferably 1150° C., and further preferably 1125° C. The same applies to the following embodiments of the present heat treatment.
[0076] In the first mode of this heat treatment, the lower limit of the first holding time is preferably 0.5 hour, more preferably 1.0 hour, more preferably 1.5 hours, more preferably 2.0 hours, more preferably 2.5 hours, more preferably 3.0 hours, more preferably 3.5 hours, more preferably 4.0 hours. In addition, the upper limit of the first holding time is preferably 90 hours, more preferably 80 hours, more preferably 70 hours, more preferably 60 hours, more preferably 50 hours, more preferably 40 hours, more preferably 30 hours, more preferably 25 hours, more preferably 20 hours, more preferably 15 hours, more preferably 10 hours. Also in the following mode of this heat treatment.
[0077] In the first embodiment of the present heat treatment, the lower limit of the first cooling end temperature is preferably -125°C, more preferably -100°C, more preferably -75°C, more preferably -50°C, more preferably -25°C, and further preferably 0°C. In addition, the upper limit of the first cooling end temperature is preferably 125°C, more preferably 100°C, more preferably 75°C, and further preferably 50°C. The same is true in the following embodiments of the present heat treatment.
[0078] In the first embodiment of the present heat treatment, the lower limit of the first cooling rate is preferably 0.1°C / minute, more preferably 0.2°C / minute, more preferably 0.3°C / minute, more preferably 0.4°C / minute, more preferably 0.5°C / minute, more preferably 0.6°C / minute, more preferably 0.7°C / minute, and further preferably 0.75°C / minute. In addition, the upper limit of the first cooling rate is preferably 250°C / minute, more preferably 200°C / minute, more preferably 150°C / minute, more preferably 100°C / minute, more preferably 50°C / minute, more preferably 25°C / minute, more preferably 10°C / minute, and further preferably 5°C / minute.
[0079] <Second Method of Heat Treatment>
[0080] The second mode of the heat treatment includes: a first holding step, holding the heat treatment object at a first holding temperature of 850°C to 1250°C; and a first cooling step, cooling the heat treatment object to a first cooling termination temperature of -150°C to 150°C after the first holding step. In the second mode of the heat treatment, the first holding step includes holding the heat treatment object for a first holding time of 0.25 hours to 100 hours. The first cooling step includes: a primary cooling step, cooling the heat treatment object at a primary cooling rate; and a secondary cooling step, after the primary cooling step, cooling the heat treatment object at a secondary cooling rate greater than the primary cooling rate. In the first cooling step, the primary cooling step includes cooling the heat treatment object to a primary cooling termination temperature of 250°C to 950°C. The secondary cooling step includes cooling the heat treatment object to a first cooling termination temperature (-150°C to 150°C). It should be noted that the second mode of the heat treatment may also include other heat treatment steps before and after each of the first holding step and the first cooling step. In the second mode of the present heat treatment, when no other heat treatment steps are included before and after the above steps, by sequentially performing only the first holding step and the first cooling step on the heat treatment object cast using the present material, it is possible to prevent unexpected thermal influences on the heat treatment object. Therefore, the linear expansion coefficient of the iron casting can be more reliably reduced.
[0081] In the second mode of this heat treatment, in the first holding process, the heat treatment object is maintained at a first holding temperature (above 850°C and below 1250°C) and a first holding time (between 0.25 hours and below 100 hours). And, in the first cooling process after the first holding process, the heat treatment object is cooled to a first cooling termination temperature (above -150°C and below 150°C). Through this first holding process, the solidification segregation of the solute elements in the heat treatment object can be reduced, and the relative difference (crystal orientation difference) of the crystal orientation inside each grain constituting the austenite phase can be reduced. Thus, the arrangement of the lattice in the austenite phase can be adjusted. As a result, the linear expansion coefficient of the iron casting can be reduced.
[0082] Furthermore, in the second mode of the present heat treatment, the first cooling process after the first holding process includes: a primary cooling process, cooling the heat treatment object at a primary cooling rate; and a secondary cooling process, after the primary cooling process, cooling the heat treatment object at a secondary cooling rate greater than the primary cooling rate. Specifically, in the primary cooling process, the heat treatment object is cooled to a primary cooling termination temperature (above 250°C and below 950°C) at a primary cooling rate. Through this primary cooling process, the carbon in the austenite phase can be diffused to the graphite side. Therefore, the amount of solid solution carbon in the austenite phase can be reduced. Therefore, excessive deformation of the lattice in the austenite phase can be suppressed. As a result, the linear expansion coefficient of the iron casting can be further reduced. Furthermore, in the secondary cooling process after the primary cooling process, the heat treatment object is cooled to a first cooling termination temperature (above -150°C and below 150°C) at a secondary cooling rate greater than the primary cooling rate. Through this secondary cooling process, it is easy to increase the change in spontaneous volume magnetostriction associated with temperature changes below the Curie point. Therefore, in temperature changes below the Curie point, it is easy to make the volume change caused by spontaneous volume magnetostriction and the volume change caused by lattice vibration offset each other. Therefore, it is easy to suppress the volume change associated with temperature changes. As a result, it is easy to further reduce the linear expansion coefficient of the iron casting.
[0083] In the second mode of the present heat treatment, it is preferred that the primary cooling rate is 0.01°C / min to 20°C / min, and the secondary cooling rate is 1°C / min to 40,000°C / min. The secondary cooling rate is preferably 100°C / min to 40,000°C / min. The first holding time is preferably 2.5 hours to 25 hours. The primary cooling termination temperature is preferably 450°C to 850°C. The first cooling termination temperature is preferably 0°C to 100°C.
[0084] In the second embodiment of the present heat treatment, the lower limit of the primary cooling end temperature is preferably 275°C, more preferably 300°C, more preferably 325°C, more preferably 350°C, more preferably 375°C, more preferably 400°C, more preferably 425°C, more preferably 450°C, more preferably 475°C, more preferably 500°C, more preferably 525°C, more preferably 550°C, more preferably 575°C, and further preferably 600°C. In addition, the upper limit of the primary cooling end temperature is preferably 925°C, more preferably 900°C, more preferably 875°C, more preferably 850°C, more preferably 825°C, and further preferably 800°C.
[0085] In the second embodiment of the present heat treatment, the lower limit of the primary cooling rate is preferably 0.1°C / min, more preferably 0.5°C / min, more preferably 0.75°C / min, more preferably 1.0°C / min, more preferably 1.25°C / min, more preferably 1.5°C / min, and further preferably 1.75°C / min. In addition, the upper limit of the primary cooling rate is preferably 17.5°C / min, more preferably 15.0°C / min, more preferably 12.5°C / min, more preferably 10.0°C / min, and further preferably 7.5°C / min.
[0086] In the second embodiment of the present heat treatment, the lower limit of the secondary cooling rate is preferably 2.5°C / min, more preferably 5°C / min, more preferably 7.5°C / min, more preferably 10°C / min, more preferably 50°C / min, more preferably 100°C / min, more preferably 200°C / min, more preferably 300°C / min, more preferably 400°C / min, more preferably 500°C / min, and further preferably 600°C / min. In addition, the upper limit of the secondary cooling rate is preferably 37500°C / min, more preferably 35000°C / min, more preferably 32500°C / min, more preferably 30000°C / min, more preferably 27500°C / min, and further preferably 25000°C / min.
[0087] <Third Method of Heat Treatment>
[0088] The third method of the heat treatment includes: a first holding step, holding the heat treatment object at a first holding temperature of 850°C to 1250°C; a first cooling step, cooling the heat treatment object to a first cooling termination temperature of -150°C to 150°C after the first holding step; a second holding step, holding the heat treatment object at a second holding temperature of 250°C to 950°C after the first cooling step; and a second cooling step, cooling the heat treatment object to a second cooling termination temperature of -150°C to 150°C after the second holding step. In the third method of the heat treatment, the first holding step includes holding the heat treatment object for a first holding time of 0.25 hours to 100 hours. The second holding step includes holding the heat treatment object for a second holding time of 0.25 hours to 25 hours. It should be noted that the third method of the heat treatment may also include other heat treatment steps before and after each of the first holding step, the first cooling step, the second holding step, and the second cooling step. In the third mode of the present heat treatment, when no other heat treatment steps are included before and after each of the above steps, by sequentially performing only the first holding step, the first cooling step, the second holding step, and the second cooling step on the heat treatment object cast using the present material, it is possible to prevent unexpected thermal influences on the heat treatment object. Therefore, the linear expansion coefficient of the iron casting can be more reliably reduced.
[0089] In the third mode of this heat treatment, in the first holding process, the heat treatment object is maintained at a first holding temperature (above 850°C and below 1250°C) and a first holding time (between 0.25 hours and below 100 hours). And, in the first cooling process after the first holding process, the heat treatment object is cooled to a first cooling termination temperature (above -150°C and below 150°C). Through this first holding process, the solidification segregation of the solute elements in the heat treatment object can be reduced, and the relative difference (crystal orientation difference) of the crystal orientation inside each grain constituting the austenite phase can be reduced. Thus, the arrangement of the lattice in the austenite phase can be adjusted. As a result, the linear expansion coefficient of the iron casting can be reduced.
[0090] Furthermore, in the third mode of the present heat treatment, in the second holding process after the first cooling process, the heat treatment object is maintained at a second holding temperature (above 250°C and below 950°C). And, in the second cooling process after the second holding process, the heat treatment object is cooled to a second cooling termination temperature (above -150°C and below 150°C). Through this second cooling process, it is easy to increase the change in spontaneous volume magnetostriction associated with temperature changes below the Curie point. Therefore, in temperature changes below the Curie point, it is easy to offset the volume change caused by spontaneous volume magnetostriction and the volume change caused by lattice vibration. Therefore, it is easy to suppress volume changes associated with temperature changes. As a result, it is easy to further reduce the linear expansion coefficient of the iron casting.
[0091] In the third mode of the present heat treatment, the first cooling process preferably includes cooling the heat treatment object at a first cooling rate of 0.01°C / minute to 300°C / minute. The first cooling rate is preferably 1°C / minute to 50°C / minute. The second cooling process preferably includes cooling the heat treatment object at a second cooling rate of 1°C / minute to 40,000°C / minute. The second cooling rate is preferably 100°C / minute to 10,000°C / minute. The first holding time is preferably 2.5 hours to 25 hours. The first cooling termination temperature is preferably 0°C to 100°C. The second holding temperature is preferably 550°C to 950°C. The second cooling termination temperature is preferably 0°C to 50°C.
[0092] In the third embodiment of the present heat treatment, the lower limit of the first cooling rate is preferably 1.0°C / minute, more preferably 5.0°C / minute, more preferably 7.5°C / minute, more preferably 10.0°C / minute, more preferably 12.0°C / minute, and further preferably 14.0°C / minute. In addition, the upper limit of the first cooling rate is preferably 250°C / minute, more preferably 200°C / minute, more preferably 150°C / minute, more preferably 100°C / minute, more preferably 75°C / minute, more preferably 50°C / minute, more preferably 45°C / minute, and further preferably 40°C / minute.
[0093] In the third embodiment of the present heat treatment, the lower limit of the second holding temperature is preferably 275°C, more preferably 300°C, more preferably 325°C, more preferably 350°C, more preferably 375°C, more preferably 400°C, more preferably 425°C, more preferably 450°C, more preferably 475°C, more preferably 500°C, more preferably 525°C, more preferably 550°C, more preferably 575°C, and further preferably 600°C. In addition, the upper limit of the second holding temperature is preferably 925°C, more preferably 900°C, more preferably 875°C, more preferably 850°C, more preferably 825°C, and further preferably 800°C.
[0094] In the third mode of this heat treatment, the lower limit of the second holding time is preferably 0.3 hour, more preferably 0.4 hour, more preferably 0.5 hour, more preferably 0.6 hour, more preferably 0.7 hour, more preferably 0.8 hour, more preferably 0.9 hour, and further preferably 1.0 hour. In addition, the upper limit of the second holding time is preferably 20 hours, more preferably 15 hours, more preferably 10 hours, more preferably 9 hours, more preferably 8 hours, more preferably 7 hours, more preferably 6 hours, and further preferably 5 hours.
[0095] In the third embodiment of the present heat treatment, the lower limit of the second cooling end temperature is preferably -125°C, more preferably -100°C, more preferably -75°C, more preferably -50°C, more preferably -25°C, and further preferably 0°C. In addition, the upper limit of the second cooling end temperature is preferably 125°C, more preferably 100°C, more preferably 75°C, more preferably 50°C, more preferably 40°C, and further preferably 30°C.
[0096] In the third embodiment of the present heat treatment, the lower limit of the second cooling rate is preferably 25°C / min, more preferably 50°C / min, more preferably 75°C / min, more preferably 100°C / min, more preferably 200°C / min, more preferably 300°C / min, and further preferably 400°C / min. In addition, the upper limit of the second cooling rate is preferably 35000°C / min, more preferably 30000°C / min, more preferably 25000°C / min, more preferably 20000°C / min, more preferably 15000°C / min, more preferably 10000°C / min, more preferably 9000°C / min, more preferably 8000°C / min, more preferably 7000°C / min, and further preferably 6000°C / min.
[0097] <First Embodiment>
[0098] The iron casting of the first embodiment is an iron casting obtained by performing the second embodiment of the present heat treatment on the heat treatment object cast using the fifth embodiment (Ni-C-Si-Co-Mn-Fe composition), the seventh embodiment (Ni-C-Si-Co-Mn-Mg-Fe composition), the eighth embodiment (Ni-C-Si-Mn-Fe composition) and the ninth embodiment (Ni-C-Si-Mn-Mg-Fe composition) of the present material. In the iron casting of the first embodiment, by performing the second embodiment of the present heat treatment, the linear expansion coefficient of the iron casting can be reduced as described above.
[0099] In addition, in the iron casting of the first embodiment, an austenitic casting material having a Ni content of 26.0% by mass or more is used to cast the heat treatment object, so that the Ms point (the temperature at which the phase transformation from austenite to martensite begins) is easily reduced. Therefore, it is easy to provide an iron casting that suppresses the generation of martensite. Furthermore, in the first holding process in the second mode of this heat treatment, the solidification segregation of the solute elements in the heat treatment object is reduced, and as a result, the final solidification portion Ni distributed in a low concentration in the heat treatment object can be highly concentrated. Thus, the Ms point of the final solidification portion can be further reduced. Therefore, in the first cooling process after the first holding process, when the heat treatment object is cooled to the first cooling termination temperature (above -150°C and below 150°C), the generation of martensite can be further suppressed. Therefore, it is possible to provide an iron casting that suppresses the generation of martensite while reducing thermal expansion. The same is true in the following embodiments.
[0100] <Second Embodiment>
[0101] The iron casting of the second embodiment is an iron casting obtained by performing the third embodiment of the present heat treatment on the heat treatment object cast using the fifth embodiment (Ni-C-Si-Co-Mn-Fe composition), the seventh embodiment (Ni-C-Si-Co-Mn-Mg-Fe composition) and the ninth embodiment (Ni-C-Si-Mn-Mg-Fe composition) of the present material. In the iron casting of the second embodiment, by performing the third embodiment of the present heat treatment, the linear expansion coefficient of the iron casting can be reduced as described above.
[0102] <Third Embodiment>
[0103] The iron casting of the third embodiment is an iron casting obtained by performing the first embodiment of the present heat treatment on the heat treatment object cast using the fifth embodiment (Ni-C-Si-Co-Mn-Fe composition), the seventh embodiment (Ni-C-Si-Co-Mn-Mg-Fe composition) and the ninth embodiment (Ni-C-Si-Mn-Mg-Fe composition) of the present material. In the iron casting of the third embodiment, by performing the first embodiment of the present heat treatment, the linear expansion coefficient of the iron casting can be reduced as described above.
[0104] According to the above-mentioned embodiment, an iron casting with reduced thermal expansion can be provided. Therefore, the iron casting of the above-mentioned embodiment is suitable for a variety of uses that require low thermal expansion (coefficient). Examples of uses of the iron casting of the above-mentioned embodiment include components such as semiconductor manufacturing equipment, electronic component manufacturing equipment, and machine tools. For example, as an application example in an environment of use of about 20°C to 50°C, in semiconductor manufacturing equipment, spindle brackets and calibration gauges (gauge blocks, etc.) can be cited, and in machine tool-related applications, workbenches and wire holding components of wire cutting machines can be cited. In addition, as an application example in an environment of use of about 20°C to 100°C (or 150°C), in semiconductor manufacturing equipment, dry vacuum pump components and probe card holders can be cited.
[0105] <Example>
[0106] Table 1 shows the composition of the examples in the first embodiment and the composition of the comparative examples relative to them. Table 2 shows the composition of the examples in the second embodiment and the composition of the comparative examples relative to them. Table 3 shows the composition of the examples in the third embodiment and the composition of the comparative examples relative to them. In Tables 1 to 3, the content (mass %) of C (carbon) is a value measured by combustion-infrared absorption method using the material carbon-sulfur analysis device "EMIA-Expert" made by Horiba, Ltd. In addition, the content (mass %) of Si (silicon), Ni (nickel), Mg (magnesium) and Co (cobalt) is a value measured by inductively coupled plasma emission spectrometry using the emission spectrometry analysis device "SPS3520UV" made by Hitachi High-Tech Science Corporation. In addition, the content (mass %) of other elements is a value measured by emission spectrometry using the emission spectrometry analysis device "PDA-8000" made by Shimadzu Corporation.
[0107] [Table 1]
[0108] (Table 1)
[0109]
[0110] [Table 2]
[0111] (Table 2)
[0112]
[0113] [Table 3]
[0114] (Table 3)
[0115]
[0116] Table 4 shows the heat treatment conditions and average linear expansion coefficients of the examples in the first embodiment, as well as the heat treatment conditions and average linear expansion coefficients of the comparative examples relative to them. Table 5 shows the heat treatment conditions and average linear expansion coefficients of the examples in the second embodiment, as well as the heat treatment conditions and average linear expansion coefficients of the comparative examples relative to them. Table 6 shows the heat treatment conditions and average linear expansion coefficients of the examples in the third embodiment, as well as the heat treatment conditions and average linear expansion coefficients of the comparative examples relative to them. In Tables 4 to 6, the holding temperature (°C) indicates the temperature at which the heat treatment object is maintained in the heat treatment furnace (heat treatment device). It should be noted that the heat treatment furnace uses a muffle furnace "QUICK TEMPER" manufactured by TEC Co., Ltd. In addition, the holding time (hours) indicates the time for which the heat treatment object is maintained in the state where the heat treatment furnace is kept at the holding temperature. In addition, the cooling method refers to a method of cooling the heat treatment object. Furnace cooling is a method of gradually cooling the heat treatment object in a heat treatment furnace. Natural air cooling is a method of cooling the heat treatment object in the air outside the heat treatment furnace. Rapid cooling is a method of rapidly cooling the heat treatment object by immersing it in water, oil, a coolant using dry ice, liquid nitrogen, etc. In addition, the cooling end temperature (°C) refers to the temperature at which the cooling of the heat treatment object based on the cooling method is terminated. The cooling end temperature during furnace cooling is the surface temperature of the heat treatment object measured in the heat treatment furnace by bringing the temperature measuring part of the thermocouple into contact with the heat treatment object in the heat treatment furnace. The cooling end temperature during natural air cooling and rapid cooling is the surface temperature of the heat treatment object measured outside the heat treatment furnace by bringing the temperature measuring part of the thermocouple into contact with the heat treatment object outside the heat treatment furnace. In addition, the cooling rate (°C / minute) or (°C / second) refers to the temperature change relative to the time from the start of cooling of the heat treatment object to the end. In addition, the average linear expansion coefficient (×10 -6 / °C) is a value obtained by collecting a linear expansion coefficient measurement test piece (6 mm in diameter, 25 mm in length) from an iron casting (Y-shaped B-size test material) after a prescribed heat treatment is performed on a heat treatment object cast by a sand casting method, and measuring the test piece using a thermal dilatometer "DIL 402 Expedis Supreme" manufactured by NETZSCH Japan Co., Ltd. in accordance with ASTM standards (ASTM E228-17), indicating an average linear expansion coefficient from 20°C as a reference to each temperature (50°C, 100°C, 150°C) in Tables 4 to 6.
[0117] [Table 4]
[0118]
[0119] [Table 5]
[0120]
[0121] [Table 6]
[0122]
[0123] (Comparison of Examples 1-1 to 1-30 with Comparative Example 1-1)
[0124] As shown in Table 4, the primary cooling termination temperature of Examples 1-1 to 1-30 is 950°C or less, whereas the primary cooling termination temperature of Comparative Example 1-1 is 1000°C. As shown in Table 4, in Examples 1-1 to 1-30, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared with Comparative Example 1-1. Specifically, in Examples 1-1 to 1-30, the average linear expansion coefficient of 20°C to 50°C is 3.51×10 -6 / ℃ or less (Comparative Example 1-1 is 3.63×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 3.58×10 -6 / ℃ or less (Comparative Example 1-1 is 3.90×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.09×10 -6 / ℃ or less (Comparative Example 1-1 is 4.28×10 -6 / °C). Thus, in Examples 1-1 to 1-30, by setting the primary cooling end temperature to 950°C or lower (particularly 900°C or lower), the thermal expansion of the iron casting can be reduced.
[0125] (Comparison of Examples 1-1 to 1-30 with Comparative Example 1-2)
[0126] As shown in Table 4, the primary cooling termination temperature of Examples 1-1 to 1-30 is 250°C or higher, whereas the primary cooling termination temperature of Comparative Example 1-2 is 200°C. As shown in Table 4, in Examples 1-1 to 1-30, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared with Comparative Example 1-2. Specifically, in Examples 1-1 to 1-30, the average linear expansion coefficient of 20°C to 50°C is 3.51×10 -6 / ℃ or less (Comparative Example 1-2 is 4.98×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 3.58×10 -6 / ℃ or less (Comparative Example 1-2 is 4.87×10-6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.09×10 -6 / ℃ or less (Comparative Example 1-2 is 4.87×10 -6 / °C). Thus, in Examples 1-1 to 1-30, by setting the primary cooling end temperature to 250°C or higher (particularly 300°C or higher), the thermal expansion of the iron casting can be reduced.
[0127] (Comparison of Examples 2-1 to 2-26 with Comparative Example 2-1)
[0128] As shown in Table 5, the second holding temperature of Examples 2-1 to 2-26 is 950°C or less, whereas the second holding temperature of Comparative Example 2-1 is 1000°C. As shown in Table 5, in Examples 2-1 to 2-26, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared to Comparative Example 2-1. Specifically, in Examples 2-1 to 2-26, the average linear expansion coefficient of 20°C to 50°C is 3.30×10 -6 / ℃ or less (Comparative Example 2-1 is 3.54×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 3.55×10 -6 / ℃ or less (Comparative Example 2-1 is 3.78×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.05×10 -6 / ℃ or less (Comparative Example 2-1 is 4.15×10 -6 / °C). Thus, in Examples 2-1 to 2-26, by setting the second holding temperature to 950°C or lower (particularly 900°C or lower), the thermal expansion of the iron casting can be reduced.
[0129] (Comparison of Examples 2-1 to 2-26 with Comparative Example 2-2)
[0130] As shown in Table 5, the second holding temperature of Examples 2-1 to 2-26 is 250°C or higher, whereas the second holding temperature of Comparative Example 2-2 is 200°C. As shown in Table 5, in Examples 2-1 to 2-26, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared to Comparative Example 2-2. Specifically, in Examples 2-1 to 2-26, the average linear expansion coefficient of 20°C to 50°C is 3.30×10 -6 / ℃ or less (Comparative Example 2-2 is 5.57×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 3.55×10 -6 / ℃ or less (Comparative Example 2-2 is 5.47×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.05×10 -6 / ℃ or less (Comparative Example 2-2 is 5.40×10 -6 / °C). Thus, in Examples 2-1 to 2-26, by setting the second holding temperature to 250°C or higher (particularly 300°C or higher), the thermal expansion of the iron casting can be reduced.
[0131] (Comparison of Examples 3-1 to 3-13 with Comparative Example 3-1)
[0132] As shown in Table 6, the first holding temperature of Examples 3-1 to 3-13 is 850°C or higher, whereas the first holding temperature of Comparative Example 3-1 is 800°C. As shown in Table 6, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared to Comparative Example 3-1. Specifically, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C is 3.80×10 -6 / ℃ or less (Comparative Example 3-1 is 4.53×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 4.16×10 -6 / ℃ or less (Comparative Example 3-1 is 5.02×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.84×10 -6 / ℃ or less (Comparative Example 3-1 is 5.58×10 -6 / °C). Thus, in Examples 3-1 to 3-13, by setting the first holding temperature to 850°C or higher (particularly 950°C or higher), the thermal expansion of the iron casting can be reduced.
[0133] (Comparison of Examples 3-1 to 3-13 with Comparative Example 3-2)
[0134] As shown in Table 6, the first holding temperature of Examples 3-1 to 3-13 is 850°C or higher, whereas the first holding temperature of Comparative Example 3-2 is 800°C. As shown in Table 6, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C and the average linear expansion coefficient of 20°C to 100°C are respectively reduced compared to Comparative Example 3-2. Specifically, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C is 3.80×10 -6 / ℃ or less (Comparative Example 3-2 is 3.89×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 4.16×10 -6 / ℃ or less (Comparative Example 3-2 is 4.17×10 -6 / °C). Thus, in Examples 3-1 to 3-13, by setting the first holding temperature to 850°C or higher (particularly 950°C or higher), the thermal expansion of the iron casting can be reduced.
[0135] (Comparison of Examples 3-1 to 3-13 with Comparative Example 3-3)
[0136] As shown in Table 6, the first holding temperature of Examples 3-1 to 3-13 is 1250°C or less, whereas the first holding temperature of Comparative Example 3-3 is 1300°C. As shown in Table 6, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C, the average linear expansion coefficient of 20°C to 100°C, and the average linear expansion coefficient of 20°C to 150°C are respectively reduced compared with Comparative Example 3-3. Specifically, in Examples 3-1 to 3-13, the average linear expansion coefficient of 20°C to 50°C is 3.80×10 -6 / ℃ or less (Comparative Example 3-3 is 5.87×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 100℃ is 4.16×10 -6 / ℃ or less (Comparative Example 3-3 is 5.72×10 -6 / ℃), the average linear expansion coefficient between 20℃ and 150℃ is 4.84×10 -6 / ℃ or less (Comparative Example 3-3 is 5.67×10 -6 / °C). Thus, in Examples 3-1 to 3-13, by setting the first holding temperature to 1250°C or lower (particularly 1200°C or lower), the thermal expansion of the iron casting can be reduced.
[0137] (Comparison of Example 3-9 with Comparative Example 3-1 and Comparative Example 3-3)
[0138] As shown in Table 3, the casting materials of Example 3-9, Comparative Example 3-1 and Comparative Example 3-3 do not contain Co. In addition, as shown in Table 6, the first holding temperature of Example 3-9 is 850°C to 1250°C, while the first holding temperature of Comparative Example 3-1 is 800°C and the first holding temperature of Comparative Example 3-3 is 1300°C. As shown in Table 6, when Example 3-9, which does not contain Co, is compared with Comparative Example 3-1 and Comparative Example 3-3, the average linear expansion coefficient of 20°C to 150°C in Example 3-9 is lower than that in Comparative Example 3-1 and Comparative Example 3-3. Specifically, in Example 3-9, the average linear expansion coefficient of 20°C to 150°C is 4.84×10 -6 / ℃ or less (Comparative Example 3-1 is 5.58×10 -6 / ℃, and Comparative Example 3-3 is 5.67×10 -6 / °C). Thus, in Example 3-9, by not containing Co and setting the first holding temperature to 850°C or more and 1250°C or less, the thermal expansion of the iron casting at a high temperature can be reduced.
[0139] (Comparison of Examples 3-1 to 3-8 and Examples 3-10 to 3-13 with Comparative Example 3-2)
[0140] As shown in Table 3, the casting materials of Examples 3-1 to 3-8, Examples 3-10 to 3-13, and Comparative Example 3-2 contain Co. In addition, as shown in Table 6, the first holding temperature of Examples 3-1 to 3-8 and Examples 3-10 to 3-13 is 850°C to 1250°C, while the first holding temperature of Comparative Example 3-2 is 800°C. As shown in Table 6, when Examples 3-1 to 3-8 and Examples 3-10 to 3-13, all of which contain Co, are compared with Comparative Example 3-2, in Examples 3-1 to 3-8 and Examples 3-10 to 3-13, the average linear expansion coefficient of 20°C to 150°C is lower than that of Comparative Example 3-2. Specifically, in Examples 3-1 to 3-8 and Examples 3-10 to 3-13, the average linear expansion coefficient of 20°C to 150°C is 4.49×10 -6 / ℃ or less (Comparative Example 3-2 is 4.53×10 -6 / °C). Thus, in Examples 3-1 to 3-8 and Examples 3-10 to 3-13, by containing Co and setting the first holding temperature to 850°C or higher and 1250°C or lower, thermal expansion of the iron casting at high temperature can be reduced.
[0141] In addition, the present disclosure can also adopt the following configurations. (1)
[0143] An iron casting obtained by subjecting a heat treatment object cast using an austenitic casting material to a first heat treatment, wherein:
[0144] The first heat treatment includes maintaining the heat treatment object in a first temperature range of 950° C. to 1200° C. (2)
[0146] The iron casting according to (1), wherein the heat treatment object is maintained in the first temperature range for a time period of not less than 1 hour and not more than 100 hours. (3)
[0148] The iron casting as described in (1) or (2), wherein after the first heat treatment, the heat treatment object is subjected to a second heat treatment.
[0149] The second heat treatment includes cooling the heat treatment object to a second temperature range of 300° C. to 900° C. (4)
[0151] The iron casting according to (3), wherein cooling to the second temperature range includes cooling the heat treatment object within a cooling rate range of 0.01° C. / min to 20° C. / min. (5)
[0153] The iron casting as described in (3) or (4), wherein after the second heat treatment, the heat treatment object is subjected to a third heat treatment.
[0154] The third heat treatment includes cooling the heat treatment object to a third temperature range of 0° C. to 100° C. inclusive. (6)
[0156] The iron casting according to (5), wherein cooling to the third temperature range includes cooling the heat treatment object within a cooling rate range of 1° C. / sec to 1000° C. / sec. (7)
[0158] The iron casting according to any one of (1) to (6), wherein the casting material contains 26.0 mass % to 42.0 mass % of Ni, and the remainder is Fe and inevitable elements. (8)
[0160] The iron casting according to (7), wherein the casting material further contains 0.3 mass % to 3.5 mass % of C. (9)
[0162] The iron casting according to (7) or (8), wherein the casting material further contains 0.1 mass % to 3.0 mass % of Si. (10)
[0164] The iron casting according to any one of (7) to (9), wherein the casting material further contains 0.001 mass % to 8.0 mass % of Co. (11)
[0166] A method for manufacturing an iron casting, comprising performing a first heat treatment on a heat treatment object cast using an austenitic casting material, wherein:
[0167] The first heat treatment includes maintaining the heat treatment object in a first temperature range of 950° C. to 1200° C. (12)
[0169] The manufacturing method described in (11), wherein the heat treatment object is maintained in the first temperature range for a time period of not less than 1 hour and not more than 100 hours. (13)
[0171] The manufacturing method as described in (11) or (12), wherein after performing the first heat treatment, the method further includes performing a second heat treatment on the heat treatment object.
[0172] The second heat treatment includes cooling the heat treatment object to a second temperature range of 300° C. to 900° C. inclusive. (14)
[0174] The manufacturing method described in (13), wherein cooling to the second temperature range includes cooling the heat treatment object within a cooling rate range of 0.01° C. / min to 20° C. / min. (15)
[0176] The manufacturing method as described in (13) or (14), wherein after performing the second heat treatment, the method further includes performing a third heat treatment on the heat treatment object.
[0177] The third heat treatment includes cooling the heat treatment object to a third temperature range of 0° C. to 100° C. inclusive. (16)
[0179] The manufacturing method described in (15), wherein cooling to the third temperature range includes cooling the heat treatment object within a cooling rate range of 1°C / sec to 1000°C / sec.
Claims
1. A method for producing an iron casting, the method comprising: heat-treating a heat-treatable object cast using an austenitic casting material to produce an iron casting, wherein: The casting material comprises 26.0 mass % to 50.0 mass % of Ni, 0.1 mass % to 3.5 mass % of C, 0.1 mass % to 3.5 mass % of Si, 0 mass % to 8.0 mass % of Co, 0 mass % to 3.0 mass % of Mn, and 0 mass % to 0.2 mass % of Mg, with the remainder being Fe and inevitable elements. The heat treatment comprises: A first holding step of holding the heat treatment object at a first holding temperature of 850° C. to 1250° C.; and a first cooling step of cooling the heat-treated object to a first cooling end temperature of not less than -150° C. and not more than 150° C. after the first holding step; The first holding step includes holding the heat treatment object for a first holding time of not less than 0.25 hours and not more than 100 hours.
2. The method for producing an iron casting according to claim 1, wherein: The first cooling step includes cooling the heat treatment object at a first cooling rate of 0.01° C. / min to 300° C. / min.
3. The method for producing an iron casting according to claim 2, wherein: The first cooling rate is 0.01° C. / minute to 20° C. / minute.
4. The method for producing an iron casting according to any one of claims 1 to 3, wherein: The first holding time is not less than 2.5 hours and not more than 25 hours.
5. The method for producing an iron casting according to any one of claims 1 to 4, wherein: The first cooling end temperature is 0° C. or higher and 100° C. or lower.
6. The method for producing an iron casting according to claim 1, wherein: The first cooling process comprises: a primary cooling step of cooling the heat treatment object at a primary cooling rate; and a secondary cooling step of cooling the heat treatment object at a secondary cooling rate greater than the primary cooling rate after the primary cooling step, The primary cooling step includes cooling the heat-treated object to a primary cooling end temperature of 250° C. to 950° C., The secondary cooling step includes cooling the heat treatment object to the first cooling end temperature.
7. The method for producing an iron casting according to claim 6, wherein: The primary cooling rate is 0.01°C / min to 20°C / min. The secondary cooling rate is not less than 1° C. / minute and not more than 40000° C. / minute.
8. The method for producing an iron casting according to claim 7, wherein: The secondary cooling rate is not less than 100° C. / minute and not more than 40000° C. / minute.
9. The method for producing an iron casting according to any one of claims 6 to 8, wherein: The first holding time is not less than 2.5 hours and not more than 25 hours.
10. The method for producing an iron casting according to any one of claims 6 to 9, wherein: The primary cooling termination temperature is 450°C or higher and 850°C or lower.
11. The method for producing an iron casting according to any one of claims 6 to 10, wherein: The first cooling end temperature is 0° C. or higher and 100° C. or lower.
12. The method for producing an iron casting according to claim 1, wherein: The heat treatment further comprises: a second holding step of holding the heat treatment object at a second holding temperature of 250° C. to 950° C., both inclusive, after the first cooling step; and a second cooling step of cooling the heat-treated object to a second cooling end temperature of not less than -150°C and not more than 150°C after the second holding step; The second holding step includes holding the heat treatment object for a second holding time of not less than 0.25 hours and not more than 25 hours.
13. The method for producing an iron casting according to claim 12, wherein: The first cooling step includes cooling the heat treatment object at a first cooling rate of 0.01° C. / min to 300° C. / min.
14. The method for producing an iron casting according to claim 13, wherein: The first cooling rate is 1° C. / minute to 50° C. / minute.
15. The method for producing an iron casting according to any one of claims 12 to 14, wherein: The second cooling step includes cooling the heat treatment object at a second cooling rate of 1° C. / minute to 40000° C. / minute.
16. The method for producing an iron casting according to claim 15, wherein: The second cooling rate is not less than 100° C. / minute and not more than 10000° C. / minute.
17. The method for producing an iron casting according to any one of claims 12 to 16, wherein: The first holding time is not less than 2.5 hours and not more than 25 hours.
18. The method for producing an iron casting according to any one of claims 12 to 17, wherein: The first cooling end temperature is 0° C. or higher and 100° C. or lower.
19. The method for producing an iron casting according to any one of claims 12 to 18, wherein: The second holding temperature is 550° C. or higher and 950° C. or lower.
20. The method for producing an iron casting according to any one of claims 12 to 19, wherein: The second cooling end temperature is 0° C. or higher and 50° C. or lower.
21. The method for producing an iron casting according to any one of claims 1 to 20, wherein: The Co content of the casting material is 0.1 mass % or more and 8.0 mass % or less.
22. The method for producing an iron casting according to any one of claims 1 to 21, wherein: The Mn content of the casting material is 0.01 mass % or more and 3.0 mass % or less.
23. The method for producing an iron casting according to any one of claims 1 to 22, wherein: The Mg content of the casting material is 0.01 mass % or more and 0.2 mass % or less.
24. A method for producing an iron casting, the method producing the iron casting by heat-treating a heat-treatable object cast using an austenitic casting material, wherein: The heat treatment comprises: A first holding step of holding the heat treatment object at a first holding temperature of 850° C. to 1250° C.; and a first cooling step of cooling the heat-treated object to a first cooling end temperature of not less than -150° C. and not more than 150° C. after the first holding step; The first holding step includes holding the heat treatment object for a first holding time of not less than 0.25 hours and not more than 100 hours.
25. A method of manufacturing an iron casting as claimed in claim 24, wherein: The first cooling process comprises: a primary cooling step of cooling the heat treatment object at a primary cooling rate; and a secondary cooling step of cooling the heat treatment object at a secondary cooling rate greater than the primary cooling rate after the primary cooling step, The primary cooling step includes cooling the heat-treated object to a primary cooling end temperature of 250° C. to 950° C., The secondary cooling step includes cooling the heat treatment object to the first cooling end temperature.
26. The method of manufacturing an iron casting as claimed in claim 24, wherein: The heat treatment further comprises: a second holding step of holding the heat treatment object at a second holding temperature of 250° C. to 950° C., both inclusive, after the first cooling step; and a second cooling step of cooling the heat-treated object to a second cooling end temperature of not less than -150°C and not more than 150°C after the second holding step; The second holding step includes holding the heat treatment object for a second holding time of not less than 0.25 hours and not more than 25 hours.