Machine component

By using quenching and tempering steel on the bearing components and forming a nitriding layer, and combining low-temperature treatment to improve the martensite dislocation density, the problem of insufficient static load capacity of bearing components in the prior art is solved, and a higher static load capacity is achieved and hardness, suitable for efficient miniaturization applications such as electric vehicles and hydrogen utilization equipment.

CN118922572APending Publication Date: 2024-11-08NTN CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029142.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The static load capacity of existing bearing components still has room for improvement in some applications, especially in electric vehicles, hybrid vehicles and hydrogen utilization equipment, which affects the miniaturization and efficiency improvement of components.

Method used

Using mechanical components made of quenched and tempered steel, a nitriding layer is formed on the surface, with a steel content of 0.95%~1.10%, less than 0.30% silicon, less than 0.50% manganese, less than 0.0080% sulfur and 1.3%~1.6% of chromium, the surface nitrogen concentration is above 0.10%, and the residual austenite volume is below 20 volume %. The martensite dislocation density is increased by low temperature treatment, satisfying specific X-ray diffraction conditions and maximum contact surface pressure. Trace depth requirements.

Benefits of technology

It significantly improves the static load capacity of bearing components to reach more than 6.0GPa, improves hardness and wear resistance, and meets the needs of miniaturization and efficient application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922572A_ABST
    Figure CN118922572A_ABST
Patent Text Reader

Abstract

The machine component (10) has a surface and is made of quenched and tempered steel. The machine component is provided with a nitrided layer (11) formed on a surface (10a, 10b, 10c, 10d). The steel contains 0.95% by mass to 1.10% by mass (inclusive) of carbon, less than 0.30% by mass of silicon, less than 0.50% by mass of manganese, less than 0.0080% by mass of sulfur, and 1.3% by mass to 1.6% by mass (inclusive) of chromium, with the remainder comprising iron and unavoidable impurities. The average nitrogen concentration of the surface is 0.10 mass% or more. And the hardness of the surface is more than 850 Hv. The amount of retained austenite on the surface is 20 vol% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to mechanical components. Background Art

[0002] For example, Japanese Patent Laid-Open No. 2013-119930 (Patent Document 1) describes a bearing component. The bearing component described in Patent Document 1 contacts other components on the surface. The bearing component described in Patent Document 1 is made of steel that has been quenched and tempered. The steel contains 0.90 mass % to 1.05 mass % carbon, 0.15 mass % to 0.35 mass % silicon, 0.01 mass % to 0.50 mass % manganese, and 1.30 mass % to 1.65 mass % chromium, and the remainder is composed of iron and unavoidable impurities.

[0003] In the bearing component described in Patent Document 1, the surface is nitrided to a nitrogen concentration of 0.25 mass % or more, and the amount of retained austenite on the surface of the bearing component described in Patent Document 1 is 6 volume % or more and 12 volume % or less. In the bearing component described in Patent Document 1, the static load capacity of the surface is improved by tempering at a high temperature.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2013-119930 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] Bearings are used in electric motors, transmissions, differentials, etc. installed in electric vehicles (BEVs). In addition, bearings are also used in electric VTCs (variable valve trains), electric compressors, transmission systems, axles, etc. installed in plug-in hybrid vehicles (PHVs), hybrid vehicles (HVs), and engine vehicles. In these applications, if the static load capacity of the bearing is increased, the bearing can be miniaturized, and even the surrounding mechanical parts can be miniaturized.

[0009] Even for bearings mounted on hydrogen utilization equipment used in hydrogen environments such as fuel cell vehicles (FCVs) and hydrogen refueling stations, miniaturization of the bearings can be achieved by increasing the static load capacity, which may improve the efficiency of the hydrogen utilization equipment. However, the static load capacity of the bearing component surface described in Patent Document 1 still has room for improvement.

[0010] The present invention has been made in view of the above-mentioned problems of the prior art. More specifically, the present invention provides a mechanical component having an improved static load capacity on the surface.

[0011] Technical solutions adopted to solve technical problems

[0012] The mechanical part of the present invention has a surface and is made of steel that has been quenched and tempered. The mechanical part has a nitriding layer formed on the surface. The steel contains carbon of 0.95 mass % to 1.10 mass %, silicon of less than 0.30 mass %, manganese of less than 0.50 mass %, sulfur of less than 0.0080 mass %, and chromium of 1.3 mass % to 1.6 mass %, and the remainder is composed of iron and unavoidable impurities. The average nitrogen concentration on the surface is above 0.10 mass %. The hardness of the surface is above 850 Hv. The amount of retained austenite on the surface is below 20 volume %.

[0013] In the above-mentioned mechanical part, the half-value width of the X-ray profile of martensite obtained by X-ray diffraction of the surface can be 7.2° or more and 8.0° or less. The peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface can be 128° or more.

[0014] In the above mechanical parts, the dislocation density of the surface martensite can be 1.1×10 15 m -2 The dislocation density of the surface austenite can be above 2.5×10 14 m -2 above.

[0015] In the above-mentioned mechanical parts, the amount of retained austenite on the surface, the average nitrogen concentration on the surface, and the dislocation density of austenite on the surface are recorded as A (unit: volume %), B (unit: mass %), and C (unit: m -2 ), the relationship 4.332+0.005×A-0.580×B-0.295×LogC≤0 can be satisfied.

[0016] In the above-mentioned mechanical parts, the amount of retained austenite on the surface, the average nitrogen concentration on the surface, and the dislocation density of martensite on the surface are recorded as A (unit: volume %), B (unit: mass %), and D (unit: m -2 ), the relationship -47.73-0.025×A-2.141×B+3.155×LogD≥0 can be satisfied.

[0017] In the above-mentioned mechanical component, the depth of the indentation formed on the surface when a maximum contact surface pressure of 4.5 GPa is applied to the surface can be less than 0.2 μm. In the above-mentioned mechanical component, the static load capacity of the surface can be greater than 6.0 GPa.

[0018] Effects of the Invention

[0019] The static load capacity of a surface can be improved by means of the mechanical component of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a cross-sectional view of the inner ring 10 .

[0021] Figure 2 It is a process diagram showing a method for manufacturing the inner ring 10 .

[0022] Figure 3 This is a graph showing the relationship between the maximum contact surface pressure of the surfaces of Samples 1 to 6 and the value obtained by dividing the indentation depth by the ceramic ball diameter.

[0023] Figure 4 It is a cross-sectional view of the ball screw 20 .

[0024] Figure 5 is a cross-sectional view of the rolling bearing 100 . DETAILED DESCRIPTION

[0025] The embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the following drawings, the same or corresponding parts are marked with the same reference symbols, and repeated descriptions are not repeated.

[0026] The mechanical part of the embodiment is, for example, a raceway ring of a rolling bearing. The mechanical part of the embodiment may be a rolling element, a shaft, a sliding member such as a ball screw of a rolling bearing. The mechanical part of the embodiment is not limited thereto, but the inner ring 10 of a deep groove ball bearing is used as an example of the mechanical part of the embodiment for explanation below.

[0027] (Configuration of the inner ring 10)

[0028] Next, the structure of the inner ring 10 will be described.

[0029] Figure 1 is a cross-sectional view of the inner ring 10. Figure 1 As shown, the inner ring 10 has a surface. More specifically, the inner ring 10 has a width surface 10a, a width surface 10b, an inner peripheral surface 10c, and an outer peripheral surface 10d as surfaces. The central axis of the inner ring 10 is the central axis A. The direction along the central axis A is the axial direction. The direction perpendicular to the axial direction and passing through the central axis A is the radial direction. The direction along the circumference centered on the central axis A is the circumferential direction.

[0030] The width surface 10a and the width surface 10b constitute the end surface of the inner ring 10 in the axial direction. The width surface 10b is the opposite surface of the width surface 10a. The inner peripheral surface 10c extends along the circumferential direction. The inner peripheral surface 10c faces the center axis A. One end and the other end of the inner peripheral surface 10c in the axial direction are connected to the width surface 10a and the width surface 10b respectively. The inner ring 10 is embedded in the shaft (not shown) at the inner peripheral surface 10c.

[0031] The outer peripheral surface 10d extends in the circumferential direction. The outer peripheral surface 10d faces the side opposite to the central axis A. That is, the outer peripheral surface 10d is the surface opposite to the inner peripheral surface 10c in the radial direction. One end and the other end of the outer peripheral surface 10d in the axial direction are connected to the width surface 10a and the width surface 10b, respectively.

[0032] The outer peripheral surface 10d has a track surface 10da. The track surface 10da is the portion of the outer peripheral surface 10d that contacts the rolling element. The track surface 10da is located at the center of the outer peripheral surface 10d in the axial direction. The track surface 10da extends along the circumferential direction. The outer peripheral surface 10d is recessed toward the inner peripheral surface 10c at the track surface 10da. In a cross-sectional view orthogonal to the circumferential direction, the track surface 10da is, for example, in the shape of a partial arc.

[0033] The inner ring 10 is made of steel that has been quenched and tempered. That is, the steel constituting the inner ring 10 contains martensite and retained austenite. The surfaces (width surface 10a, width surface 10b, inner peripheral surface 10c, and outer peripheral surface 10d) of the inner ring 10 are nitrided. That is, a nitrided layer 11 is formed on the surface of the inner ring 10. In addition, nitrogen is dissolved in the steel at the nitrided layer 11, rather than forming nitrides in the nitrided layer 11.

[0034] The steel constituting the inner ring 10 contains 0.95 mass % to 1.10 mass % carbon, less than 0.30 mass % silicon, less than 0.50 mass % manganese, less than 0.0080 mass % sulfur, and 1.3 mass % to 1.6 mass % chromium. The remainder of the steel constituting the inner ring 10 is composed of iron and unavoidable impurities. In addition, the steel constituting the inner ring 10 may not contain silicon, manganese and sulfur.

[0035] Bearing steel is a specific example of the steel constituting the inner ring 10. Specific examples of bearing steel include SUJ2 specified in the JIS standard, 52100 specified in the ASTM standard, 100Cr6 specified in the ISO standard, and GCr15 specified in the GB standard.

[0036] The average nitrogen concentration on the surface of the inner ring 10 is 0.10 mass % or more. The average nitrogen concentration on the surface of the inner ring 10 can be measured, for example, by using EPMA (Electron Probe Micro Analyzer) radiation analysis. In addition, at this time, a calibration curve is prepared using a sample with a clear nitrogen concentration.

[0037] The amount of retained austenite on the surface of the inner ring 10 is less than 20 volume %. The amount of retained austenite on the surface of the inner ring 10 is measured by X-ray diffraction. This measurement is performed using a Cr tube ball type X-ray diffraction device. In the Cr tube ball type X-ray diffraction device, the wavelength of the Cr-Kα ray is 2.29093×10 -10m, the tube voltage is 30 kV, the tube current is 10 mA, and the collimator size is 2 mm × 2 mm.

[0038] The hardness of the inner ring 10 surface is 850 Hv or more. The hardness of the inner ring 10 surface is measured according to the Vickers hardness test method specified in the JIS standard. The load when measuring the hardness of the inner ring 10 surface is 300 g. The hardness of the inner ring 10 surface is measured at three or more different points, and the average value of these measured values ​​is adopted.

[0039] The half width of the X-ray profile of martensite obtained by X-ray diffraction of the surface of the inner ring 10 is preferably 7.2° or more and 8.0° or less. The peak position (2θ) of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10 is preferably 128° or more. The interplanar spacing of austenite on the surface of the inner ring 10 is preferably 1.275×10 -10 m or less.

[0040] The X-ray profile of martensite and the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10 are obtained by using a Cr tube ball type X-ray diffraction device. In the Cr tube ball type X-ray diffraction device, the wavelength of Cr-Kα rays is 2.29093×10 -10 m, tube voltage is 30 kV, tube current is 10 mA, and collimator size is 2 mm × 2 mm. The X-ray profile of martensite obtained by X-ray diffraction on the surface of the inner ring 10 is measured within the range of 2θ of 142.75° to 170.8°, and the X-ray profile of austenite obtained by X-ray diffraction on the surface of the inner ring 10 is measured within the range of 2θ of 114.75° to 142.8°.

[0041] The X-ray profile of martensite and the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10 are background processed. The peak position showing the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10 is obtained from the center position of the half-value width.

[0042] The interplanar spacing of austenite on the surface of the inner ring 10 is calculated by applying the following Bragg formula to the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10. In this formula, d is the interplanar spacing of austenite on the surface of the inner ring 10 (unit: m), λ is the wavelength of Cr-Kα rays used in the Cr tube ball type X-ray diffraction device (unit: m), and θ is the diffraction angle of the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10 (unit: °).

[0043] [Mathematical formula 1]

[0044] Mathematical formula 1

[0045]

[0046] The dislocation density of the martensite on the surface of the inner ring 10 is preferably 1.1×10 15 m -2 The dislocation density of austenite on the surface of the inner ring 10 is preferably 2.5×10 14 m -2 above.

[0047] The dislocation density of martensite and austenite on the surface of the inner ring 10 was measured using a Co tube-ball X-ray diffractometer. More specifically, first, the X-ray profiles of martensite and austenite on the surface of the inner ring 10 were obtained using a Co tube-ball X-ray diffractometer. In the Co tube-ball X-ray diffractometer, the wavelength of Co-Kα rays is 1.7889×10 -10 m, tube voltage 40 kV, tube current 50 mA, collimator size 1 mm in diameter. The X-ray profiles of martensite and austenite obtained by X-ray diffraction of the surface of the inner ring 10 were measured within the range of 2θ of 30° to 135°.

[0048] Second, based on the Rietveld analysis, the half-value width of the peak of the X-ray profile of martensite and austenite obtained by X-ray diffraction of the surface of the inner ring 10 is separated into the crystallite size and strain. Third, by applying the crystallite size and strain to the following Williamson-Hall formula, the dislocation density of martensite and the dislocation density of austenite on the surface of the inner ring 10 are obtained. In this formula, ρ is the dislocation density (unit: m -2 ), ε is the above strain, b is the length of the Burgers vector (b = 0.25 × 10 -9 m).

[0049] [Mathematical formula 2]

[0050] Mathematical formula 2

[0051]

[0052] In the X-ray profile of martensite obtained by X-ray diffraction of the surface of the inner ring 10, the peaks of the {110} plane, {200} plane, {211} plane, and {220} plane are measured. In the X-ray profile of austenite obtained by X-ray diffraction of the surface of the inner ring 10, the peaks of the {111} plane, {200} plane, {220} plane, {311} plane, and {222} plane are measured. The reason for performing the Rietveld analysis is to reduce the influence of the {200} plane of martensite and the {200} plane of austenite, which have different elastic moduli.

[0053] The depth of the indentation formed when a maximum contact surface pressure of 4.5 GPa is applied to the surface of the inner ring 10 (track surface 10da) is preferably less than 0.2 μm. The indentation depth is measured by using the white light interferometry function of a laser microscope after the ceramic ball is brought into contact with the surface of the inner ring 10 at a maximum contact surface pressure of 4.5 GPa using an Autograph. In addition, the load loading speed at this time is 3 N / sec, and the load is maintained for 120 seconds after reaching the load.

[0054] The static load capacity of the inner ring 10 surface is preferably 6.0 GPa or more. In the measurement of the static load capacity of the inner ring 10 surface, first, the maximum contact surface pressure is changed by using Autograph in the same manner as described above to form an indentation on the surface of the inner ring 10. Second, each time the maximum contact surface pressure is changed, the value obtained by dividing the indentation depth by the ceramic ball diameter is calculated. The maximum contact surface pressure when the value obtained by dividing the indentation depth by the ceramic ball diameter reaches 1 / 10000 is the static load capacity of the inner ring 10 surface.

[0055] The amount of retained austenite on the surface of the inner ring 10, the average nitrogen concentration on the surface of the inner ring 10, and the dislocation density of austenite on the surface of the inner ring 10 are respectively denoted as A (unit: volume %), B (unit: mass %), C (unit: m -2 The inner ring 10 preferably satisfies the relationship 4.332+0.005×A-0.580×B-0.295×LogC≤0.

[0056] The dislocation density of the martensite on the surface of the inner ring 10 is denoted as D (unit: m -2 ). The surface of the inner ring 10 preferably satisfies the relationship -47.73-0.025×A-2.141×B+3.155×LogD≥0.

[0057] (Method of Manufacturing Inner Ring 10)

[0058] Next, a method for manufacturing the inner ring 10 will be described.

[0059] Figure 2 1 is a process diagram showing a method for manufacturing the inner ring 10. Figure 2 As shown, the method for manufacturing the inner ring 10 includes a preparation step S1 , a nitriding treatment step S2 , a quenching step S3 , a cryogenic treatment step S4 , a tempering step S5 , and a post-treatment step S6 .

[0060] The processing object member is prepared in the preparation step S1. The nitriding treatment step S2 is performed after the preparation step S1. The nitriding treatment step S2 is performed by maintaining the processing object member at a temperature above the A1 transformation point in an atmosphere gas containing a nitrogen source. The nitriding treatment step S2 is performed to allow nitrogen to penetrate and diffuse to the position that becomes the surface of the inner ring 10 after the post-treatment step S6. The quenching step S3 is performed after the nitriding treatment step S2. In the quenching step S3, the processing object member is maintained at a temperature above the A1 transformation point and then cooled to M S Temperature below the phase transition point.

[0061] The cryogenic treatment step S4 is performed after the quenching step S3. In the cryogenic treatment step S4, the processing object member is cooled to a temperature higher than -100°C and below room temperature. Thereby, a part of the retained austenite formed in the steel constituting the processing object member in the quenching step S3 is transformed into martensite. Instead of the cryogenic treatment step S4, a deep cryogenic treatment step S7 may be performed. In the deep cryogenic treatment step S7, the processing object member is cooled to a temperature lower than -100°C. Thereby, a part of the retained austenite formed in the steel constituting the processing object member in the quenching step S3 is transformed into martensite.

[0062] As the refrigerant in the cryogenic treatment step S4 and the cryogenic treatment step S7, for example, liquid nitrogen, liquid helium, etc. are used. The cryogenic treatment step S4 and the cryogenic treatment step S7 are preferably performed within 2 hours after the quenching step S3 is completed.

[0063] The tempering step S5 is performed after the cryogenic treatment step S4 (the cryogenic treatment step S7). In the tempering step S5, the workpiece is kept at a temperature lower than the A1 transformation point. Thereby, a part of the martensite in the steel constituting the workpiece is decomposed. The holding temperature in the tempering step S5 is, for example, 180°C to 220°C. The holding time in the tempering step S5 is, for example, 2 hours.

[0064] The post-processing step S6 is performed after the tempering step S5. In the post-processing step S6, the surface of the workpiece is machined (for example, ground and polished). Figure 1 The inner ring 10 of the structure shown.

[0065] (Effect of inner circle 10)

[0066] The effects of the inner ring 10 will be described below.

[0067] As described in Patent Document 1, in order to improve the static load capacity of the raceway ring surface, it is considered that tempering should be performed at a high temperature (e.g., above 230°C). However, in this case, the martensite formed by quenching is sometimes excessively decomposed by tempering, thereby reducing the hardness of the raceway ring surface and causing the static load capacity of the raceway ring surface to be insufficient.

[0068] On the other hand, in the inner ring 10, nitrogen is dissolved in the nitrided layer 11, thereby solid solution strengthening the surface of the inner ring 10. In addition, in the inner ring 10, by performing the low temperature treatment step S4 (deep cryogenic treatment step S7), the amount of retained austenite on the surface is reduced (martensite is increased), and the dislocation density of the retained austenite and martensite on the surface is increased. As a result, in the inner ring 10, the surface hardness reaches 850 Hv or more. Therefore, the static load capacity of the surface of the inner ring 10 is improved compared with the case of tempering at high temperature.

[0069] More specifically, because the amount of retained austenite on the surface of the inner ring 10 is less than 20 volume %, the average nitrogen concentration on the surface of the inner ring 10 is greater than 0.10 mass %, and the hardness of the surface of the inner ring 10 is greater than 850 Hv, the indentation depth when a maximum contact surface pressure of 4.5 GPa is applied to the surface of the inner ring 10 is less than 0.2 μm, and the static load capacity of the surface of the inner ring 10 is greater than 6.0 GPa.

[0070] In addition, nitrogen is an austenite stabilizing element, and the nitriding treatment is performed to enrich the retained austenite on the surface of the raceway ring. Therefore, when the nitriding treatment is performed, low temperature treatment (or deep cryogenic treatment) is usually not performed to reduce the amount of retained austenite on the surface.

[0071] (Evaluation of static load capacity and indentation depth)

[0072] In order to evaluate the static load capacity of the surface of the mechanical component of the embodiment, samples 1 to 6 were prepared. The shape of samples 1 to 6 was a flat plate with a diameter of 85 mm and a thickness of 5 mm. Samples 1 to 6 were formed of SUJ2 specified in the JIS standard. Table 1 shows the details of the heat treatment performed on samples 1 to 6.

[0073] [Table 1]

[0074] Table 1

[0075]

[0076] For sample 1, nitriding step S2, quenching step S3, cryogenic treatment step S7 and tempering step S5 were performed as heat treatment. For samples 2 and 3, nitriding step S2, quenching step S3, cryogenic treatment step S4 and tempering step S5 were performed as heat treatment. That is, samples 1 to 3 are samples simulating the mechanical parts of the embodiment. In the tempering step S5 performed on samples 1 to 3, the temperature was kept at 180°C.

[0077] Sample 4 was subjected to nitriding step S2, quenching step S3 and tempering step S5 as heat treatment, and low temperature treatment step S4 (or cryogenic treatment step S7) was not performed. In the tempering step S5 performed on Sample 4, tempering was performed at high temperature (specifically, at 230°C).

[0078] Sample 5 was subjected to nitriding step S2, quenching step S3, and tempering step S5 as heat treatment, and the cryogenic treatment step S4 (or deep cryogenic treatment step S7) was not performed. In the tempering step S5 performed on Sample 5, the temperature was maintained at 180°C. Sample 6 was subjected to quenching step S3 and tempering step S5 as heat treatment, and the nitriding step S2 and cryogenic treatment step S4 (or deep cryogenic treatment step S7) were not performed. In the tempering step S5 performed on Sample 5, the temperature was maintained at 180°C.

[0079] For Samples 1 to 6, the average nitrogen concentration on the surface, the hardness on the surface, the amount of retained austenite on the surface, the indentation depth when a maximum contact surface pressure of 4.5 GPa was applied to the surface, and the static load capacity on the surface were measured.

[0080] Table 2 shows the measurement results of the average nitrogen concentration on the surface, the hardness on the surface, the amount of retained austenite on the surface, the indentation depth when a maximum contact surface pressure of 4.5 GPa was applied to the surface, and the static load capacity on the surface. Figure 3 This is a graph showing the relationship between the maximum contact surface pressure on the surfaces of Samples 1 to 6 and the value obtained by dividing the indentation depth by the ceramic ball diameter. The ceramic ball diameter is 3 / 8 inch (9.525 mm).

[0081] [Table 2]

[0082] Table 2

[0083]

[0084] The average nitrogen concentration on the surface being 0.10 mass % or more, the hardness on the surface being 850 Hv or more, and the amount of retained austenite on the surface being 20 volume % or less are respectively recorded as Condition 1, Condition 2, and Condition 3. As shown in Table 2, Samples 1 to 3 satisfy all of Conditions 1, 2, and 3. On the other hand, Samples 4 to 6 do not satisfy at least any one of Conditions 1, 2, and 3.

[0085] As shown in Table 1 and Figure 3 As shown, in samples 1 to 3, the indentation depth when the maximum contact surface pressure of 4.5 GPa was applied to the surface reached less than 0.2 μm, and the static load capacity of the surface reached more than 6.0 GPa. On the other hand, in samples 4 to 6, the indentation depth when the maximum contact surface pressure of 4.5 GPa was applied to the surface exceeded 0.2 μm, and the static load capacity of the surface was less than 6.0 GPa. From this comparison, it can be experimentally known that the static load capacity of the surface can be improved by satisfying conditions 1, 2, and 3.

[0086] Samples 1-1 to 1-3, Samples 2-1 to 2-3, and Samples 3-1 to 3-3 are samples subjected to the same heat treatment as Samples 1, 2, and 3. Samples 4-1 to 4-4 are samples subjected to the same heat treatment as Sample 4. The steel type and shape of these samples are SUJ2 and a flat plate with a diameter of 85 mm and a thickness of 5 mm.

[0087] [Table 3]

[0088] Table 3

[0089]

[0090] As shown in Table 3, samples 1-1 to 1-3, samples 2-1 to 2-3, and samples 3-1 to 3-3 satisfy all of conditions 1, 2, and 3. On the other hand, samples 4-1 to 4-4 do not satisfy at least one of conditions 1, 2, and 3.

[0091] In samples 1-1 to 1-3, samples 2-1 to 2-3, and samples 3-1 to 3-3, the half-value width of the X-ray profile of martensite obtained by X-ray diffraction of the surface is greater than 7.2° and less than 8.0°, and the peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface is greater than 128°.

[0092] On the other hand, in Samples 4-1 to 4-4, the half-value width of the X-ray profile of martensite obtained by surface X-ray diffraction is less than 7.2°, and the peak position of the {220} plane in the X-ray profile of austenite obtained by surface X-ray diffraction is less than 128°.

[0093] From this comparison, it can be seen that when conditions 1, 2 and 3 are met, the half-value width of the X-ray profile of martensite obtained by X-ray diffraction of the surface is greater than 7.2° and less than 8.0°, and the peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface is greater than 128°.

[0094] If this point is described from another perspective, it is obvious that by not performing the tempering step S5 at a high temperature and performing the low temperature treatment step S4 or the deep cryogenic treatment step S7, the dislocation density of the surface martensite is increased, the half-value width of the X-ray profile is increased, and the dislocation density of the surface austenite is increased, indicating that the peak position of the {220} plane is shifted to the high angle side.

[0095] As shown in Table 4, in Samples 1, 2, and 3, the half-value width of the X-ray profile of martensite obtained by X-ray diffraction of the surface was 7.2° or more and 8.0° or less, and the peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface was 128° or more. In addition, in Samples 1, 2, and 3, the dislocation density of the surface martensite and the dislocation density of the austenite were 1×10 15 m -2 Above and 2.5×10 14 m -2 above.

[0096] On the other hand, in Sample 4, the half width of the X-ray profile of martensite obtained by X-ray diffraction of the surface was less than 7.2°, and the peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface was less than 128°. In addition, in Sample 4, the dislocation density of the surface martensite and the dislocation density of the austenite were less than 1×10 15 m -2 and less than 2.5×10 14 m -2 .

[0097] [Table 4]

[0098] Table 4

[0099]

[0100] The indentation depth when the maximum contact surface pressure of 4.5 GPa was applied to the surface was compared with the amount of retained austenite on the surface (A: in volume %), the average nitrogen concentration on the surface (B: in mass %), and the dislocation density of austenite on the surface (C: in m -2) were subjected to a multiple regression analysis. As a result of the multiple regression analysis, the indentation depth (unit: μm) when the maximum contact surface pressure of 4.5 GPa is applied to the surface can be estimated by the formula 4.532+0.005×A-0.580×B-0.295×LogC≤0. The coefficient of determination (R 2 ) is 0.94. Therefore, when the relationship of 4.332+0.005×A-0.580×B-0.295×LogC≤0 is satisfied, the indentation depth when a maximum contact surface pressure of 4.5 GPa is applied to the surface can be reduced to 0.2 μm or less.

[0101] The static load capacity on the surface is related to the amount of retained austenite on the surface (A: in volume %), the average nitrogen concentration on the surface (B: in mass %), and the dislocation density of martensite on the surface (D: in m -2 ) were subjected to multiple regression analysis. As a result of the multiple regression analysis, the static load capacity (unit: GPa) of the surface can be estimated by the formula -41.73-0.025×A-2.141×B+3.155×LogD≥0. The coefficient of determination (R 2 ) is 0.94. Therefore, when the relationship -47.73-0.025×A-2.141×B+3.155×LogD≥0 is satisfied, the static load capacity of the surface can be made to be 6.0 GPa or more.

[0102] (Another Example of Mechanical Components of Embodiment)

[0103] Hereinafter, examples of mechanical components according to the embodiment other than the inner ring 10 will be described.

[0104] Figure 4 20 is a cross-sectional view of the ball screw 20. Figure 4 As shown, the ball screw 20 has a screw shaft 21, a ball nut 22, a plurality of balls 23, and a sealing member 24. The circulation method of the balls 23 in the ball screw 20 is not particularly limited. The circulation method of the balls 23 in the ball screw 20 is, for example, a tube type, a return tube (insertion tube) type, a deflector type, an end deflector type, an end cover type, a gyro type, etc.

[0105] The screw shaft 21 has an outer peripheral surface 21a. A screw groove 21b is formed on the outer peripheral surface 21a. A hole extending along the central axis direction of the screw shaft 21 is formed on the ball nut 22. The inner wall surface of the hole is the inner peripheral surface 22a of the ball nut 22. A screw groove 22b is formed on the inner peripheral surface 22a. The screw shaft 21 is inserted into the ball nut 22 in a manner that the outer peripheral surface 21a and the inner peripheral surface 22a face each other. The ball 23 is arranged between the screw groove 21b and the screw groove 22b. The hole of the ball nut 22 through which the screw shaft 21 passes is sealed by a sealing member 24. The screw shaft 21 also passes through the hole formed in the sealing member 24.

[0106] The screw shaft 21, the ball nut 22 and the ball 23 are formed by quenched and tempered steel. The steel contains carbon of 0.95 mass % to 1.10 mass %, silicon of less than 0.30 mass %, manganese of less than 0.50 mass %, sulfur of less than 0.0080 mass %, and chromium of 1.3 mass % to 1.6 mass %. The remaining part of the steel is composed of iron and inevitable impurities. The steel is, for example, bearing steel (SUJ2 specified in the JIS standard, 52100 specified in the ASTM standard, 100Cr6 specified in the ISO standard, and GCr15 specified in the GB standard, etc.).

[0107] The surfaces of the screw shaft 21, the ball nut 22 and the ball 23 are formed with a nitriding layer 11 ( Figure 4 The average nitrogen concentration on the surface is above 0.10 mass %. The hardness of the surface of the screw shaft 21, the ball nut 22 and the ball 23 is above 850 Hv. The amount of retained austenite on the surface of the screw shaft 21, the ball nut 22 and the ball 23 is below 20 volume %. That is, the screw shaft 21, the ball nut 22 and the ball 23 are mechanical parts of the embodiment.

[0108] In the ball screw 20, the static load capacity of the screw shaft 21, the ball nut 22 and the surface of the ball 23 is improved, so that a high load capacity can be achieved, and a small size and light weight can also be achieved. By miniaturizing the ball screw 20, the miniaturization of peripheral parts and structural members can also be achieved.

[0109] Among them, it is sufficient that at least one of the screw shaft 21, the ball nut 22 and the ball 23 satisfies the above-mentioned steel composition, the above-mentioned surface hardness, the above-mentioned surface nitrogen concentration and the above-mentioned surface retained austenite amount. If this point is described from another perspective, in the ball screw 20, it is sufficient that at least one of the screw shaft 21, the ball nut 22 and the ball 23 is a mechanical component of the embodiment.

[0110] By rotating the screw shaft 21 around its central axis, the rotational power of the screw shaft 21 can be transmitted to the ball nut 22 through the ball 23, and the ball nut 22 moves along the central axis direction of the screw shaft 21. That is, the ball screw 20 is a device that converts the rotational motion of a motor or the like into a linear motion. The ball screw 20 is used, for example, in electric actuators, positioning devices, electric jacks, servo cylinders, electric servo presses, mechanical presses, electric brake devices, transmission systems, electric power steering devices, electric injection molding machines, and the like.

[0111] (Rolling bearing 100 using inner ring 10)

[0112] Figure 5 is a cross-sectional view of the rolling bearing 100. Figure 5 As shown, the rolling bearing 100 has an inner ring 10 , an outer ring 30 , a plurality of rolling elements 40 , and a cage 50 .

[0113] The outer ring 30 has a width surface 30a, a width surface 30b, an inner peripheral surface 30c and an outer peripheral surface 30d. The width surface 30a and the width surface 30b constitute the end surface of the inner ring 30 in the axial direction. The width surface 30b is the opposite surface of the width surface 30a. The inner peripheral surface 30c and the outer peripheral surface 30d extend in the circumferential direction. The inner peripheral surface 30c and the outer peripheral surface 30d face the central axis A side and the opposite side of the central axis A, respectively. The outer ring 30 is fitted with the housing (not shown) at the outer peripheral surface 30d. The outer ring 30 is arranged on the radially outer side of the inner ring 10 so that the inner peripheral surface 30c and the outer peripheral surface 10d face each other.

[0114] The inner circumferential surface 30c has a track surface 30ca. The track surface 30ca is the portion of the inner circumferential surface 30c that contacts the rolling element 40. The track surface 30ca is located at the center of the inner circumferential surface 30c in the axial direction. The track surface 30ca extends along the circumferential direction. The inner circumferential surface 30c is recessed toward the outer circumferential surface 30d at the track surface 30ca. In a cross-sectional view orthogonal to the circumferential direction, the track surface 30ca is, for example, partially arc-shaped. The track surface 30ca faces the track surface 10da.

[0115] The rolling element 40 is, for example, spherical. The rolling element 40 is disposed between the track surface 10da and the track surface 30ca. The plurality of rolling elements 40 are arranged at intervals in the circumferential direction. The retainer 50 retains the plurality of rolling elements 40 in such a manner that the interval between two adjacent rolling elements 40 is within a certain range. The retainer 50 is disposed between the outer peripheral surface 10d and the inner peripheral surface 30c.

[0116] The outer ring 30 and the rolling element 40 are, for example, mechanical parts of the embodiment. That is, the outer ring 30 and the rolling element 40 are formed of steel that has been quenched and tempered, and the steel contains 0.95 mass% to 1.10 mass% carbon, less than 0.30 mass% silicon, less than 0.50 mass% manganese, less than 0.0080 mass% sulfur, and 1.3 mass% to 1.6 mass% chromium, and the remainder is composed of iron and inevitable impurities. In addition, the average nitrogen concentration, hardness, and retained austenite amount on the surface of the outer ring 30 and the rolling element 40 are respectively 0.10 mass% or more, 850 Hv or more, and 20 volume% or less. However, the outer ring 30 and the rolling element 40 may also be mechanical parts of the embodiment.

[0117] The embodiments disclosed this time should be considered in all aspects as illustrative and non-restrictive. The scope of the present invention is indicated by the claims rather than the above embodiments, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0118] Explanation of symbols

[0119] 10 inner ring, 10a and 10b width surfaces, 10c inner circumferential surface, 10d outer circumferential surface, 10da raceway surface, 11 nitriding layer, 20 ball screw, 21 screw shaft, 21a outer circumferential surface, 21b screw groove, 22 ball nut, 22a inner circumferential surface, 22b screw groove, 23 ball, 24 sealing member, 30 outer ring, 30a and 30b width surfaces, 30c inner circumferential surface, 30ca raceway surface, 30d outer circumferential surface, 40 rolling element, 50 retainer, A center axis, S1 preparation step, S2 nitriding treatment step, S3 quenching step, S4 cryogenic treatment step, S5 tempering step, S6 post-treatment step, S7 cryogenic treatment step.

Claims

1. A mechanical component having a surface and made of quenched and tempered steel, wherein: having a nitrided layer formed on the surface, The steel contains 0.95 mass % to 1.10 mass % of carbon, less than 0.30 mass % of silicon, less than 0.50 mass % of manganese, less than 0.0080 mass % of sulfur, and 1.3 mass % to 1.6 mass % of chromium, with the remainder being iron and unavoidable impurities, The average nitrogen concentration of the surface is 0.10 mass % or more, The hardness of the surface is above 850Hv, The amount of retained austenite on the surface is less than 20 volume %.

2. The mechanical component according to claim 1, wherein: The half width of an X-ray profile of martensite obtained by X-ray diffraction of the surface is 7.2° or more and 8.0° or less, and the peak position of the {220} plane in the X-ray profile of austenite obtained by X-ray diffraction of the surface is 128° or more.

3. The mechanical component according to claim 1, wherein: The dislocation density of the surface martensite is 1.1×10 15 m -2 The above-mentioned dislocation density of the austenite on the surface is 2.5×10 14 m -2 above.

4. The mechanical component according to claim 1, wherein: The amount of retained austenite on the surface, the average nitrogen concentration on the surface, and the dislocation density of austenite on the surface are denoted as A (unit: volume %), B (unit: mass %), and C (unit: m -2 ), the relationship 4.332+0.005×A-0.580×B-0.295×LogC≤0 is satisfied.

5. The mechanical component according to claim 1, wherein: The amount of retained austenite on the surface, the average nitrogen concentration on the surface, and the dislocation density of martensite on the surface are denoted as A (unit: volume %), B (unit: mass %), and D (unit: m -2 ), the relationship -47.73-0.025×A-2.141×B+3.155×LogD≥0 is satisfied.

6. The mechanical component according to claim 1, wherein: When a maximum contact surface pressure of 4.5 GPa is applied to the surface, a depth of an indentation formed on the surface is less than 0.2 μm.

7. The mechanical component according to claim 1, wherein: The static load capacity of the surface is above 6.0 GPa.