Particle inorganic material equipped with elemental silver and elemental ruthenium
By using particulate inorganic materials of elemental silver and ruthenium in antimicrobial materials, the efficient antimicrobial carrier material is formed through reduction and pyrolysis treatment, which solves the problem of limited effects of existing materials and achieves effective inhibition and widespread microorganisms Applicability of application scenarios.
Patent Information
- Application Number
- CN202380028251.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-02-03
- Publication Date
- 2024-11-08
AI Technical Summary
Existing antimicrobial materials have limited effects when treating microorganisms, especially in application scenarios where efficient antimicrobials are required, which are difficult to meet the requirements.
A particulate inorganic material composed of elemental silver and elemental ruthenium is used to form a particulate support material by reducing silver and ruthenium precursors, and combined with specific inorganic material composition and treatment methods, a product with high antimicrobial activity is prepared. The method includes using sodium borohydride, hydrazine, hypophosphite and formate as reducing agents in an alkaline environment, controlling the temperature and pH values, ensuring complete reduction of silver and ruthenium, and forming efficiently through drying and pyrolysis treatment. Particulate material.
Achieve efficient antimicrobial effects, significantly improve the material's ability to inhibit microorganisms, and is suitable for a variety of scenarios such as metal surfaces, coatings, plastics, etc., and the antimicrobial activity of the material shows significant inhibition in conventional inhibition zone tests. Effect.
Abstract
Description
[0001] The present invention relates to a particulate inorganic material provided with elemental noble metals in the form of elemental silver and elemental ruthenium and to two efficient processes for preparing the same.
[0002] WO 2021 / 084140 A2 discloses a method for preparing a particulate support material equipped with elemental silver and elemental ruthenium, which can be used as an additive for the antimicrobial treatment of a wide variety of materials and substances.
[0003] The object of the present invention is to provide highly antimicrobially active materials based on support materials provided with elemental silver and elemental ruthenium.
[0004] This object can be achieved by providing a product in the form of a particulate inorganic material provided with elemental silver and elemental ruthenium, said inorganic material having an average particle size (d50) in the range of 50 nm to 40 μm and an average particle size (d50) in the range of 1 nm to 40 μm. 2 / g to 1600m 2 / g, wherein the inorganic material (the inorganic material itself) is selected from the group consisting of: aluminum nitride, titanium nitride, silicon nitride, corundum (alpha-aluminum oxide), titanium dioxide in the form of anatase, titanium dioxide in the form of rutile, pyrogenic silica (pyrogenic silicon dioxide), precipitated silica (precipitated silicon dioxide), sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-aluminum oxide hydroxide. The product according to the invention is also referred to below as "particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention". Its silver plus ruthenium weight ratio formed by elemental silver and elemental ruthenium can be, for example, in the range of 0.1% to 50% by weight (weight percentage), preferably 1% to 40% by weight, while the dominant silver:ruthenium weight ratio is, for example, in the range of 1 part by weight to 2000 parts by weight of silver: 1 part by weight of ruthenium.
[0005] The particulate inorganic material or particles of inorganic material are a support material for elemental silver and elemental ruthenium, i.e. in the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention, the particulate inorganic material serves as a support for elemental silver and elemental ruthenium. Typically and preferably, only one type of support material is present in the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention.
[0006] The particulate inorganic material provided with elemental silver and elemental ruthenium according to the invention comprises inorganic material particles provided with elemental silver and elemental ruthenium in a proportion, for example, in the range of 95% by weight to 100% by weight, in particular 100% by weight. A possible proportion of no more than 5% by weight can be formed by corresponding inorganic particles without precious metals. In other words, the particulate inorganic material provided with elemental silver and elemental ruthenium according to the invention can consist of 95% by weight to 100% by weight of inorganic material particles provided with elemental silver and elemental ruthenium and 0% by weight to 5% by weight of corresponding inorganic particles without precious metals, wherein the weight percentages add up to 100% by weight.
[0007] The term "average particle size" as used herein refers to the volume-average primary particle diameter (d50) that can be measured by laser diffraction. In this case, what is called the equivalent circular area diameter (ECAD) can be advantageously used as a measure of particle diameter (see RENLIANG XU et al.: "Comparison of sizing small particles using different technologies to small particles using different technologies", "Powder Technology", Elsevier, Basel (Switzerland), Vol. 132, No. 2-3, June 24, 2003 (06-24-2003), pp. 145-153). Laser diffraction measurement can be performed using a corresponding particle size measuring instrument, such as Mastersizer 3000 or Mastersizer 2000 from Malvern Instruments according to a wet determination method. In the wet determination method, as a part of sample preparation, the particle sample can be dispersed in ethanol by ultrasound.
[0008] The term “BET surface” as used herein refers to the specific surface area which can be determined by means of a BET measurement in accordance with DIN ISO 9277:2014-01 (according to Chapter 6.3.1, static volume measurement procedure, gas used: nitrogen).
[0009] The invention also relates to two methods for preparing such particulate inorganic materials provided with elemental silver and elemental ruthenium according to the invention. From another perspective, both methods can also be understood as methods for providing the corresponding particulate inorganic materials with elemental silver and elemental ruthenium.
[0010] In a first method according to the invention, the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention can be obtained by reducing at least one silver precursor and at least one ruthenium precursor in the presence of water-suspended particles of the corresponding inorganic material, then separating the solid formed in the process from the aqueous phase, optionally washing the separated solid with water and optionally drying the solid. The first method according to the invention thus comprises the steps of reducing at least one silver precursor and at least one ruthenium precursor in the presence of water-suspended particles of the corresponding inorganic material; separating the solid formed in the course of the reduction from the aqueous phase; optionally washing the separated solid with water; and optionally drying the separated and optionally washed solid. During the reduction, the silver and ruthenium precursors can be reduced successively or preferably simultaneously.
[0011] The silver precursor and ruthenium precursor used in the first method according to the invention are silver and ruthenium compounds. Elemental silver or elemental ruthenium can be generated from silver and ruthenium compounds respectively by reduction.
[0012] Examples of suitable silver compounds include silver acetate, silver sulfate, and preferably silver nitrate.
[0013] Examples of suitable ruthenium compounds include ruthenium oxalate, ruthenium acetate, and in particular ruthenium nitrosyl nitrate.
[0014] Particularly preferred is the use of a combination of silver nitrate and ruthenium nitrosyl nitrate as a combination of precursor compounds in the first method according to the present invention.
[0015] The particles of the inorganic material used in the first method according to the present invention have an average particle size (d50) in the range of 50 nm to 40 μm and a particle size in the range of 1 μm to 20 μm. 2 / g to 2000m 2 / g range, the material itself is selected from the group consisting of aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in anatase form, titanium dioxide in rutile form, pyrogenic silica (pyrogenic silicon dioxide), precipitated silica (precipitated silica), sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-aluminum hydroxide. In other words, the particles are composed of a material selected from the group consisting of aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in anatase form, titanium dioxide in rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-aluminum hydroxide. Preferred are corresponding particles of titanium nitride, corundum, titanium dioxide in anatase or rutile form, pyrogenic or precipitated silica and gamma-aluminum hydroxide.
[0016] The reduction occurring in the first method according to the invention can be carried out at an alkaline pH in the range of 9 to 14, preferably 10 to 12, and at a suitable temperature with a reducing agent selected from the group consisting of sodium borohydride, hydrazine, hypophosphite and formates. For example, sodium borohydride or hydrazine can conveniently work in the temperature range of 20°C to 40°C; for example, hypophosphite or formates can conveniently work in the temperature range of 60°C to 90°C.
[0017] Hydrazine can be used as such, but is preferably used as hydrazine hydrate with a hydrazine content in the range of 30% to 65% by weight. Hydrazine can also be used as a hydrazine salt, for example as hydrazine sulfate. Preference is given to working with hydrazine hydrate.
[0018] Hypophosphites and formates are mentioned in this text. These are salts, in particular alkali metal salts, alkaline earth metal salts and ammonium salts (NH4 salts). Preferred are sodium and potassium hypophosphites or sodium and potassium formate.
[0019] In the first method according to the invention, in order to completely reduce the silver and ruthenium precursors to elemental silver and elemental ruthenium, the reducing agent is used in a stoichiometric amount or more, but preferably in an amount not exceeding 110% (hydrazine as reducing agent) or not exceeding 200% (sodium borohydride, hypophosphite or formate as reducing agent) of the stoichiometric amount. Using hydrazine as an example for explanation, this means that 1 mol of the reducing agent hydrazine can provide 4 mol of electrons with reducing effect and thus release 1 mol of N2 in the reduction; thus, for example, 1 mol of Ag is reduced. + 0.25 mol of hydrazine is needed to reduce 1 mol of Ru 3+ 0.75 mol of hydrazine is required.
[0020] Two embodiments of the first method according to the invention for preparing the particulate inorganic material according to the invention equipped with elemental silver and elemental ruthenium are disclosed below.
[0021] In a first embodiment, the first preparation method according to the present invention comprises the following consecutive steps:
[0022] (1a) providing an aqueous suspension comprising water, inorganic material particles, at least one silver precursor and at least one ruthenium precursor,
[0023] (2a) contacting the aqueous suspension with a reducing agent selected from the group consisting of sodium borohydride, hydrazine, hypophosphite and formates at an alkaline pH as described above and at a suitable temperature as described above,
[0024] (3) separating the formed solid from the aqueous phase,
[0025] (4) optionally washing the separated solid with water, and
[0026] (5) optionally drying the solid.
[0027] The order of steps (1a) to (5) involves consecutive steps, and they may be directly consecutive steps without intermediate steps.
[0028] In step (1a) of the first embodiment of the first method according to the present invention, an aqueous suspension comprising water, inorganic material particles, at least one silver precursor and at least one ruthenium precursor is provided.
[0029] The aqueous suspension may be prepared by adding inorganic material particles to an aqueous solution of at least one silver precursor and an aqueous solution of at least one ruthenium precursor and suspending them therein.
[0030] However, preference is given to working in the following manner: the silver precursor and the ruthenium precursor, preferably in each case as aqueous solutions, are added simultaneously or in any order (overlapping with a time delay, alternating or successively) to the initial charge aqueous suspension of the inorganic material particles. Particular preference is given to adding aqueous solutions of both precursors (at least one silver precursor and at least one ruthenium precursor) to the initial charge aqueous suspension of the inorganic material particles. In general, mixing is carried out during and also after the addition, for example by means of stirring. It may also be advantageous to carry out mixing when the pH of the aqueous suspension is in the pH range that prevails in the subsequent step (2a); for this purpose, a base, in particular an alkali metal hydroxide, in particular sodium hydroxide or potassium hydroxide, may be added to adjust the pH accordingly.
[0031] The weight ratio of the inorganic material particles of the aqueous suspension provided in step (1a) of the first embodiment of the first method according to the present invention may be, for example, in the range of 5 wt % to 30 wt %.
[0032] The weight ratio of the precious metal formed by silver and ruthenium in the aqueous suspension provided in step (1a) of the first embodiment of the first method according to the present invention can be, for example, in the range of 1% by weight to 20% by weight. The aqueous suspension provided in step (1a) of the first embodiment of the first method according to the present invention is characterized in that the weight of the two precious metals is, for example, in the range of 1 part by weight to 2000 parts by weight of silver: 1 part by weight of ruthenium and is generally significantly in favor of silver.
[0033] The aqueous suspension provided in step (1a) of the first embodiment of the first method according to the present invention generally contains only water and optionally a base for adjusting the pH, in addition to the inorganic material particles and the noble metal precursor.
[0034] In step (2a) of the first embodiment of the first method according to the invention, the aqueous suspension provided in step (1a) is contacted with a reducing agent selected from the group consisting of sodium borohydride, hydrazine, hypophosphite and formates at an alkaline pH as described above and a suitable temperature as described above. If necessary, the corresponding pH and the corresponding temperature of the aqueous suspension can be adjusted first in this case. The alkaline pH can be adjusted using a base, in particular an alkali metal hydroxide, especially sodium hydroxide or potassium hydroxide. As described above, the reducing agent is used in the stoichiometric amount required or more for completely reducing the silver and ruthenium precursors to elemental silver and elemental ruthenium, respectively. It is preferred to work in the following way: the reducing agent is added to the aqueous suspension in the form of an aqueous solution. Preferably, the addition is carried out within a period of 10 minutes to 60 minutes. It is advantageous to mix during the addition and usually also after the addition, for example by stirring.
[0035] In a second embodiment, the first preparation method according to the present invention comprises the following consecutive steps:
[0036] (1b) providing an alkaline aqueous suspension comprising water, inorganic material particles, a base and a reducing agent selected from the group consisting of sodium borohydride, hydrazine, hypophosphite and formates,
[0037] (2b) contacting the aqueous suspension (i) with an aqueous solution comprising at least one silver precursor and at least one ruthenium precursor, or (ii) with an aqueous solution comprising at least one silver precursor and then with an aqueous solution comprising at least one ruthenium precursor, or (iii) with an aqueous solution comprising at least one ruthenium precursor and then with an aqueous solution comprising at least one silver precursor, at an alkaline pH as described above and at a suitable temperature as described above,
[0038] (3) separating the formed solid from the aqueous phase,
[0039] (4) optionally washing the separated solid with water, and
[0040] (5) Optionally drying the solid.
[0041] The order of steps (1b) to (5) involves consecutive steps, and they may be directly consecutive steps without intermediate steps.
[0042] In step (1b) of the second embodiment of the first method according to the present invention, an alkaline aqueous suspension comprising water, inorganic material particles, a base and a reducing agent is provided, the reducing agent being selected from the group consisting of sodium borohydride, hydrazine, hypophosphite and formates. The alkaline aqueous suspension can be prepared by adding the inorganic material particles to an aqueous solution of the reducing agent and suspending them therein. However, it is preferred to work in the following manner: the reducing agent, preferably as an aqueous solution, is added to the initial feed aqueous suspension of the inorganic material particles. The alkaline pH can be adjusted using a base, in particular an alkali metal hydroxide, especially sodium hydroxide or potassium hydroxide, advantageously within the pH range that prevails in the subsequent step (2b). It is advantageous to mix during and usually also after the addition, for example by stirring.
[0043] The weight ratio of the inorganic material particles in the aqueous suspension provided in step (1b) of the second embodiment of the first method according to the present invention may be, for example, in the range of 5 wt % to 30 wt %.
[0044] The weight proportion of the reducing agent in the aqueous suspension provided in step (1b) of the second embodiment of the first method according to the present invention may, for example, be in the range of 0.5% to 10% by weight.
[0045] The aqueous suspension provided in step (1b) of the second embodiment of the first method according to the present invention generally contains only water and a base for adjusting the pH, in addition to the inorganic material particles and the reducing agent.
[0046] In step (2b) of the second embodiment of the first method according to the invention, the aqueous suspension provided in step (1b) is contacted (i) with an aqueous solution comprising at least one silver precursor and at least one ruthenium precursor, or (ii) with an aqueous solution comprising at least one silver precursor and then with an aqueous solution comprising at least one ruthenium precursor, or (iii) with an aqueous solution comprising at least one ruthenium precursor and then with an aqueous solution comprising at least one silver precursor, at an alkaline pH as described above and a suitable temperature as described above. As described above, a single reducing agent is used in the stoichiometrically required amount or more for the complete reduction of the silver and ruthenium precursors to elemental silver and elemental ruthenium, respectively. Preference is given to working according to variant (i).
[0047] The weight ratio of the precious metal formed by silver and ruthenium in the aqueous suspension provided in step (1b) of the second embodiment of the first method according to the present invention can be, for example, in the range of 1% by weight to 20% by weight. The aqueous suspension provided in step (1b) of the second embodiment of the first method according to the present invention is characterized in that the weight of the two precious metals is, for example, in the range of 1 part by weight to 2000 parts by weight of silver: 1 part by weight of ruthenium and is generally significantly in favor of silver.
[0048] Mixing is advantageously carried out during and generally also after the contacting according to step (2b), for example by stirring, for example over a period of 1 to 2 hours.
[0049] Steps (3) to (5) are the same in both embodiments of the first method according to the present invention.
[0050] In step (3), the solid formed in the corresponding step (2a) or (2b) is separated from the aqueous phase. Examples of solid-liquid separation methods suitable for this purpose include methods known to those skilled in the art, such as decantation, pressing, filtration, suction filtration, centrifugation or a combination thereof.
[0051] Step (4) of the first process according to the invention is an optional but generally advantageous step in which the solid separated in step (3) can be washed with water. Water-soluble components can be removed here. The washing can be carried out, for example, on a Nutsche filter.
[0052] Step (5) of the first method according to the invention is an optional but generally advantageous step, in which the solid separated in step (3) and optionally washed in step (4) can be dried. In this case, the water present and any other volatile components are removed from the solid obtained after completion of step (3) or step (4). Water can be removed in the sense of almost completely removing water, or in the sense of removing water until the desired residual moisture content is reached. For this purpose, most of the water can be removed by conventional methods, such as pressing, filter pressing, suction filtration, centrifugation or the like, and then drying, optionally supported by reduced pressure, is carried out at a temperature in the range of, for example, 20° C. to 150° C.
[0053] After completion of step (3) or optionally (4) or optionally (5) and optionally subsequent comminution and / or classification, a particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention is obtained. Silver and ruthenium may be present on the inner surface (in the pores and / or cavities) and / or on the outer surface of the inorganic material particles that are initially free of silver and free of ruthenium, and may thus form, for example, discontinuous layers and / or small silver or ruthenium particles (silver or ruthenium islands). Scanning electron microscopy may be a suitable method for observing such morphological properties. Silver and ruthenium are not alloyed, but statistically distributed, and the two noble metals are at least partially in contact with each other. It is clear to a person skilled in the art that silver and ruthenium may include other silver substances other than elemental metallic silver and other ruthenium substances other than elemental metallic ruthenium on their surfaces, such as corresponding oxides, halides and / or sulfides. Such substances may be formed during or after the execution of the first method according to the invention, for example during storage, use or further processing of the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention.
[0054] In a second method according to the invention, the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention can be obtained by pyrolysis treatment under a reducing atmosphere of a previously dried preparation which, before drying, already contained water, particles of the corresponding inorganic material, at least one silver precursor and at least one ruthenium precursor.
[0055] In the second method according to the present invention, inorganic material particles, a silver precursor, and a ruthenium precursor are used.
[0056] The silver precursor and the ruthenium precursor used in the second method according to the invention are silver and ruthenium compounds which can be thermally decomposed under a reducing atmosphere into elemental silver and elemental ruthenium, respectively.
[0057] Examples of suitable silver compounds include silver acetate and, preferably, silver nitrate.
[0058] Examples of suitable ruthenium compounds include ruthenium oxalate, ruthenium acetate, and in particular ruthenium nitrosyl nitrate.
[0059] It is particularly preferred to use a combination of silver nitrate and ruthenium nitrosyl nitrate as a combination of precursor compounds in the second method according to the present invention.
[0060] The inorganic material particles used in the second method according to the present invention have an average particle size (d50) in the range of 50 nm to 40 μm and an average particle size (d50) in the range of 1 μm to 40 μm. 2 / g to 2000m 2 / g range, the material itself is selected from the following materials, which are selected from the group consisting of aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in anatase form, titanium dioxide in rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-aluminum hydroxide. In other words, the particles are composed of materials selected from the group consisting of aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in anatase form, titanium dioxide in rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-aluminum hydroxide. Preferred are corresponding particles of titanium nitride, corundum, titanium dioxide in anatase or rutile form, pyrogenic or precipitated silica and gamma-aluminum hydroxide.
[0061] The second preparation method according to the present invention comprises the following consecutive steps:
[0062] (1c) providing a preparation comprising water, inorganic material particles, at least one silver precursor and at least one ruthenium precursor,
[0063] (2c) drying the preparation provided in step (1c), and
[0064] (3c) subjecting the dried preparation obtained after completing step (2c) to a pyrolysis treatment under a reducing atmosphere.
[0065] The order of steps (1c) to (3c) involves consecutive steps, and they may be directly consecutive steps without intermediate steps.
[0066] In step (1c) of the second method according to the present invention, a preparation comprising water, inorganic material particles, at least one silver precursor and at least one ruthenium precursor is provided. The preparation may be in the form of an aqueous suspension or in the form of impregnated particles. The two forms (a) aqueous suspension and (b) impregnated particles differ in the presence or absence of an aqueous liquid between the particles; while in the case of an aqueous suspension, an aqueous liquid is present between the particles, this is not the case with the impregnated particles, which have the appearance of a dry or free-flowing powder, and the aqueous liquid forms a component of the particles or is within the particles.
[0067] The aqueous suspension may be prepared by adding inorganic material particles to an aqueous solution of at least one silver precursor and an aqueous solution of at least one ruthenium precursor and suspending them therein.
[0068] However, preference is given to working in such a way that the silver precursor and the ruthenium precursor, preferably in each case as aqueous solutions, are added simultaneously or in any order (overlapping with a time delay, alternating or successively) to the initial charge aqueous suspension of the inorganic material particles. Particular preference is given to adding aqueous solutions of both precursors (at least one silver precursor and at least one ruthenium precursor) to the initial charge aqueous suspension of the inorganic material particles. In general, mixing is carried out during and also after the addition, for example by means of stirring.
[0069] The weight ratio of the inorganic material particles in the aqueous suspension provided in step (1c) of the second embodiment of the second method according to the present invention may be, for example, in the range of 5 wt % to 30 wt %.
[0070] The weight ratio of the precious metal formed by silver and ruthenium in the aqueous suspension provided in step (1c) of the second method according to the present invention can be, for example, in the range of 1% by weight to 20% by weight. The aqueous suspension provided in step (1c) of the second method according to the present invention is characterized in that the weight of the two precious metals is, for example, in the range of 1 part by weight to 2000 parts by weight of silver: 1 part by weight of ruthenium and is generally significantly in favor of silver.
[0071] Besides the inorganic material particles and the noble metal precursor, the aqueous suspension provided in step (1c) of the second method according to the invention generally comprises only water and optionally the corresponding acid from the noble metal precursor.
[0072] The preparation in the form of impregnated particles is preferred. It can be carried out by impregnating the inorganic material particles with an aqueous solution of at least one silver precursor and at least one ruthenium precursor in a manner commonly used in the art. The impregnation process can be carried out once or repeatedly, in the latter case, a drying step is carried out between each impregnation step.
[0073] The impregnation process must be carried out in such a way that no aqueous suspension is produced, i.e., neither a thin slurry nor a slurry, paste or dough-like substance is produced, but rather impregnated particles in the form of a macroscopically uniform and free-flowing powder are formed. In other words, the volume of the aqueous solution must be selected to be small enough and suitable for impregnating the inorganic material particles with it. When impregnating, it is advantageous to allow the particles of the inorganic material to mix with the aqueous solution for a sufficient time. For example, it may be appropriate to mix for a sufficiently long time, in particular until the macroscopic uniform state of the mixed material is achieved. The volume of the aqueous solution can be selected by adjusting the corresponding concentration of the noble metal precursor to the amount of particles of the inorganic material to be contacted therewith and their absorption behavior to the aqueous solution. If the volume is too large, the aforementioned undesirable slurry, slurry, dough or paste is produced. Those skilled in the art can easily determine the absorption behavior of the relevant inorganic material particles to the relevant aqueous solution in a directed laboratory test, and therefore determine the upper limit of the number of liters of the aqueous solution per kilogram of inorganic material particles without any loss of the free flowability.
[0074] The weight ratio of the inorganic material particles in the impregnated particles provided in step (1c) of the second method according to the present invention may be, for example, in the range of 50 wt % to 90 wt %.
[0075] The weight ratio of the precious metal formed by silver and ruthenium in the impregnated particles provided in step (1c) of the second method according to the invention can be, for example, in the range of 3% to 15% by weight. The impregnated particles provided in step (1c) of the second method according to the invention are characterized in that the weight of the two precious metals is, for example, in the range of 1 to 2000 parts by weight of silver: 1 part by weight of ruthenium and is generally significantly in favor of silver.
[0076] In addition to the inorganic material particles and the noble metal precursor, the impregnated particles provided in step (1c) of the second method according to the invention generally contain only water and optionally the corresponding acid from the noble metal precursor. The water content of the impregnated particles provided in step (1c) of the second method according to the invention may, for example, be in the range of 7 wt % to 35 wt %.
[0077] In step (2c) of the second process according to the invention, the preparation provided in step (1c) is dried, ie water and any other volatile substances present are removed.
[0078] In the case of an aqueous suspension, it is evaporated to dryness. Advantageously, the aqueous suspension is stirred during concentration, for example by stirring and / or shaking and / or rotating, i.e. rotating the reservoir or container containing the aqueous suspension. Generally speaking, heating and / or negative pressure are applied during concentration to remove water and any other volatile substances that may be present. During concentration, it is possible to work, for example, at a temperature ranging from 40° C. to 95° C. If desired, the material obtained after drying can be comminuted.
[0079] In the case of impregnated particles, these may be dried in an oven at a temperature in the range of, for example, 40° C. to 95° C. Negative pressure may be applied to assist the process. The dried material may be pulverized if desired.
[0080] In step (3c) of the second method according to the invention, the noble metal precursor is thermally decomposed to form elemental silver and elemental ruthenium. For this purpose, the material obtained after completion of step (2c) and optionally pulverized undergoes a pyrolysis treatment under a reducing atmosphere. For this purpose, the material can be heated in a stationary state or in motion, for example in a static furnace, a fluidized bed reactor or a rotary kiln, to a target temperature that ensures the thermal decomposition of the noble metal precursor to form the corresponding elemental noble metal, for example in the range of 150° C. to 800° C.
[0081] As used herein, the term "reducing atmosphere" refers to an atmosphere consisting of a gas containing reducing properties (such as hydrogen), or a mixture of an inert gas (such as nitrogen or argon) and hydrogen, the volume fraction of the latter being in particular in the range of 5% to 10% by volume. During step (3c), the furnace chamber is advantageously flushed with a gas containing reducing properties; the gas stream can also be used to remove gaseous decomposition products.
[0082] After completion of step (3c) and optionally subsequent comminution and / or classification, a particulate inorganic material containing elemental silver and elemental ruthenium according to the present invention is obtained. Silver and ruthenium may be present on the inner surface (in the pores and / or cavities) and / or outer surface of the inorganic material particles that are initially free of silver and ruthenium, and may thus form, for example, discontinuous layers and / or small silver or ruthenium particles (silver or ruthenium islands). Scanning electron microscopy may be a suitable method for observing such morphological properties. Silver and ruthenium are not alloyed, but statistically distributed, and the two precious metals are at least partially in contact with each other. It is clear to a person skilled in the art that silver and ruthenium may include other silver substances other than elemental metallic silver and other ruthenium substances other than elemental metallic ruthenium on their surfaces, such as corresponding oxides, halides and / or sulfides. Such substances may be formed during or after the execution of the second method according to the present invention, for example during the storage, use or further processing of the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the present invention.
[0083] The particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention is characterized by a correspondingly low lightness L*, for example a dark or black color in the range of 35 to 45, which can be disruptive for some applications. The lightness L* is a specific *L* in the CIEL*a*b* color space (DIN EN ISO / CIE11664-4:2020-03) determined spectrophotometrically in a measuring geometry of d / 8°; the spectrophotometric measurement of the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention can be carried out on samples which are poured into a colorless glass container to a filling height of 1 cm via the glass flat bottom of the glass container placed on the measuring head of the spectrophotometer used.
[0084] If desired, the particulate inorganic material provided with elemental silver and elemental ruthenium according to the invention can be further processed to form a brightening particulate material having a brightness L*, for example, in the range of 50 to 85. For brightening purposes, the particulate inorganic material provided with elemental silver and elemental ruthenium according to the invention can be contacted with at least one C1 to C4 alkoxide of aluminum, magnesium, calcium, silicon, zinc, zirconium and / or titanium in the presence of at least an amount of water sufficient to completely hydrolyze the at least one C1 to C4 alkoxide. As described above, a brightening particulate material can be formed, i.e. a particulate material having a color, for example gray, having a brightness L*, for example, in the range of 50 to 85. The brightening particulate material consists of the particulate inorganic material provided with elemental silver and elemental ruthenium according to the invention, the particulate carbon material having a solid at least partially located thereon. According to the selection of at least one C1 to C4 alkoxide, the solid is a solid selected from the group consisting of aluminum oxide, aluminum hydroxide, aluminum oxyhydroxide, magnesium oxide, magnesium hydroxide, magnesium oxyhydroxide, calcium oxide, calcium hydroxide, calcium oxyhydroxide, silicon dioxide, silica, zinc oxide, zinc hydroxide, zinc oxyhydroxide, zirconium dioxide, zirconium (IV) oxyhydroxide, titanium dioxide, titanium (IV) oxyhydroxide and combinations thereof.
[0085] The particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention, optionally brightened as described above, is characterized by a particularly high antimicrobial effect, as can be determined in a conventional inhibition zone test or by determining the minimum inhibition concentration from the growth curve of the microorganisms. In this respect, the invention also relates to the use of the particulate inorganic material equipped with elemental silver and elemental ruthenium according to the invention, optionally brightened, as an additive for the antimicrobial treatment of: metal surfaces; coating agents, such as varnishes and other coatings; plasters; moulding materials; plastic materials in the form of plastic films, plastic parts or plastic fibers; synthetic resin products; ion exchange resins; silicone products; cellulose-based products; foams; cosmetics; and many others.
[0086] The particulate inorganic material according to the invention equipped with elemental silver and elemental ruthenium, optionally brightened as described above, can also act as a heterogeneous catalyst in the catalytic formation of hydroxyl radicals, for example in an aqueous medium permissive for bacterial growth.
[0087] The particulate inorganic material according to the invention equipped with elemental silver and elemental ruthenium, optionally brightened as described above, can be used in the abovementioned uses as dry powder, as powder with residual moisture or desired moisture content or as aqueous suspension. Example
[0088] Reference Example 1 (cellulose powder provided with 18.9 wt. % of elemental silver and 1.0 wt. % of elemental ruthenium) Reductive preparation):
[0089] 75.6 g (445 mmol) of solid silver nitrate and 13.94 g of ruthenium nitrosyl nitrate solution (ruthenium content 19.0 wt. %; 26.2 mmol Ru) were dissolved in 416.8 g of deionized water, and the precursor aqueous solution obtained in this way was mixed with 211.2 g of cellulose powder (from Rettenmaier und GmbH & Co KG L-600) was uniformly mixed to form an orange, free-flowing impregnated particulate material. At room temperature, 705 mL of a hydrazine aqueous solution with a pH of 13.9 [4.19 g (131 mmol) hydrazine and 81.81 g of a 32 wt. % sodium hydroxide solution (654.51 mmol NaOH, the remainder: water] was metered into the free-flowing impregnated particulate material at a metering rate of 30 mL / min while stirring. Over time, a homogeneous slurry that was easy to stir was formed. After the metering was completed, stirring was continued for 30 minutes until nitrogen release was no longer observed. The material was then filtered off with suction, washed with a total of 1,000 mL of water and dried in a drying oven at 105°C / 300 mbar to a residual moisture content of 15 wt. %. The silver content of the final product of 18.9 wt. % and the ruthenium content of 1.0 wt. % (relative to 0 wt. % residual moisture) were determined by ICP-OES.
[0090] Example 2 according to the invention (particles provided with 18.8 wt. % of elemental silver and 1.0 wt. % of elemental ruthenium) Reductive preparation of inorganic materials):
[0091] 52.5 g of an aqueous solution of silver nitrate (silver content 36.2 wt. %; 176 mmol Ag) and 5.4 g of an aqueous solution of ruthenium nitrosyl nitrate (ruthenium content 18.7 wt. %; 10 mmol Ru) were added to 80 g of silicon dioxide (silicon dioxide from Evonik). 150) in a suspension in 1500 mL of water. The suspension was stirred at 80° C. for 7 hours. The suspension was then cooled to 30° C., a solution consisting of 2.6 g of hydrazine hydrate (hydrazine content 64% by weight; 52 mmol), 32.2 g of sodium hydroxide solution (sodium hydroxide content 32%) and 250 mL of water was metered in over a period of 10 minutes and stirred for a further 5 hours. The material was then filtered off with suction, washed with a total of 5 L of water and dried in a drying oven at 105° C. / 300 mbar and ground with an agate mortar. The product had a silver content of 18.8% by weight and a ruthenium content of 1.0% by weight (relative to a residual moisture content of 0% by weight) determined with the aid of ICP-OES.
[0092] Example 3 according to the invention (particles provided with 18.3% by weight of elemental silver and 0.8% by weight of elemental ruthenium) Pyrolysis preparation of inorganic materials):
[0093] 52.5 g of aqueous silver nitrate solution (silver content 36.2 wt. %; 176 mmol Ag) and 5.4 g of aqueous ruthenium nitrosyl nitrate solution (ruthenium content 18.7 wt. %; 10 mmol Ru) were added to 80 g of silicon dioxide (from Evonik 150) in a suspension in 1500mL water. The suspension was stirred at 80°C for 7 hours. The material was then concentrated to dryness using a rotary evaporator (90°C / 350mbar). The dried material was then calcined at 250°C for 5 hours in a tubular furnace under a synthetic gas atmosphere (5% by volume hydrogen / 95% by volume nitrogen) and crushed with an agate mortar. The product had a silver content of 18.3% by weight and a ruthenium content of 0.8% by weight (relative to 0% by weight residual moisture) determined by ICP-OES.
[0094] Example 4 according to the invention (particles provided with 18.0 wt. % of elemental silver and 1.0 wt. % of elemental ruthenium) Pyrolysis preparation of inorganic materials):
[0095] An aqueous solution prepared from 8.8 g of aqueous silver nitrate solution (silver content 36.2 wt. %; 29 mmol Ag) and 0.9 g of aqueous ruthenium nitrosyl nitrate solution (ruthenium content 18.7 wt. %; 1.7 mmol Ru) was added to 40 g of boehmite powder (Nabaltec) while shaking. 200SM). The material was then dried in a drying oven at 105° C. / 300 mbar. The process was repeated three times until a total of 26.2 g of aqueous silver nitrate solution (silver content 36.2% by weight; 88 mmol Ag) and 2.7 g of aqueous ruthenium nitrosyl nitrate solution (ruthenium content 18.7% by weight; 5 mmol Ru) had been used. The material was then calcined at 250° C. for 5 hours in a tube furnace under a forming gas atmosphere (5% by volume hydrogen / 95% by volume nitrogen) and crushed with an agate mortar. The product had a silver content of 18.0% by weight and a ruthenium content of 1.0% by weight (relative to 0% by weight of residual moisture) determined by means of ICP-OES.
[0096] Example 5 (Testing of the products of Reference Example 1 and Examples 2 and 3 according to the present invention for comparison Their antimicrobial effects):
[0097] In a separate conical flask, 30mL of methicillin-resistant Staphylococcus aureus (MRSA) culture in tryptic soy broth (TSB) was adjusted to an optical density of 0.05. Then weigh different amounts of the product from reference example 1 in the range of 1 mg to 20 mg. The sample was incubated in a shaking incubator at 37 ° C and 150 rpm. Within 6 hours, the optical density (OD600) at a wavelength of 600 nm was determined at hourly intervals. The inhibition of bacterial growth is indicated by the increase in optical density compared to the control sample. MRSA cultures without the addition of active antimicrobial substances were used as control samples. In the case of complete inhibition of bacterial growth, no increase in optical density was observed. The corresponding sample amount of the product of reference example 1 or embodiments 2 to 4 according to the present invention is used to calculate the minimum inhibitory concentration. This results in a minimum inhibitory concentration of 0.55 mg / mL for the product from reference example 1 and, in contrast, a lower minimum inhibitory concentration of 0.40 mg / mL for the product from example 2 according to the invention, a lower minimum inhibitory concentration of 0.40 mg / mL for the product from example 3 according to the invention and a lower minimum inhibitory concentration of 0.35 mg / mL for the product from example 4 according to the invention.
Claims
1. A particulate inorganic material provided with elemental silver and elemental ruthenium, said inorganic material having an average particle size (d50) in the range of 50 nm to 40 μm and a particle size (d50) in the range of 1 nm to 40 μm. 2 / g to 1600m 2 / g range, wherein the inorganic material itself is selected from the group consisting of aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in anatase form, titanium dioxide in rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolite, hydrotalcite and gamma-alumina hydroxide.
2. The particulate inorganic material provided with elemental silver and elemental ruthenium according to claim 1, wherein the particulate inorganic material has a weight ratio of silver plus ruthenium formed by the elemental silver and the elemental ruthenium in the range of 0.1% by weight to 50% by weight, wherein the weight ratio of silver:ruthenium which prevails simultaneously is in the range of 1 part by weight to 2000 parts by weight of silver: 1 part by weight of ruthenium.
3. A method for preparing a particulate inorganic material provided with elemental silver and elemental ruthenium according to claim 1 or claim 2, said method The following steps are involved: reducing at least one silver precursor and at least one ruthenium precursor in the presence of water-suspended particles of the corresponding inorganic materials; separating the solid formed during the reduction from the aqueous phase; optionally washing the separated solid with water; and optionally drying the separated and optionally washed solid.
4. The method of claim 3, wherein the silver and ruthenium precursors are reduced sequentially or simultaneously.
5. The method of claim 3 or claim 4, wherein the at least one silver precursor is selected from the group consisting of silver acetate, silver sulfate and silver nitrate, and wherein the at least one ruthenium precursor is selected from the group consisting of ruthenium oxalate, ruthenium acetate and ruthenium nitrosyl nitrate.
6. The method according to any one of claims 3 to 5, wherein the particles of the inorganic material are selected from the group consisting of a material having an average particle size (d50) in the range of 50 nm to 40 μm and a particle size in the range of 1 μm to 20 μm. 2 / g to 2000m 2 Particles having a BET surface area in the range of 1:1 to 1:1 / g: aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in the anatase form, titanium dioxide in the rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolites, hydrotalcites and gamma-aluminum oxide hydroxide.
7. The process according to any one of claims 3 to 6, wherein the reduction is carried out at an alkaline pH in the range of 9 to 14 and a temperature in the range of 20°C to 40°C with a reducing agent selected from the group consisting of sodium borohydride and hydrazine, or at a temperature of 60°C to 90°C with a reducing agent selected from the group consisting of hypophosphites and formates.
8. A method for preparing a particulate inorganic material equipped with elemental silver and elemental ruthenium according to claim 1 or claim 2, wherein before drying, the dry preparation which already contains water, particles of the corresponding inorganic material, at least one silver precursor and at least one ruthenium precursor is subjected to a pyrolysis treatment under a reducing atmosphere.
9. The method of claim 8, wherein the at least one silver precursor is selected from the group consisting of silver acetate, silver sulfate, and silver nitrate, and wherein the at least one ruthenium precursor is selected from the group consisting of ruthenium oxalate, ruthenium acetate, and ruthenium nitrosyl nitrate.
10. The method according to claim 8 or claim 9, wherein the particles of the inorganic material are selected from the group consisting of a material having an average particle size (d50) in the range of 50 nm to 40 μm and a particle size in the range of 1 μm to 20 μm. 2 / g to 2000m 2 Particles having a BET surface area in the range of 1:1 to 1:1 / g: aluminum nitride, titanium nitride, silicon nitride, corundum, titanium dioxide in the anatase form, titanium dioxide in the rutile form, pyrogenic silica, precipitated silica, sodium aluminum silicate, zirconium silicate, zeolites, hydrotalcites and gamma-aluminum oxide hydroxide.
11. The method according to any one of claims 8 to 10, comprising the following consecutive steps: (1c) providing a preparation comprising water, the inorganic material particles, at least one silver precursor and at least one ruthenium precursor, (2c) drying the preparation provided in step (1c), and (3c) subjecting the dried preparation obtained after completing step (2c) to a pyrolysis treatment under a reducing atmosphere.
12. The method according to claim 11, wherein the preparation provided in step (1c) is in the form of an aqueous suspension or in the form of impregnated particles.
13. A method according to any one of claims 3 to 12, wherein the particulate inorganic material provided with elemental silver and elemental ruthenium is further treated to form a brightening particulate material having a brightness L* in the range of 50 to 85 by contacting the resulting particulate inorganic material equipped with elemental silver and elemental ruthenium with at least one C1 to C4 alkoxide of aluminum, magnesium, calcium, silicon, zinc, zirconium and / or titanium in the presence of an amount of water at least sufficient to completely hydrolyze the at least one C1 to C4 alkoxide.
14. Use of the particulate inorganic material equipped with elemental silver and elemental ruthenium according to claim 1 or claim 2 or the product produced by the process according to any one of claims 3 to 13, as an additive for the antimicrobial treatment of metal surfaces; coating agents; plasters; molding compounds; plastics in the form of plastic films, plastic parts or plastic fibers; textiles; textile applications; synthetic resin products; ion exchange resins; silicone products; cellulose-based products; foams; and cosmetics.
15. Use of a particulate inorganic material equipped with elemental silver and elemental ruthenium according to claim 1 or claim 2, or a product prepared by a process according to any one of claims 3 to 13, as a heterogeneous catalyst in the catalysis of the formation of hydroxyl radicals in an aqueous medium allowing bacterial growth.
Citation Information
Patent Citations
Method for producing a particulate carrier material provided with elementary silver and elementary ruthenium
WO2021084140A2