Slurry composition for functional layer of non-aqueous secondary battery, method for producing same, separator for non-aqueous secondary battery, and non-aqueous secondary battery

By using a slurry composition containing a specific bonding material in the functional layer of the secondary battery, the problems of insufficient anti-adhesion, electrolyte liquid injection and high-temperature cycle characteristics in the prior art are solved, and a high-level performance is achieved.

CN118922995APending Publication Date: 2024-11-08ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028333.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing secondary battery functional layer has shortcomings in improving the anti-blocking properties, electrolyte liquid injection properties, and high-temperature circulation characteristics, and it is difficult to take into account high-level performance.

Method used

Using a slurry composition containing a particulate polymer and a specific bonding material, the glass transition temperature of the particulate polymer is above 30°C and below 95°C. The bonding material comprises hydroxyl groups and acidic functional groups and alkali metal salt groups, preferably ethylene. A copolymer of alcohol and an ethylenically unsaturated carboxylic acid alkali metal neutralizer and a functional layer is formed on the spacer.

Benefits of technology

The functional layer has excellent anti-blocking properties, electrolyte liquid injection properties and high-temperature circulation characteristics, and the overall performance of the secondary battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047226010000371
    Figure BDA0005047226010000371
  • Figure BDA0005047226010000381
    Figure BDA0005047226010000381
Patent Text Reader

Abstract

A slurry composition for a functional layer of a non-aqueous secondary battery, which contains a particulate polymer having a glass transition temperature within a predetermined range and a binder (A) containing an alkali metal salt group and a hydroxyl group and / or an acidic functional group.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a slurry composition for a non-aqueous secondary battery functional layer and a method for producing the same, a separator for a non-aqueous secondary battery, and a non-aqueous secondary battery. Background Art

[0002] Non-aqueous secondary batteries such as lithium-ion secondary batteries (hereinafter sometimes simply referred to as “secondary batteries”) are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications.

[0003] Here, the secondary battery generally has an electrode (positive electrode and negative electrode), and a separator that isolates the positive electrode from the negative electrode and prevents a short circuit between the positive electrode and the negative electrode. In addition, a porous film layer for improving heat resistance and strength, an adhesive layer for improving the adhesion between battery components, etc. (hereinafter, sometimes collectively referred to as "functional layer") are provided on the surface of the electrode and / or separator. Specifically, an electrode formed by further forming a functional layer on an electrode substrate formed by arranging an electrode composite material layer on a current collector, and a separator formed by forming a functional layer on a separator substrate are used as battery components.

[0004] In the past, various studies have been conducted on compositions for forming functional layers for the purpose of improving the electrochemical characteristics of the obtained secondary batteries. For example, Patent Documents 1 and 2 propose that a polymer compound containing acrylic repeating units and having ONa groups and OLi groups be added to a binder material for a secondary battery. In addition, for example, Patent Documents 3 and 4 disclose that a granular polymer having a glass transition temperature that satisfies specified conditions is added as a binder component to be added to a composition for a functional layer.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent document 1: Japanese Patent No. 6888139;

[0008] Patent document 2: International Publication No. 2021 / 172383;

[0009] Patent document 3: International Publication No. 2013 / 151144;

[0010] Patent document 4: International Publication No. 2020 / 175025. Summary of the invention

[0011] Problem that the invention aims to solve

[0012] Here, in the manufacture of secondary batteries, it is necessary that even when the battery components containing the functional layer are temporarily kept in a stacked state, the battery components are not easy to adhere to each other across the functional layer (hereinafter referred to as "anti-adhesion"). In addition, in the manufacture of secondary batteries, it is preferred that when the electrolyte is injected into the outer package containing the battery components, the electrolyte can be well infiltrated into the battery components (i.e., the electrolyte injection is excellent). In addition, the secondary battery also needs to have excellent cycle characteristics at high temperatures. However, the functional layer formed using the functional layer composition according to the above-mentioned prior art has room for improvement in terms of improving anti-adhesion and taking into account the electrolyte injection and high temperature cycle characteristics of the secondary battery having the functional layer at a high level.

[0013] Therefore, an object of the present invention is to provide a slurry composition for a non-aqueous secondary battery functional layer that can provide a functional layer having excellent anti-blocking properties and can provide a secondary battery that can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics.

[0014] Another object of the present invention is to provide a separator for a non-aqueous secondary battery that can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0015] Another object of the present invention is to provide a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics.

[0016] Furthermore, an object of the present invention is to provide a method for efficiently producing the slurry composition for a non-aqueous secondary battery functional layer of the present invention.

[0017] Solutions for solving problems

[0018] The present inventors have conducted intensive research for the purpose of solving the above-mentioned problems, focusing on the properties of the granular polymer used in the formation of the functional layer and the binder material different therefrom. Then, it was newly discovered that when the glass transition temperature of the granular polymer is within a specified range and a polymer containing at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group is used as the binder material, a functional layer with excellent anti-blocking properties can be provided, and at the same time, a non-aqueous secondary battery with excellent electrolyte injection properties and high-temperature cycle characteristics can be provided, thereby completing the present invention.

[0019] That is, the object of the present invention is to advantageously solve the above-mentioned problems. [1] The slurry composition for a non-aqueous secondary battery functional layer of the present invention is characterized in that it contains a granular polymer and a binder material A, the granular polymer has at least one glass transition temperature in the temperature range of 30°C to 95°C, and the binder material A contains at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group. Thus, according to the slurry composition for a functional layer containing a granular polymer and a binder material A, the glass transition temperature of the granular polymer is within the above-mentioned temperature range, and the binder material A contains at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group, the anti-blocking property of the obtained functional layer can be improved, while the electrolyte injection property and high-temperature cycle characteristics of the obtained secondary battery can be taken into account at a high level.

[0020] In addition, the "glass transition temperature" of the particulate polymer is a value determined based on a differential scanning calorimetry (DSC) curve. When the DSC curve has multiple peaks, the temperature shown by the peak with the largest shift is taken as the glass transition temperature of the polymer. When multiple peaks with equal shifts are detected and it is the maximum value among the detected peaks, the average value is taken as the glass transition temperature of the polymer.

[0021] In addition, the functional groups and alkali metal salt groups contained in the adhesive material A can be used 1 H-NMR, 13 C-NMR and other nuclear magnetic resonance (NMR) methods for detection.

[0022] [2] In the non-aqueous secondary battery functional layer slurry composition of [1], the binder material A is preferably a copolymer of vinyl alcohol and an alkali metal neutralized product of an olefinic unsaturated carboxylic acid. If the binder material A is a copolymer of vinyl alcohol and an alkali metal neutralized product of an olefinic unsaturated carboxylic acid, the adhesion of the obtained functional layer in the electrolyte can be further improved, and the high temperature cycle characteristics of the obtained secondary battery can be further improved.

[0023] [3] In addition, in the slurry composition for non-aqueous secondary battery functional layer of [1] or [2], the yellowness index of a 3% by mass aqueous solution of the above-mentioned binder material A is preferably 14.0 or less. If the yellowness index of a 3% by mass aqueous solution of the binder material A is 14.0 or less, the adhesion of the obtained functional layer in the electrolyte can be further improved, and the high temperature cycle characteristics of the obtained secondary battery can be further improved. In addition, the yellowness index of the binder material A can be evaluated according to the method described in the examples of this specification.

[0024] [4] In addition, in the slurry composition for a non-aqueous secondary battery functional layer of any one of [1] to [3] above, the volume average particle size of the granular polymer is preferably greater than 0.25 μm and less than 5 μm. If the volume average particle size of the granular polymer is within the above range, the adhesion of the obtained functional layer can be improved, and the internal resistance of the secondary battery can be reduced. In addition, the "volume average particle size" of the granular polymer refers to the particle size D50 at which the cumulative volume calculated from the small particle size side becomes 50% in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution measuring device. Specifically, it can be measured using the method described in the examples of this specification.

[0025] [5] In the non-aqueous secondary battery functional layer slurry composition according to any one of [1] to [4], the particulate polymer preferably has a core-shell structure. If the particulate polymer has a core-shell structure, the adhesion of the functional layer can be improved, and the high temperature cycle characteristics of the secondary battery obtained can be further improved.

[0026] [6] In addition, the slurry composition for a non-aqueous secondary battery functional layer according to any one of [1] to [5] may further contain heat-resistant particles. If the slurry composition contains heat-resistant particles, a functional layer that improves the heat resistance of a battery member can be appropriately produced.

[0027] [7] In addition, the present invention aims to advantageously solve the above-mentioned problems. The separator for a non-aqueous secondary battery of the present invention is characterized in that it comprises a separator substrate and a functional layer formed on at least a portion of at least one surface of the separator substrate, wherein the functional layer is a dried product of the slurry composition for a non-aqueous secondary battery functional layer of any one of the above [1] to [6]. Thus, the separator having the separator substrate and the functional layer which is a dried product of any one of the above slurry compositions has excellent anti-blocking properties, and can simultaneously achieve both electrolyte injection properties and high-temperature cycle characteristics of the obtained secondary battery at a high level.

[0028] [8] In addition, the present invention aims to advantageously solve the above-mentioned problems. The non-aqueous secondary battery of the present invention is characterized in that it comprises a positive electrode, a negative electrode, a separator and an electrolyte, and the separator is the separator for a non-aqueous secondary battery of [7]. Thus, the secondary battery having the separator can achieve both electrolyte injection properties and high-temperature cycle characteristics at a high level.

[0029] [9] Furthermore, the object of the present invention is to advantageously solve the above-mentioned problems. The method for producing a slurry composition for a non-aqueous secondary battery functional layer of the present invention is the method for producing a slurry composition for a non-aqueous secondary battery functional layer of any one of [1] to [6], characterized in that it comprises the following steps: polymerizing a monomer composition containing at least one of a vinyl ester monomer and an ethylenically unsaturated carboxylic acid ester monomer to obtain a polymer, and further saponifying the polymer in the presence of an alkali metal compound and a reducing agent to obtain a saponified product of the polymer as the above-mentioned binder A. According to this production method, the above-mentioned slurry composition for a functional layer of the present invention can be efficiently produced.

[0030] Effects of the Invention

[0031] According to the present invention, a slurry composition for a nonaqueous secondary battery functional layer can provide a functional layer having excellent anti-blocking properties and a secondary battery having both high electrolyte injection properties and high-temperature cycle characteristics.

[0032] Furthermore, according to the present invention, it is possible to provide a separator for a non-aqueous secondary battery which can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0033] Furthermore, according to the present invention, a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics can be provided.

[0034] Furthermore, according to the present invention, the slurry composition for a non-aqueous secondary battery functional layer of the present invention can be produced efficiently. DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described in detail.

[0036] Here, the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention can be used as a material for preparing the functional layer possessed by battery components such as separators or electrodes. Moreover, the separator for the non-aqueous secondary battery of the present invention has a functional layer formed by the dried product of the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention. Moreover, the non-aqueous secondary battery of the present invention has a separator for the non-aqueous secondary battery of the present invention. Furthermore, according to the method for manufacturing the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention, the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention can be efficiently manufactured. In addition, the so-called functional layer can be an adhesive layer that exerts the bonding ability between the battery component having the functional layer and other battery components as the adherend, or the functional layer can also be a heat-resistant adhesive layer containing heat-resistant particles and capable of exerting heat-resistant functions in addition to the above-mentioned bonding ability.

[0037] (Slurry composition for non-aqueous secondary battery functional layer)

[0038] The slurry composition for a non-aqueous secondary battery functional layer of the present invention contains a particulate polymer and a binder A, and may further contain a solvent and other components as desired.

[0039] Here, the granular polymer included in the slurry composition of the present invention has at least one glass transition temperature in a temperature range of 30°C to 95°C. Furthermore, the binder material A included in the slurry composition of the present invention contains at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group. According to the slurry composition containing both the granular polymer and the binder material A satisfying the specified properties, a functional layer with excellent anti-blocking properties can be provided, and at the same time, a secondary battery that can take into account both electrolyte injection properties and high-temperature cycle characteristics at a high level can be provided.

[0040] <Particle polymer>

[0041] The granular polymer has at least one glass transition temperature in the temperature range of 30°C to 95°C. The granular polymer preferably has no glass transition temperature outside the above range. In addition, the granular polymer is preferably water-insoluble. Here, in the present invention, the polymer is "water-insoluble" means that when 0.5 g of the polymer is dissolved in 100 g of water at a temperature of 25°C, the insoluble component is 90% by mass or more.

[0042] <<Glass transition temperature>>

[0043] The temperature range in which the granular polymer has at least one glass transition temperature needs to be above 30°C and below 95°C, preferably below 75°C, more preferably below 70°C, preferably above 35°C, and more preferably above 45°C. If the temperature range in which the granular polymer has at least one glass transition temperature is above the above lower limit, the anti-adhesion property of the obtained functional layer can be improved, and the internal resistance of the obtained secondary battery can be reduced. If the temperature range in which the granular polymer has at least one glass transition temperature is below the above upper limit, the deformability of the granular polymer during the pressing process when making the secondary battery is improved, the adhesion of the functional layer after the electrolyte is impregnated can be further improved, and the high temperature cycle characteristics of the obtained secondary battery can be improved. In addition, the glass transition temperature of the granular polymer can be adjusted by, for example, changing the type and proportion of the monomers used to prepare the granular polymer.

[0044] When the particulate polymer is a polymer having a core-shell structure as described below, or when a plurality of polymers are used in combination, as described in Examples below, the temperature shown by the peak with a large shift is taken as the glass transition temperature of the polymer.

[0045] <<Core-shell structure>>

[0046] The granular polymer preferably has a core-shell structure. The granular polymer having a core-shell structure has the following core-shell structure: a shell having a core and an outer surface coating the core. By using a granular polymer having a core-shell structure, if the granular polymer has a core-shell structure, the adhesion of the functional layer after electrolyte impregnation can be improved, and the high temperature cycle characteristics of the obtained secondary battery can be further improved. Here, the shell can cover the outer surface of the core as a whole, or it can be partially coated. In addition, even if it looks like the outer surface of the core is completely coated by the shell, as long as a hole connecting the inside and outside of the shell is formed, the shell is also a shell of the outer surface of the core partially coated. Therefore, for example, a granular polymer having a shell and the shell having pores connected from the outer surface of the shell (i.e., the peripheral surface of the granular polymer) to the outer surface of the core belongs to a granular polymer in which the shell partially coats the outer surface of the core.

[0047] In addition, as long as the desired effect is not significantly impaired, the granular polymer may also have any constituent elements other than the above-mentioned core and shell. Specifically, for example, the granular polymer may have a portion formed by a polymer different from the core inside the core. When citing a specific example, the seed particles used when the granular polymer is manufactured by the seed polymerization method may remain inside the core. However, from the viewpoint of significantly exerting the desired effect, the granular polymer preferably only has a core and shell.

[0048] <<Volume average particle size>>

[0049] The volume average particle size of the granular polymer is preferably 0.25 μm or more, more preferably 0.30 μm or more, further preferably 0.40 μm or more, preferably 5.0 μm or less, more preferably 4.0 μm or less, and further preferably 3.0 μm or less. If the volume average particle size of the granular polymer is above the above lower limit, it is presumed that it is easy to ensure that there is a small gap in the functional layer, so the internal resistance of the secondary battery obtained can be reduced. On the other hand, if the volume average particle size of the granular polymer is below the above upper limit, the adhesion of the functional layer after the electrolyte is impregnated can be further improved.

[0050] The volume average particle size of the particulate polymer can be adjusted by, for example, changing the type and ratio of monomers used to prepare the particulate polymer and / or changing the polymerization conditions of the particulate polymer (for example, the amount of emulsifier used).

[0051] <<Composition>>

[0052] The composition of the granular polymer is not particularly limited as long as it has at least one glass transition temperature in a temperature range of 30°C to 95°C. For example, the granular polymer may be a homopolymer formed by repeating units of a single monomer, or a copolymer comprising copolymer units of a plurality of monomers. As a homopolymer, there is no particular limitation, and examples include: polyvinyl acetate, polyvinylidene fluoride, and polymethyl methacrylate. In the case where the granular polymer is a homopolymer, polyvinyl acetate is particularly preferred. In addition, as a copolymer, for example, a copolymer of the composition exemplified below can be cited. Moreover, in the case where the granular polymer is a polymer having the above-mentioned core-shell structure, the composition of the polymer forming the core portion can be the following composition.

[0053] The repeating unit contained in the particulate polymer is not particularly limited, and preferably includes an aromatic monovinyl monomer unit and a crosslinking monomer unit. The particulate polymer may contain only one type of monomer unit (repeating unit) or may contain a plurality of types of monomer units (repeating units).

[0054] -Aromatic monovinyl monomer unit-

[0055] Examples of the aromatic monovinyl monomers that can form the aromatic monovinyl monomer units of the granular polymer include styrene, styrene sulfonic acid and its salts (e.g., sodium styrene sulfonate, etc.), α-methylstyrene, vinyltoluene, 4-(tert-butoxy)styrene, etc. These may be used alone or in combination of a plurality of types. Among these, styrene is preferred.

[0056] Moreover, with all repeating units as 100 mass %, the ratio of the aromatic monovinyl monomer units contained in the granular polymer is preferably more than 20 mass %, more preferably more than 30 mass %, more preferably more than 40 mass %, preferably less than 85 mass %, more preferably less than 75 mass %. If the proportion of the aromatic monovinyl monomer units in the polymer of the core is above the above lower limit, the glass transition temperature of the polymer of the core is improved, and the anti-adhesion property of the battery component with the functional layer can be improved. On the other hand, if the proportion of the aromatic monovinyl monomer units in the polymer of the core is below the above upper limit, the deformability of the granular polymer in the process such as the pressing when making the secondary battery can be fully ensured, so the adhesion of the functional layer after the electrolyte impregnation can be further improved.

[0057] - Cross-linking monomer unit-

[0058] The crosslinkable monomer that can form the crosslinkable monomer unit of the granular polymer is not particularly limited, and examples thereof include monomers that can form a crosslinked structure by polymerization. Examples of crosslinkable monomers generally include monomers having thermal crosslinkability. More specifically, examples thereof include: a crosslinkable monomer having a crosslinkable group having thermal crosslinkability and having one ethylenic double bond per molecule; and a crosslinkable monomer having two or more ethylenic double bonds per molecule.

[0059] Examples of the heat-crosslinkable crosslinkable group include an epoxy group, an N-methylolamide group, an oxetane group, Among these, an epoxy group is more preferred from the viewpoint of easy cross-linking and easy adjustment of cross-linking density.

[0060] Examples of crosslinkable monomers having an epoxy group as a heat-crosslinkable crosslinkable group and having an ethylenic double bond include unsaturated glycidyl ethers such as vinyl glycidyl ether, allyl glycidyl ether, butenyl glycidyl ether, and o-allylphenyl glycidyl ether; monoepoxy of dienes or polyenes such as butadiene monoepoxide, chloroprene monoepoxide, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexene, and 1,2-epoxy-5,9-cyclododecadiene; substances; alkenyl epoxides such as 3,4-epoxy-1-butene, 1,2-epoxy-5-hexene, and 1,2-epoxy-9-decene; and glycidyl esters of unsaturated carboxylic acids such as glycidyl acrylate, glycidyl methacrylate, glycidyl crotonate, glycidyl 4-heptenoate, glycidyl sorbate, glycidyl linoleate, glycidyl 4-methyl-3-pentenoate, glycidyl ester of 3-cyclohexenecarboxylic acid, and glycidyl ester of 4-methyl-3-cyclohexenecarboxylic acid.

[0061] In addition, as an example of a crosslinkable monomer having an N-hydroxymethylamide group as a heat-crosslinkable crosslinkable group and having an ethylenic double bond, there can be mentioned (meth)acrylamides having a hydroxymethyl group such as N-hydroxymethyl (meth)acrylamide. In addition, in this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid.

[0062] Furthermore, examples of crosslinkable monomers having an oxetane group as a heat-crosslinkable crosslinkable group and having an olefinic double bond include: 3-((meth)acryloyloxymethyl)oxetane, 3-((meth)acryloyloxymethyl)-2-trifluoromethyloxetane, 3-((meth)acryloyloxymethyl)-2-phenyloxetane, 2-((meth)acryloyloxymethyl)oxetane, and 2-((meth)acryloyloxymethyl)-4-trifluoromethyloxetane. In addition, in the present specification, "(meth)acryloyl" refers to acryloyl and / or methacryloyl.

[0063] In addition, as a Examples of crosslinkable monomers having a thermally crosslinkable crosslinkable group and an ethylenic double bond include: 2-vinyl-2-oxazoline group. Oxazoline, 2-vinyl-4-methyl-2- Oxazoline, 2-vinyl-5-methyl-2- Oxazoline, 2-isopropenyl-2- Oxazoline, 2-isopropenyl-4-methyl-2- Oxazoline, 2-isopropenyl-5-methyl-2- Oxazoline and 2-isopropenyl-5-ethyl-2- Oxazoline.

[0064] Furthermore, examples of crosslinking monomers having two or more ethylenic double bonds per molecule include allyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipropylene glycol diallyl ether, polyglycol diallyl ether, triethylene glycol divinyl ether, hydroquinone diallyl ether, tetraallyloxyethane, trimethylolpropane diallyl ether, allyl or vinyl ethers of polyfunctional alcohols other than those mentioned above, triallylamine, methylenebisacrylamide and divinylbenzene.

[0065] In addition, in the present invention, "(meth)acrylate" means acrylate and / or methacrylate.

[0066] The crosslinking monomer may be used alone or in combination of two or more. Among these, a crosslinking monomer having two or more ethylenic double bonds per molecule is preferred, ethylene glycol dimethacrylate and allyl methacrylate are more preferred, and ethylene glycol dimethacrylate is further preferred.

[0067] Moreover, with all repeating units as 100 mass %, the proportion of the crosslinking monomer units contained in the granular polymer is preferably 0.05 mass % or more, more preferably 0.1 mass % or more, preferably 15.0 mass % or less, more preferably 13.0 mass % or less. If the proportion of the crosslinking monomer units in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte immersion and the rate characteristics and high temperature cycle characteristics of the secondary battery can be improved.

[0068] -Other monomer units-

[0069] The monomer units (other monomer units) other than the aromatic monovinyl monomer unit and the crosslinking monomer unit that may be contained in the particulate polymer are not particularly limited, and examples thereof include acidic group-containing monomer units, (meth)acrylic acid ester monomer units, and nitrile group-containing monomer units.

[0070] -Acidic group-containing monomer unit

[0071] As the acidic group-containing monomers that can form the acidic group-containing monomer units of the granular polymer, carboxylic acid group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, etc. can be enumerated. These can be used alone or in combination. In addition, the acid group of the acidic group-containing monomer unit can also form salts with alkali metals, ammonia, etc.

[0072] Examples of the carboxylic acid group-containing monomer include ethylenically unsaturated monocarboxylic acids and derivatives thereof, ethylenically unsaturated dicarboxylic acids and anhydrides thereof, and derivatives thereof.

[0073] Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, crotonic acid, etc. Examples of derivatives of ethylenically unsaturated monocarboxylic acids include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, β-diaminoacrylic acid, etc.

[0074] Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, itaconic acid, mesaconic acid, etc. Moreover, examples of anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, acrylic anhydride, methyl maleic anhydride, dimethyl maleic anhydride, etc. Furthermore, examples of derivatives of ethylenically unsaturated dicarboxylic acids include methyl maleic acid, dimethyl maleic acid, phenyl maleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, fluoroalkyl maleate, etc.

[0075] Examples of the sulfonic acid group-containing monomer include vinyl sulfonic acid, methylvinyl sulfonic acid, (meth)allyl sulfonic acid, ethyl (meth)acrylate-2-sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid.

[0076] In the present invention, "(meth)allyl" means allyl and / or methallyl, and "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.

[0077] Examples of the phosphoric acid group-containing monomer include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate.

[0078] Among these, as the acidic group-containing monomer, a carboxylic acid group-containing monomer is preferred, acrylic acid, methacrylic acid, and itaconic acid are more preferred, and methacrylic acid is further preferred.

[0079] With all repeating units as 100 mass %, the ratio of the acidic group-containing monomeric unit that can be arbitrarily included in the granular polymer can be more than 1.0 mass %, can also be more than 1.5 mass %, is preferably below 7.0 mass %, more preferably below 6.0 mass %, further preferably below 5.0 mass %. If the shared ratio of the acidic group-containing monomeric unit in the granular polymer is more than the above-mentioned lower limit, the adhesion of the functional layer obtained in the electrolyte can be improved. On the other hand, if the shared ratio of the acidic group-containing monomeric unit in the granular polymer is below the above-mentioned upper limit, the high temperature cycle characteristics of the secondary battery can be further improved.

[0080] -(Meth)acrylate monomer unit-

[0081] Examples of the (meth)acrylate monomers that can form the (meth)acrylate monomer units of the particulate polymer include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate; and alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and glycidyl methacrylate. These may be used alone or in combination of two or more. Among these, 2-ethylhexyl acrylate, n-butyl acrylate, and ethyl acrylate are preferred, and 2-ethylhexyl acrylate is more preferred.

[0082] Moreover, taking all repeating units as 100 mass %, the proportion of (meth)acrylate monomer units arbitrarily contained in the granular polymer is preferably 20 mass % or more, preferably 50 mass % or less, and more preferably 40 mass % or less. If the proportion of (meth)acrylate monomer units in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte immersion and the rate characteristics and high temperature cycle characteristics of the secondary battery can be improved.

[0083] -Nitrile-containing monomer unit-

[0084] As the nitrile-containing monomers capable of forming nitrile-containing monomer units of the granular polymer, α, β-ethylenically unsaturated nitrile monomers can be cited. Specifically, as α, β-ethylenically unsaturated nitrile monomers, there are no particular limitations as long as they are α, β-ethylenically unsaturated compounds having nitrile groups, and examples thereof include: acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile and α-ethylacrylonitrile, etc. These can be used alone or in combination of multiple types. Moreover, among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred.

[0085] Moreover, taking all repeating units as 100 mass %, the proportion of nitrile-containing monomer units arbitrarily contained in the granular polymer can be 1 mass % or more, can also be 5 mass % or more, is preferably 20 mass % or less, and more preferably 15 mass % or less. If the proportion of nitrile-containing monomer units in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte impregnation and the rate characteristics and high temperature cycle characteristics of the secondary battery can be improved.

[0086] Here, as described above, when the particulate polymer is a core-shell polymer having a core-shell structure, the polymer forming the core portion is preferably as described above, and the polymer forming the shell portion is preferably as described below.

[0087] [Shell]

[0088] In the case where the particulate polymer is a core-shell polymer having a core-shell structure, the repeating units contained in the polymer forming the shell portion are not particularly limited, and preferably aromatic monovinyl monomer units and acidic group-containing monomer units can be cited. In addition, the polymer in the shell portion can contain only one monomer unit (repeating unit) or multiple monomer units (repeating units).

[0089] -Aromatic monovinyl monomer unit-

[0090] As the aromatic monovinyl monomers of the aromatic monovinyl monomer units of the polymer capable of forming the shell portion, the same monomers as those mentioned above can be cited. These can be used alone or in combination of a plurality of types. Among these, styrene is preferred.

[0091] Moreover, with all repeating units contained in the granular polymer (that is, the total of the polymer of the core portion and the polymer of the shell portion) as 100 mass%, the ratio of the aromatic monovinyl monomer unit contained in the polymer of the shell portion is preferably more than 10 mass%, more preferably more than 20 mass%. If the proportion of the aromatic monovinyl monomer unit of the shell portion in the granular polymer is more than 10 mass%, then in the granular polymer with a core-shell structure, the glass transition temperature of the polymer of the shell portion is improved, and the anti-adhesion property of the battery component with a functional layer can be improved. In addition, the upper limit of the proportion of the aromatic monovinyl monomer unit of the shell portion in the granular polymer is preferably less than 40 mass%, more preferably less than 30 mass%.

[0092] -Acidic group-containing monomer unit

[0093] As the acidic group-containing monomers of the acidic group-containing monomer units of the polymer capable of forming the shell portion, the same monomers as those described in the "core portion" can be cited. These can be used alone or in combination of multiple types. Moreover, among these, carboxylic acid group-containing monomers are preferred, acrylic acid, methacrylic acid, itaconic acid are more preferred, and methacrylic acid is further preferred.

[0094] And, with the whole repeating units comprised in granular polymer (that is, the total of the polymer of core portion and the polymer of shell portion) as 100 mass %, the ratio of the acidic group-containing monomeric unit comprised in the polymer of shell portion is preferably more than 0.01 mass %, more preferably more than 0.1 mass %, preferably below 1.0 mass %, more preferably below 0.6 mass %.If the ratio shared by the acidic group-containing monomeric unit of shell portion in granular polymer is more than the above-mentioned lower limit, then the adhesion of the functional layer in the electrolyte can be improved.On the other hand, if the ratio shared by the acidic group-containing monomeric unit of shell portion in granular polymer is below the above-mentioned upper limit, then the high temperature cycle characteristics of secondary battery can be further improved.

[0095] -Other monomer units-

[0096] The monomer units (other monomer units) that can be included in the monomer units other than the aromatic monovinyl monomer units and the acidic group-containing monomer units as the polymer forming the shell portion are not particularly limited, and examples thereof include the crosslinking monomer units, (meth) acrylate monomer units, and nitrile-containing monomer units. Moreover, among these, the polymer of the shell portion preferably includes nitrile-containing monomer units.

[0097] As the nitrile-containing monomers of the nitrile-containing monomer units of the polymer capable of forming the shell portion, the same monomers as those mentioned above can be cited. These can be used alone or in combination of a plurality of types. And, among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred.

[0098] Moreover, with all repeating units contained in the granular polymer (i.e., the total of the polymer of the core portion and the polymer of the shell portion) as 100 mass%, the proportion of the nitrile-containing monomeric unit contained in the polymer of the shell portion is preferably 0.5 mass% or more, more preferably 1.0 mass% or more, preferably 10.0 mass% or less, more preferably 5.0 mass% or less. If the proportion of the nitrile-containing monomeric unit in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte impregnation and the rate characteristics and high temperature cycle characteristics of the secondary battery can be further improved.

[0099] <<Preparation method>>

[0100] Moreover, the preparation method of the granular polymer is not particularly limited, and can be a method performed according to conventional methods such as emulsion polymerization. For example, in the case where the granular polymer is a core-shell polymer having a core-shell structure, it can be prepared, for example, in the following manner: using monomers of the polymer of the core portion and monomers of the polymer of the shell portion, the ratio of their monomers is changed over time to perform stage-by-stage polymerization. Specifically, the granular polymer with a core-shell structure can be prepared by a continuous multi-stage emulsion polymerization method and a multi-stage suspension polymerization method such that the polymer in the later stage is sequentially coated on the polymer in the previous stage (for example, with reference to International Publication No. 2020 / 175025).

[0101] <Adhesive material A>

[0102] The slurry composition of the present invention contains a binder material A containing at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group. The binder material A can be a saponified product. Moreover, in the heat-resistant layer formed using the slurry composition, the binder material A is a component that can function as a binder material, can impart bonding ability to the functional layer formed using the slurry composition, and can keep the components other than the binder material A, such as the heat-resistant particles contained in the functional layer, from detaching from the functional layer.

[0103] Here, the binder material A is not particularly limited as long as it contains at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group, and may contain any functional group other than these.

[0104] <<Acidic functional group>>

[0105] Examples of the acidic functional group that can be contained in the adhesive material A include ethylenically unsaturated carboxylic acid groups, carboxylic acid groups, sulfonic acid groups, phosphoric acid groups, etc. Among them, from the viewpoint of improving the adhesion of the obtained functional layer, the acidic functional group is preferably an ethylenically unsaturated carboxylic acid group such as an acrylic acid group, a methacrylic acid group, and a crotonic acid group.

[0106] <<Alkali metal salt group>>

[0107] Examples of alkali metals constituting the alkali metal salt group include lithium, sodium, potassium, rubidium, cesium, and francium, among which lithium and sodium are preferred. The alkali metal salt group in the binder material A can be derived from an alkali metal compound. The alkali metal compound is not particularly limited, and examples thereof include hydroxides of the above-mentioned alkali metals.

[0108] <<Polymer composition>>

[0109] Here, the polymer composition of the adhesive material A is not particularly limited as long as it contains the above-mentioned functional groups and alkali metal salt groups. The adhesive material A can contain any monomer unit as a repeating unit. In addition, in this specification, "containing a monomer unit" means "a repeating unit derived from a monomer is contained in a polymer obtained by using the monomer".

[0110] For example, as a monomer that can be used to introduce a hydroxyl group into the adhesive material A, a vinyl ester monomer can be cited. By saponifying the vinyl ester monomer unit formed using the vinyl ester monomer, a hydroxyl group can be introduced into the adhesive material A. As the vinyl ester monomer, vinyl acetate, vinyl pivalate, vinyl formate, vinyl propionate, vinyl butyrate, vinyl n-hexanoate, vinyl isocaproate, vinyl octanoate, vinyl laurate, vinyl palmitate, vinyl stearate, trimethylacetic acid vinyl, vinyl chloroacetate, vinyl trichloroacetate, vinyl trifluoroacetate, vinyl benzoate, etc. can be cited. These can be used alone or in combination of two or more. Among them, as the vinyl ester monomer, vinyl acetate is preferably used.

[0111] Taking all repeating units constituting the adhesive material A as 100 mass %, the proportion of monomer units derived from vinyl ester monomers in the adhesive material A is preferably 5 mass % or more, more preferably 20 mass % or more, further preferably 50 mass % or more, preferably 95 mass % or less, more preferably 90 mass % or less. If the proportion of monomer units derived from vinyl ester monomers is within the above range, the adhesion of the obtained functional layer can be further improved, and the high temperature cycle characteristics and electrolyte injection properties of the obtained secondary battery can be further improved.

[0112] Furthermore, examples of monomers that can be used to introduce an acidic functional group into the adhesive material A include ethylenically unsaturated carboxylic acid ester monomers. Examples of ethylenically unsaturated carboxylic acid ester monomers include (meth)acrylic acid ester monomers and crotonate monomers. Among them, examples of the (meth)acrylate monomers that can be preferably used include: alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and glycidyl methacrylate. These may be used alone or in combination of two or more. Among these, methyl acrylate and methyl methacrylate are preferred.

[0113] Taking all repeating units constituting the adhesive material A as 100 mass %, the proportion of monomer units derived from ethylenically unsaturated carboxylic acid ester monomers in the adhesive material A is preferably 5 mass % or more, more preferably 10 mass % or more, preferably 95 mass % or less, more preferably 80 mass % or less, and further preferably 50 mass parts or less. If the proportion of monomer units derived from ethylenically unsaturated carboxylic acid ester monomers is within the above range, the adhesion of the obtained functional layer can be further improved, and the high temperature cycle characteristics and electrolyte injection properties of the obtained secondary battery can be further improved.

[0114] Here, the copolymer of vinyl alcohol and alkali metal neutralized product of olefinic unsaturated carboxylic acid is preferred as the binder material A. If the binder material A is a copolymer of vinyl alcohol and alkali metal neutralized product of olefinic unsaturated carboxylic acid, the adhesion of the obtained functional layer in the electrolyte can be further improved, and the high temperature cycle characteristics of the obtained secondary battery can be further improved.

[0115] The copolymer of vinyl alcohol and alkali metal neutralized product of olefinic unsaturated carboxylic acid as the bonding material A can be manufactured in the following manner: in the presence of alkali metal compounds such as alkali metal hydroxides and a reducing agent, the copolymer of the above-mentioned vinyl ester and olefinic unsaturated carboxylic acid ester monomer is saponified. In more detail, by saponifying the vinyl ester, the unit containing a hydroxyl group, i.e., the vinyl alcohol unit, can be introduced into the copolymer. In addition, the olefinic unsaturated carboxylic acid group of the olefinic unsaturated carboxylic acid ester unit constituting the copolymer forms a salt with an alkali metal, and an alkali metal salt of the olefinic unsaturated carboxylic acid group can be formed. In this way, the bonding material A as a copolymer of vinyl alcohol and alkali metal neutralized product of olefinic unsaturated carboxylic acid can be efficiently manufactured.

[0116] <<Other repeating units>>

[0117] In addition to the above-mentioned repeating units, the adhesive material A may also contain other repeating units. The other repeating units are not particularly limited, and examples thereof include monomer units derived from known monomers such as the crosslinking monomer unit described in the "granular polymer". In addition, the adhesive material A may contain one other repeating unit, or may contain two or more other repeating units at any ratio.

[0118] Moreover, when all repeating units (all monomer units) contained in the adhesive material A are set to 100 mass%, the content ratio of other repeating units is preferably 10 mass% or less, more preferably 5 mass% or less, further preferably 1 mass% or less, and particularly preferably 0 mass%.

[0119] <Yellowness index of adhesive material A>

[0120] The yellow index of polymer A is preferably less than 14.0, more preferably less than 11.0, and further preferably less than 10.0. In addition, the lower limit of the yellow index of polymer A is not particularly limited, for example, it can be 0. If the yellow index of polymer A is below the above upper limit, the adhesion of the obtained functional layer in the electrolyte can be further improved, and the high temperature cycle characteristics of the obtained secondary battery can be further improved. In addition, the yellow index of the polymer can be controlled by adjusting the manufacturing conditions when manufacturing the bonding material. Specifically, the yellow index can be suppressed by adding a reducing agent during manufacturing. In addition, the yellow index can be changed according to the type of reducing agent and alkali metal compound used.

[0121] <Amount of adhesive material A>

[0122] The amount of the binder material A in the slurry composition is preferably 0.1 parts by mass or more relative to 100 parts by mass of the granular polymer, more preferably 0.5 parts by mass or more, more preferably 1.5% by mass or more, preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and more preferably 5.0 parts by mass or less. If the amount of the binder material A is above the lower limit, the electrolyte injection and high temperature cycle characteristics of the obtained secondary battery can be further improved. In addition, if the amount of the binder material A is below the upper limit, the anti-blocking property of the obtained functional layer can be further improved.

[0123] <Adhesive material B>

[0124] In addition to the above-mentioned granular polymer and binder A, the slurry composition of the present invention preferably further comprises a polymer different from these polymers, namely, a binder B. As the binder B, there is no particular limitation as long as it can exert the bonding ability for maintaining the granular polymer and other components in the functional layer and / or the bonding ability between the functional layer and the adherend, and any polymer can be used. Among them, as the binder B, a polymer having a glass transition temperature of less than 20°C is preferred. In addition, the binder B is preferably water-insoluble.

[0125] <<Glass transition temperature>>

[0126] The glass transition temperature of the adhesive material B is preferably less than 20°C, preferably less than 15°C, more preferably less than 12°C, preferably above -40°C, more preferably above -20°C, and further preferably above -10°C. If a slurry composition containing an adhesive material B having a glass transition temperature less than the above upper limit value in addition to the above-mentioned particulate polymer is used, the adhesion of the functional layer after electrolyte impregnation can be improved, and the rate characteristics of the secondary battery can be further improved. On the other hand, if the glass transition temperature of the adhesive material B is above the above lower limit value, the anti-blocking property of the obtained functional layer can be improved.

[0127] In addition, the glass transition temperature of the adhesive material B can be adjusted by, for example, changing the type and ratio of monomers used to prepare the adhesive material B.

[0128] <<Composition>>

[0129] The composition of the adhesive material B is not particularly limited. For example, the adhesive material B may be an aromatic vinyl polymer in which the content ratio of the aromatic monovinyl monomer unit is 50% by mass or more of the total repeating units, or may be an acrylic polymer in which the content ratio of the (meth)acrylate monomer unit is 50% by mass or more of the total repeating units. As other monomer units other than the aromatic monovinyl monomer unit that can constitute the aromatic vinyl polymer, there is no particular limitation, and examples thereof include aliphatic conjugated diene monomer units from 1,3-butadiene, etc., hydroxyl-containing monomer units from 2-hydroxyethyl acrylate, etc., and acidic group-containing monomer units from itaconic acid, etc. In addition, as other monomer units other than the (meth)acrylate monomer unit that can constitute the acrylic polymer, there is no particular limitation, and examples thereof include acidic group-containing monomer units from (meth)acrylic acid, etc., and nitrile-containing monomer units from acrylonitrile, etc.

[0130] The polymerization method of the binder material B is carried out according to a conventional method and is not particularly limited. In addition, as the binder material B, a commercially available binder material can also be used.

[0131] <<Amount>>

[0132] The amount of the binder B mixed in the slurry composition of the present invention is not particularly limited, and is preferably 1 part by mass or more, more preferably 2 parts by mass or more, preferably 50 parts by mass or less, and more preferably 40 parts by mass or less relative to 100 parts by mass of the granular polymer. If the amount of the binder B mixed relative to 100 parts by mass of the granular polymer is greater than the above lower limit, the adhesion of the functional layer after the electrolyte is further improved, and if it is less than the above upper limit, the anti-blocking property of the battery component having the functional layer can be ensured.

[0133] <Solvent>

[0134] As the solvent contained in the slurry composition of the present invention, a known solvent that can be used as at least a dispersion medium of the above-mentioned particulate polymer can be used. Among them, water is preferably used as the solvent. In addition, at least a part of the solvent of the slurry composition can be a polymerization solvent used in the preparation of the particulate polymer, etc., without particular limitation.

[0135] <Other ingredients>

[0136] The slurry composition of the present invention may further include any other components in addition to the above-mentioned components. Other components are not particularly limited as long as they do not affect the battery reaction, and known components can be used. In addition, these other components may be used alone or in combination of two or more.

[0137] Furthermore, examples of other components include heat-resistant particles, wetting agents (polyethylene oxide, polypropylene oxide, etc.), and water-soluble polymers (carboxymethylcellulose and its salts, polyvinyl alcohol, etc.).

[0138] The heat-resistant particles to be blended in the slurry composition are not particularly limited, and examples thereof include known heat-resistant particles used in non-aqueous secondary batteries.

[0139] Specifically, as heat-resistant particles, inorganic particles and organic particles other than the above-mentioned granular polymer and bonding material B can be used, and inorganic particles are generally used. Among them, as the material of the heat-resistant particles, it is preferred that the material is stably present and electrochemically stable under the use environment of the non-aqueous secondary battery. When the preferred examples of the material of the heat-resistant particles are given from this point of view, oxide particles such as aluminum oxide (alumina), hydrated aluminum oxide (boehmite), silicon oxide, magnesium oxide (magnesia), calcium oxide, titanium oxide (Titania), BaTiO3, ZrO, aluminum oxide-silicon dioxide composite oxides, etc.; nitride particles such as aluminum nitride and boron nitride; covalently bonded crystalline particles such as silicon and diamond; insoluble ionic crystalline particles such as barium sulfate, calcium fluoride, and barium fluoride; clay particles such as talc and montmorillonite, etc. In addition, these particles can be subjected to element replacement, surface treatment, solid solution, etc. as needed.

[0140] When organic fine particles are used as heat-resistant particles, the glass transition temperature and / or melting point of the organic fine particles is usually higher than 150°C, preferably higher than 180°C, and more preferably higher than 200°C.

[0141] The above-mentioned heat-resistant particles may be used alone or in combination of two or more.

[0142] Here, the amount of the heat-resistant particles contained in the slurry composition is not particularly limited, but is preferably 200 parts by mass or more and 1500 parts by mass or less relative to 100 parts by mass of the particulate polymer.

[0143] (Method for producing slurry composition for non-aqueous secondary battery functional layer)

[0144] The method for manufacturing a slurry composition for a non-aqueous secondary battery functional layer of the present invention includes the following steps: polymerizing a monomer composition comprising at least one of a vinyl ester monomer and an ethylenically unsaturated carboxylic acid ester monomer to obtain a polymer, and then, in the presence of an alkali metal compound and a reducing agent, saponifying the polymer to obtain a saponified polymer as a binder material A (binder material manufacturing step). According to the manufacturing method of the present invention, the slurry composition for a non-aqueous secondary battery functional layer of the present invention can be efficiently manufactured. Furthermore, the manufacturing method of the present invention can also include a mixing step of mixing the binder material A manufactured in the binder material manufacturing step with other components.

[0145] <Adhesive material manufacturing process>

[0146] The method for preparing the polymer in the adhesive material production step is not particularly limited, and can be carried out according to a known method such as a suspension polymerization method (for example, refer to International Publication No. 2017 / 168947).

[0147] Moreover, in the adhesive material manufacturing process, in the presence of an alkali metal compound and a reducing agent, a polymer containing repeating units from at least one of a vinyl ester monomer and an ethylenically unsaturated carboxylic acid ester monomer is saponified to obtain a saponified product of a polymer as an adhesive material A. Here, as an alkali metal compound, the above-mentioned alkali metal hydroxide can be preferably used. In addition, the saponification of the polymer can also be carried out according to a known method (for example, with reference to International Publication No. 2017 / 168947). In addition, as a reducing agent, reducing agents such as ascorbic acid, sodium thiosulfate, and hydrazine can be cited. Among them, since there are few impurities and the adhesive material can show good adhesion, ascorbic acid and sodium thiosulfate are preferably used as reducing agents.

[0148] <Mixing process>

[0149] Furthermore, the manufacturing method of the present invention can also include a mixing step: after the above-mentioned adhesive material manufacturing step, the granular polymer, adhesive material A and solvent are mixed with the adhesive material B and / or other components used as needed. In addition, as the granular polymer, solvent and other arbitrary components, the above-mentioned granular polymer, solvent and other components can be preferably used. The mixing method of the mixing step is not particularly limited. In order to disperse each component efficiently, a disperser is usually used as a mixing device for mixing. The disperser is preferably a device that can uniformly disperse and mix the above-mentioned components. For example, a ball mill, a sand mill, a pigment disperser, a grinder, an ultrasonic disperser, a homogenizer, a planetary mixer, etc. can be cited. In addition, from the viewpoint of being able to apply a high dispersion shear force, it is preferred to use a high dispersion device such as a bead mill, a roller mill, and Filmix.

[0150] (Functional layer)

[0151] The non-aqueous secondary battery functional layer slurry composition of the present invention can be used to form a functional layer on a suitable substrate. Specifically, by drying the slurry composition on a suitable substrate, a functional layer can be formed. That is, the functional layer is formed by the dried product of the above-mentioned slurry composition, usually containing the above-mentioned granular polymer and bonding material A, and arbitrarily containing the above-mentioned bonding material B and / or other components. In addition, in the case where the above-mentioned granular polymer, bonding material A and / or bonding material B include crosslinking monomer units, the granular polymer, bonding material A and / or bonding material B can be crosslinked in the drying of the slurry composition or in the heat treatment process arbitrarily implemented after drying (that is, the functional layer can include the crosslinked product of the above-mentioned granular polymer, bonding material A and / or bonding material B). In addition, the preferred existence ratio of each component contained in the functional layer is the same as the preferred existence ratio of each component in the slurry composition for non-aqueous secondary battery functional layer of the present invention.

[0152] Furthermore, the functional layer formed using the slurry composition of the present invention has excellent anti-blocking properties, and further, excellent electrolyte injection properties and adhesiveness. Therefore, if a battery component having the functional layer is used, a secondary battery with excellent electrolyte injection properties and high temperature cycle characteristics can be manufactured.

[0153] <Base material>

[0154] As a substrate for applying a slurry composition to form a functional layer thereon, there is no particular limitation. For example, in the case of using a functional layer as a component constituting a part of a spacer, a spacer substrate can be used as a substrate, and in the case of using a functional layer as a component constituting a part of an electrode, an electrode substrate formed by forming an electrode composite material layer on a current collector can be used as a substrate. In addition, the usage of the functional layer formed on the substrate is not particularly limited, for example, a functional layer can be formed on a spacer substrate, etc. and used directly as a battery component such as a spacer, a functional layer can also be formed on an electrode substrate and used as an electrode, and the functional layer formed on a release substrate can also be temporarily peeled off from the substrate and pasted on other substrates as a battery component.

[0155] However, from the viewpoint of omitting the step of peeling the release substrate from the functional layer and improving the production efficiency of the battery member, it is preferable to use a separator substrate or an electrode substrate as the substrate.

[0156] <<Spacer base material>>

[0157] As the separator substrate, there is no particular limitation, and for example, the separator substrate described in Japanese Patent Publication No. 2012-204303 can be used. Among these, from the aspect of being able to make the overall film thickness of the separator thinner, thereby being able to increase the ratio of the electrode active material in the secondary battery and increasing the capacity per unit volume, a microporous membrane formed of a polyolefin resin (polyethylene, polypropylene, polybutylene, polyvinyl chloride) is preferred.

[0158] In addition, the spacer substrate may include in a part thereof any layer capable of exerting a desired function except for the functional layer formed by the slurry composition of the present invention. For example, the spacer substrate may include in a part thereof a porous film layer containing heat-resistant particles and a bonding material but not containing at least one of the above-mentioned granular polymer and bonding material A, more specifically, the spacer substrate may have a porous film layer containing heat-resistant particles and bonding materials on one or both sides of a microporous film formed by the above-mentioned polyolefin resin. In addition, as "heat-resistant particles" in the porous film layer, heat-resistant particles exemplified in the "slurry composition for non-aqueous secondary battery functional layer" item can be used. In addition, as "bonding materials" in the porous film layer, bonding materials exemplified as "bonding material B" in the "slurry composition for non-aqueous secondary battery functional layer" item, known bonding materials can be used.

[0159] <<Electrode base material>>

[0160] The electrode substrate (positive electrode substrate and negative electrode substrate) is not particularly limited, and examples thereof include an electrode substrate in which an electrode composite material layer is formed on a current collector.

[0161] Here, the components in the current collector, the electrode composite material layer (for example, electrode active materials (positive electrode active materials, negative electrode active materials) and binding materials for electrode composite material layers (binding materials for positive electrode composite material layers, binding materials for negative electrode composite material layers)), and the method for forming an electrode composite material layer on the current collector can use known ones, for example, those described in Japanese Patent Gazette No. 2013-145763 can be used.

[0162] Furthermore, the electrode substrate may contain, in part, any layer having a desired function other than the functional layer formed from the slurry composition of the present invention (eg, the porous film layer containing heat-resistant particles and a binder as described in the section "separator substrate").

[0163] <<Release substrate>>

[0164] The release substrate is not particularly limited, and a known release substrate can be used.

[0165] <Method for forming functional layer>

[0166] As a method for forming a functional layer on the above-mentioned substrate such as the separator substrate and the electrode substrate, the following methods can be mentioned:

[0167] 1) A method of applying the slurry composition to the surface of a separator substrate or an electrode substrate (in the case of an electrode substrate, the surface on the electrode composite material layer side, the same below), followed by drying;

[0168] 2) A method of dipping a separator substrate or an electrode substrate into a slurry composition and then drying it;

[0169] 3) A method in which the slurry composition is applied onto a release substrate, dried to produce a functional layer, and the obtained functional layer is transferred to the surface of a separator substrate or an electrode substrate.

[0170] Among these, the method 1) is particularly preferred because it is easy to control the film thickness of the functional layer. In detail, the method 1) comprises: a step of applying the slurry composition to a separator substrate or an electrode substrate (coating step); and a step of drying the functional layer composition applied to the separator substrate or the electrode substrate to form a functional layer (drying step).

[0171] In the coating step, the method for coating the slurry composition on the separator substrate or the electrode substrate is not particularly limited, and examples thereof include spray coating, doctor blade coating, reverse roll coating, direct roll coating, gravure printing, extrusion, and brush coating.

[0172] In the drying step, the method for drying the slurry composition on the substrate is not particularly limited, and a known method can be used, for example, drying using warm air, hot air, or low-humidity air; vacuum drying; and drying using irradiation of infrared rays, electron beams, etc. The drying conditions are not particularly limited, but the drying temperature is preferably 30 to 80° C., and the drying time is preferably 30 seconds to 10 minutes.

[0173] The thickness of the functional layer formed on the substrate is preferably 0.1 μm or more, more preferably 0.3 μm or more, further preferably 0.5 μm or more, and is preferably 3.0 μm or less, more preferably 1.5 μm or less, further preferably 1.0 μm or less.

[0174] Here, the shape of the functional layer formed on the substrate is not particularly limited, and can be formed into any top view shape such as stripe, dot, grid, etc. Here, when the adhesive layer is formed in a dot shape, the resistance of the secondary battery can be reduced. The dot-shaped functional layer can be obtained by, for example, using a coating machine to implement an inkjet method.

[0175] In addition, the diameter of the dots of the functional layer arranged in a dot pattern is preferably 10 μm or more, more preferably 20 μm or more, preferably 300 μm or less, and more preferably 200 μm or less. If the diameter of the dots of the functional layer is above the lower limit, the adhesion between the electrode and the separator can be improved. On the other hand, if the diameter of the dots of the functional layer is below the upper limit, the output characteristics of the secondary battery can be suppressed from decreasing.

[0176] The thickness of the dots of the functional layer arranged in a dot pattern is preferably 5 μm or more. When the thickness of the dots of the functional layer is equal to or greater than the above lower limit, the adhesive force between the electrode and the separator can be increased.

[0177] (Separator for non-aqueous secondary battery)

[0178] The spacer of the present invention has a spacer substrate and a functional layer formed from the slurry composition of the present invention on at least one surface of the spacer substrate. In addition, the spacer substrate and the functional layer constituting the spacer are the same as those described in the item "functional layer".

[0179] Moreover, the separator of the present invention has a functional layer formed using the slurry composition of the present invention, so it has excellent anti-blocking properties before being impregnated with the electrolyte, and after being impregnated with the electrolyte, it can be well bonded to other adjacent battery components (such as electrodes) through the functional layer. In addition, the separator of the present invention can improve the electrolyte injection property of the secondary battery and enable the secondary battery to exert excellent high-temperature cycle characteristics.

[0180] (Non-aqueous secondary battery)

[0181] The nonaqueous secondary battery of the present invention has the above-mentioned separator for the nonaqueous secondary battery of the present invention. More specifically, the nonaqueous secondary battery of the present invention has a positive electrode, a negative electrode, a separator and an electrolyte, and the above-mentioned separator is the separator for the nonaqueous secondary battery of the present invention having a separator substrate and a functional layer.

[0182] Since the nonaqueous secondary battery of the present invention includes the separator for a nonaqueous secondary battery of the present invention, it is excellent in electrolyte injection properties and high-temperature cycle characteristics.

[0183] <Positive and negative electrodes>

[0184] In the secondary battery of the present invention, at least the separator has a functional layer, and the positive electrode and the negative electrode may also have functional layers respectively. As the positive electrode and the negative electrode having the functional layer, an electrode having a functional layer provided on an electrode substrate can be used, and the electrode substrate is formed by forming an electrode composite material layer on a current collector. In addition, as the electrode substrate and the separator substrate, the same electrode substrate and the separator substrate as those listed in the "functional layer" item can be used.

[0185] The positive electrode and the negative electrode having no functional layer are not particularly limited, and electrodes formed of the above-mentioned electrode substrates can be used.

[0186] <Electrolyte>

[0187] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can generally be used. As a supporting electrolyte, a lithium salt can be used in, for example, a lithium ion secondary battery. As a lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, LiPF6, LiClO4, CF3SO3Li are preferred because they are easily soluble in solvents and show a high degree of dissociation. In addition, the electrolyte can be used alone or in combination of two or more. Generally, there is a tendency that the higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.

[0188] As an organic solvent used in the electrolyte, there is no particular limitation as long as it can dissolve the supporting electrolyte. For example, in lithium-ion secondary batteries, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and methyl ethyl carbonate (MEC) can be preferably used; esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, carbonates are preferred because of their high dielectric constant and wide stable potential region. Generally, there is a tendency that the lower the viscosity of the solvent used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of solvent.

[0189] In addition, the concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. In addition, a known additive can be added to the electrolytic solution.

[0190] <Method for producing non-aqueous secondary battery>

[0191] The secondary battery can be manufactured by, for example, the following method: overlapping the positive electrode and the negative electrode through the non-aqueous secondary battery separator of the present invention, winding, folding, etc. as needed, placing them in a battery container, injecting an electrolyte into the battery container, and sealing. Here, a porous metal mesh, a fuse, an overcurrent protection element such as a PTC element, a guide plate, etc. can be placed in the battery container as needed to prevent the pressure inside the battery from rising and overcharging and discharging. The shape of the battery can be any shape such as a coin shape, a button shape, a sheet shape, a cylindrical shape, a square shape, a flat shape, etc.

[0192] Example

[0193] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.

[0194] In a polymer produced by copolymerizing a plurality of monomers, the ratio of a monomer unit formed by polymerizing a certain monomer in the polymer is usually the same as the ratio (feed ratio) of the certain monomer in all monomers used to polymerize the polymer unless otherwise specified.

[0195] In addition, in Examples and Comparative Examples, various properties were measured and evaluated according to the following methods.

[0196] <Glass transition temperature>

[0197] The aqueous dispersion of the polymer to be measured (particulate polymer, binder B) was dried at 25° C. for 48 hours to obtain a powdery measurement sample.

[0198] 10 mg of the sample was weighed in an aluminum pan, and the differential thermal analysis measuring device (manufactured by Seiko Nanotech Co., Ltd., product name "EXSTAR DSC6220") was used to measure the temperature range of -100°C to 200°C, at a heating rate of 20°C / min, under the conditions specified in JIS Z8703, to obtain a differential scanning calorimetry (DSC) curve. In addition, an empty aluminum pan was used as a reference. During the heating process, the temperature at which the differential signal (DDSC) showed a peak was determined as the glass transition temperature (°C). In addition, when multiple peaks were measured, the temperature shown by the peak with a large displacement was taken as the glass transition temperature of the polymer.

[0199] <Volume average particle size>

[0200] The volume average particle size of the polymer is measured by laser diffraction. Specifically, the aqueous dispersion of the polymer adjusted to 0.1% by mass of the solid content concentration is used as a sample. Then, in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution measuring device (Beckman Coulter, product name "LS-13 320"), the particle size D50 at which the cumulative volume calculated from the small particle size side becomes 50% is used as the volume average particle size.

[0201] <Yellow Index>

[0202] 0.6 g of the polymer as the binder material A obtained in the examples and comparative examples was measured, 19.4 g of water was added, and the mixture was heated and dissolved at 80°C for 3 hours to obtain a 3% aqueous solution of each polymer. The obtained 3% aqueous solution was used as a measurement sample, and the yellow index (YI value) was measured using a spectrophotometer. The measurement sample was heated in a 93°C water bath, and immediately taken out and placed in a quartz unit (optical path length 10 mm) after the internal temperature reached 90°C. The YI value is based on JIS K 7373-2006, using UH-4150 (manufactured by Hitachi, Ltd.) as a spectrophotometer, and the transmittance in the range of 250 nm to 800 nm was measured at 1 nm intervals using auxiliary lighting C and a 2-degree field of view by spectrophotometry, and the tristimulus values ​​X, Y, and Z in the XYZ color system were obtained based on this, and the values ​​of X, Y, and Z were calculated by the following formula.

[0203] Yellowness index (YI) = 100 (1.2769X-1.0592Z) / Y

[0204] <Adhesion after electrolyte immersion>

[0205] A single-layer polyethylene spacer (thickness: 12 μm) manufactured by a wet process was prepared as a spacer substrate. The slurry composition prepared in the examples and comparative examples was applied to one surface of the spacer substrate, and the slurry composition on the spacer substrate was dried at 50° C. for 10 minutes to form a functional layer (coated unit area mass: 0.2 g / m 2 ). A separator having the functional layer on one side was used as an evaluation separator.

[0206] In addition, a negative electrode was prepared as a negative electrode for evaluation in the same manner as in Example 1 described later.

[0207] The evaluation negative electrode and the evaluation spacer obtained above were cut into rectangles of 10mm×100mm respectively. Then, a negative electrode negative electrode composite material layer was added to the functional layer surface of the spacer as a test piece, and placed in a laminated packaging material together with about 400μL of electrolyte (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinyl carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 with a concentration of 1M). After 12 hours, the test piece was pressed together with the laminated packaging material at 80°C and a pressure of 1.0Mpa for 10 minutes.

[0208] Afterwards, take out the test piece and wipe off the electrolyte attached to the surface. Next, the surface of the current collector side of the negative electrode of the test piece is facing down, and a transparent tape is pasted on the surface of the current collector side of the negative electrode. At this time, the transparent tape specified in JIS Z1522 is used as the transparent tape. In addition, the transparent tape is fixed on a horizontal test bench. Then, one end of the spacer is stretched vertically upward at a tensile speed of 50 mm / min, and the stress during peeling is measured. This measurement is carried out three times, and the average value of the stress is calculated as the peel strength, and it is evaluated according to the following benchmarks. The greater the peel strength, the better the adhesion of the functional layer after immersion in the electrolyte, and the spacer and the electrode (negative electrode) can be firmly bonded through the functional layer in the electrolyte.

[0209] A: Peel strength is 6.0N / m or more

[0210] B: Peel strength is 2.0 N / m or more and less than 6.0 N / m

[0211] C: Peel strength is 0.5 N / m or more and less than 2.0 N / m

[0212] D: Peel strength less than 0.5N / m

[0213] <Electrolyte injection properties>

[0214] An electrolyte (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinyl carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 at a concentration of 1M) is injected into the lithium ion secondary battery made in the embodiments and comparative examples. Then, the interior of the lithium ion secondary battery is depressurized to -100kPa and maintained in this state for 1 minute. After that, heat sealing is implemented. Then, after 10 minutes, the electrode (positive electrode) is disassembled and the impregnation state of the electrolyte in the electrode is visually confirmed. Then, evaluation is performed according to the following criteria. In the electrode, the more parts impregnated with the electrolyte, the higher the electrolyte injection property.

[0215] A: All surfaces of the electrode are impregnated with the electrolyte.

[0216] B: The remaining portion of the electrode that is not impregnated with electrolyte is less than 1 cm 2 (Except when all surfaces are impregnated with electrolyte).

[0217] C: 1 cm of the electrode remains without electrolyte 2 Over and less than 2cm 2 .

[0218] D: The portion of the electrode that is not soaked in electrolyte remains 2cm 2 above.

[0219] <Anti-blocking properties>

[0220] The same spacer as the spacer with a functional layer on one side formed in the evaluation of "adhesion after electrolyte immersion" is cut into a square of 5 cm wide × 5 cm long to obtain two square pieces. Next, the two square pieces are overlapped in such a way that the surfaces of the functional layer formed on the spacer substrate are opposite to each other, and then placed under a temperature of 40°C and a pressure of 0.1MPa for 24 hours, thereby making a test piece in a pressed state (pressed test piece). Then, in the pressed test piece after being placed for 24 hours, the bonding state of the two overlapping square pieces is visually confirmed, and the anti-blocking property is evaluated according to the following benchmarks. In addition, in the case where the two overlapping square pieces are bonded to each other, one of the two square pieces is fixed as a whole, and the other is stretched with a force of 0.3N / m to confirm whether the square pieces can be peeled off from each other. The less the two overlapping square pieces are bonded to each other, the better the anti-blocking property of the spacer having the functional layer.

[0221] A: The two square pieces are not glued to each other

[0222] B: Two square sheets adhere to each other, but can be separated by stretching

[0223] C: Two square sheets are bonded to each other and cannot be separated after stretching.

[0224] <High temperature cycle characteristics>

[0225] After injecting the electrolyte into the secondary battery prepared in the embodiment and the comparative example, let it stand for 24 hours at 25°C. Use a caliper to measure the thickness of the battery at this time. After that, the following charge and discharge operations are performed at 25°C: charge to 4.2V (cutoff condition: 0.02C) by constant voltage constant current (CC-CV) at a charge rate of 1C, and discharge to 3.0V by constant current (CC) at a discharge rate of 1C. Furthermore, repeat the same charge and discharge operation at 45°C, and use a caliper to measure the thickness of the battery after 300 cycles. Then, the increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is evaluated as the expandability of the battery. The smaller the increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle, the better the expandability.

[0226] A: The increase in the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is less than 1%

[0227] B: The increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is 1% or more and less than 5%

[0228] C: The increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is 5% or more and less than 10%

[0229] D: The thickness of the battery after the cycle increases by 10% or more relative to the thickness of the battery before the cycle

[0230] <Rate characteristics>

[0231] After injecting the electrolyte into the secondary batteries made in the examples and comparative examples, let them stand at a temperature of 25°C for 5 hours. Next, charge at a temperature of 25°C with a constant current method of 0.2C until the battery cell voltage is 3.65V, and then perform an aging treatment at a temperature of 60°C for 12 hours. Then, discharge at a temperature of 25°C with a constant current method of 0.2C until the battery cell voltage is 3.00V. After that, CC-CV charging is performed at a constant current of 0.2C (upper limit battery cell voltage 4.35V), and CC discharge is performed at a constant current of 0.2C until the battery cell voltage is 3.00V. Repeat this 0.2C charge and discharge 3 times.

[0232] Next, at a temperature of 25°C, a constant current charge and discharge of 0.2C is performed between the battery cell voltage of 4.2 and 3.00V, and the discharge capacity at this time is defined as C0. After that, CC-CV charging is performed at a constant current of 0.2C in the same manner, and discharge is performed at a constant current of 0.5C to 3.0V at a temperature of -10°C, and the discharge capacity at this time is defined as C1. Then, the capacity retention rate represented by ΔC = (C1 / C0) × 100 (%) is obtained as the rate characteristic, and evaluated according to the following criteria. The larger the value of the capacity retention rate ΔC, the lower the internal resistance, and the higher the discharge capacity at high current in a low temperature environment.

[0233] A: Capacity retention rate ΔC is 70% or more

[0234] B: Capacity retention rate ΔC is less than 70%

[0235] (Example 1)

[0236] <Preparation of granular polymer>

[0237] As the particulate polymer, a polymer having a core-shell structure was prepared.

[0238] When forming the core part, 45.7 parts of styrene as an aromatic monovinyl monomer, 28.2 parts of 2-ethylhexyl acrylate as a (meth)acrylate monomer, 8.5 parts of acrylonitrile as a nitrile group-containing monomer, 0.1 parts of ethylene glycol dimethacrylate as a crosslinking monomer, 2.5 parts of methacrylic acid as an acidic group-containing monomer, 0.3 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 0.3 parts of potassium persulfate as a polymerization initiator were added to a 5 MPa pressure-resistant container equipped with a stirrer, and after being sufficiently stirred, the mixture was heated to 70° C. to initiate polymerization. The polymerization was continued until the polymerization conversion rate reached 96%, thereby obtaining an aqueous dispersion containing a particulate polymer constituting the core part. Next, in order to form the shell part, 10.0 parts of styrene as an aromatic monovinyl monomer, 4.5 parts of acrylonitrile as a nitrile group-containing monomer, and 0.5 parts of methacrylic acid as an acidic group-containing monomer were continuously added when the polymerization conversion rate reached 96%, and the polymerization was continued by heating to 70°C. When the conversion rate reached 96%, the reaction was terminated by cooling to obtain an aqueous dispersion of a granular polymer. The obtained granular polymer has a core-shell structure in which the outer surface of the core part is partially covered by the shell part.

[0239] Then, the glass transition temperature and volume average particle size of the obtained particulate polymer were measured. The results are shown in Table 1.

[0240] <Preparation of Adhesive Material B>

[0241] In a 5MPa pressure-resistant container with a stirrer, 62.2 parts of styrene as an aromatic monovinyl monomer, 33.0 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.8 parts of itaconic acid as an acidic group-containing monomer, 1.0 parts of 2-hydroxyethyl acrylate as a hydroxyl-containing monomer, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts by mass of ion exchange water and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction and a mixture containing a polymer was obtained. After adding a 5% sodium hydroxide aqueous solution to the mixture containing the polymer to adjust the pH to 8, the unreacted monomers were removed from the mixture by heating and reduced pressure distillation. Thereafter, the mixture was cooled to below 30°C to obtain an aqueous dispersion of the adhesive material B.

[0242] Then, the glass transition temperature of the obtained adhesive material B was measured. The results are shown in Table 1.

[0243] <Preparation of bonding material A>

[0244] 2660g of ion exchange water and 42g of anhydrous sodium sulfate were placed in a 10L flask with a rubber stopper, and the inside of the flask was replaced with nitrogen at a flow rate of 100mL / min. Next, 3.5g of partially saponified polyvinyl alcohol (saponification degree 90%) as a dispersant and 3.5g of lauroyl peroxide as a polymerization initiator were added, and the internal temperature was raised to 60°C. Then, 179g of methyl acrylate as an ethylenically unsaturated carboxylic acid ester monomer and 720g of vinyl acetate as a vinyl ester were mixed and added dropwise to the flask using a dropping funnel over 4 hours, and the internal temperature was maintained at 65°C for 2 hours. After that, 1558g of methanol, 1445g of water, 455g of lithium hydroxide as an alkali metal compound, and 1.82g of ascorbic acid as a reducing agent were added in batches over 10 hours at 30°C. After all were added, stirred at 30°C for 3 hours. After the stirring was completed, the solid was filtered out, washed with methanol, and dried at 70°C for 8 hours to obtain a copolymer of vinyl alcohol / lithium methyl acrylate neutralized product as the adhesive material A. 1 H-NMR measurement confirmed the presence of vinyl alcohol units and methyl acrylate units having a lithium salt group.

[0245] <Preparation of slurry composition for non-aqueous secondary battery functional layer>

[0246] In a stirring container, 100 parts (equivalent to the solid content) of an aqueous dispersion of a granular polymer, 2.0 parts (equivalent to the solid content) of an aqueous dispersion of an adhesive material A, 10 parts (equivalent to the solid content) of an aqueous dispersion of an adhesive material B, and 2 parts (equivalent to the solid content) of "NOPTEX (registered trademark) ED-052" (manufactured by San Nopco Co., Ltd.) as a wetting agent are mixed to obtain a mixture.

[0247] The obtained mixture was diluted with ion exchange water to obtain a slurry composition (solid content concentration: 10%). A separator having a functional layer on one side was prepared using the slurry composition, and the adhesion of the functional layer after electrolyte immersion and the anti-blocking property of the separator having the functional layer were evaluated. The results are shown in Table 1.

[0248] <Production of a spacer having functional layers on both sides>

[0249] A polyethylene microporous membrane (manufactured by Asahi Kasei Corporation, product name "ND412", thickness: 12 μm) was prepared. A ceramic slurry (manufactured by Japan Zeon Co., Ltd., product name "BM-2000M", containing alumina as heat-resistant particles and a binder) was applied to the surface of the prepared microporous membrane, and dried at a temperature of 50° C. for 3 minutes to obtain a spacer substrate having a porous membrane layer on one side (thickness of the porous membrane layer: 3 μm).

[0250] The above-mentioned non-aqueous secondary battery functional layer slurry composition was applied to the surface of the separator substrate provided with the porous membrane layer, and dried for 3 minutes at a temperature of 50° C. The same operation was performed on the other side of the separator substrate to obtain a separator having functional layers on both sides (the thickness of the functional layers: each was 0.6 μm).

[0251] <Production of negative electrode>

[0252] In a 5MPa pressure-resistant container with a stirrer, 33 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.5 parts of itaconic acid as an acidic group-containing monomer, 63.5 parts of styrene as an aromatic monovinyl monomer, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the polymerization reaction was terminated by cooling to obtain a mixture containing a granular binder (styrene-butadiene copolymer). After adding 5% sodium hydroxide aqueous solution to the above mixture to adjust the pH to 8, the unreacted monomers were removed by heating and reduced pressure distillation. After that, the mixture was cooled to below 30°C to obtain an aqueous dispersion containing a binder for the negative electrode.

[0253] In a planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360 mAh / g), 48.75 parts of natural graphite (theoretical capacity: 360 mAh / g), and 1 part of carboxymethyl cellulose as a thickener were added as negative electrode active materials. Furthermore, the mixture was diluted with ion exchange water to a solid content concentration of 60%, and then mixed at a speed of 45 rpm for 60 minutes. After that, 1.5 parts of an aqueous dispersion containing a negative electrode binder obtained as described above was added in a solid content equivalent, and mixed at a speed of 40 rpm for 40 minutes. Then, ion exchange water was added in such a way that the viscosity became 3000 ± 500 mPa·s (B-type viscometer, measured at 25°C and 60 rpm), thereby preparing a slurry composition for a negative electrode composite material layer.

[0254] The negative electrode composite material layer slurry composition was coated with a notch wheel coater so that the coating amount became 11±0.5 mg / cm 2 The copper foil was coated with the slurry composition for the negative electrode composite material layer in a manner of 15 μm thick. The copper foil coated with the slurry composition for the negative electrode composite material layer was then conveyed in an oven at a temperature of 80°C for 2 minutes at a speed of 400 mm / min, and then conveyed in an oven at a temperature of 110°C for another 2 minutes, thereby drying the slurry composition on the copper foil to obtain a negative electrode raw material having a negative electrode composite material layer formed on the current collector.

[0255] Afterwards, the negative electrode composite material layer side of the prepared negative electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 11 t (tons) to obtain a negative electrode composite material layer with a density of 1.60 g / cm 3 Then, the negative electrode was placed in an environment of temperature 25±3°C and relative humidity 50±5% for 1 week.

[0256] <Manufacturing of positive electrode>

[0257] 96 parts of Co-Ni-Mn lithium composite oxide (CELLSEED (registered trademark), NMC111, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), 2 parts of acetylene black (manufactured by Denka Co., Ltd., product name "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Chemical Co., Ltd., product name "KF-1100") as a binder, and then N-methyl-2-pyrrolidone (NMP) as a dispersion medium is added to mix in a manner so that the total solid content concentration becomes 67% to prepare a slurry composition for a positive electrode composite material layer.

[0258] Next, the obtained slurry composition for positive electrode composite material layer was coated with a notch wheel coater so that the coating amount became 20±0.5 mg / cm 2 The molten-salt film was coated on an aluminum foil with a thickness of 20 μm as a current collector.

[0259] The slurry composition on the aluminum foil was dried by conveying it in an oven at 90°C for 2 minutes at a speed of 200 mm / min and in an oven at 120°C for another 2 minutes to obtain a positive electrode raw material having a positive electrode composite material layer formed on the current collector.

[0260] Afterwards, the positive electrode composite material layer side of the prepared positive electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 14 t (tons) to obtain a positive electrode composite material layer density of 3.40 g / cm 3 Thereafter, the positive electrode was placed in an environment of a temperature of 25±3° C. and a relative humidity of 50±5% for 1 week.

[0261] <Manufacturing of secondary batteries>

[0262] The separator with functional layers on both sides, the negative electrode and the positive electrode obtained as described above were used to make a wound battery unit (discharge capacity equivalent to 520 mAh) and placed in an aluminum packaging material. The wound battery unit and the aluminum packaging material were pressed together at a temperature of 70°C and a pressure of 1.0 MPa using a flat hot press for 8 seconds to bond the separator to the electrodes (negative and positive electrodes).

[0263] After that, the aluminum packaging material is filled with an electrolyte. In addition, as the electrolyte, a solution prepared by dissolving LiPF6 (supporting electrolyte) at a concentration of 1 mol / liter in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC) and vinylene carbonate (VC) (volume ratio: EC / DEC / VC=68.5 / 30 / 1.5) is used. Furthermore, in order to seal the opening of the aluminum packaging material, the aluminum packaging material is sealed by heat sealing at a temperature of 150°C to manufacture a lithium ion secondary battery. The lithium ion secondary battery is used to evaluate the electrolyte injection properties, rate characteristics and high temperature cycle characteristics. The results are shown in Table 1.

[0264] (Examples 2-3)

[0265] When preparing the granular polymer, the types and usage ratios of the monomers used to form the core portion were changed as shown in Table 1, and various operations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core portion was partially covered by the shell portion. In addition, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0266] (Example 4)

[0267] As the particulate polymer, a polymer not having a core-shell structure was prepared.

[0268] In a 5 MPa pressure-resistant container equipped with a stirrer, 65.5 parts of styrene as an aromatic monovinyl monomer, 24.0 parts of butyl acrylate as a (meth)acrylate monomer, 0.5 parts of ethylene glycol dimethacrylate and 10.0 parts of glycidyl methacrylate as crosslinking monomers, 0.3 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.3 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to 70° C. to initiate polymerization. The polymerization was continued until the polymerization conversion rate reached 96%, thereby obtaining an aqueous dispersion containing a particulate polymer having no core-shell structure.

[0269] Other than this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0270] (Example 5)

[0271] A polymer without a core-shell structure was prepared in the same manner as in Example 4 except that the preparation conditions of the granular polymer were changed so that the volume average particle size of the obtained granular polymer became 4 μm. When preparing the slurry composition, 30 parts (solid content equivalent) of the aqueous dispersion of the granular polymer thus obtained, 3 parts (solid content equivalent) of the aqueous dispersion of the binder B, 2.0 parts of the binder A, 70 parts of alumina (AKP-3000 manufactured by Sumitomo Chemical, volume average particle size D50=0.7 μm) as heat-resistant particles, and 0.2 parts (solid content equivalent) of "NOPTEX (registered trademark) ED-052" (manufactured by San Nopco Corporation) as a wetting agent were mixed in a stirring container to obtain a mixture.

[0272] The obtained mixture was diluted with ion exchange water to obtain a slurry composition (solid content concentration: 40%). The slurry composition was used to make a spacer having a functional layer on one side, and the adhesion of the functional layer after electrolyte immersion and the anti-blocking property of the spacer having the functional layer were evaluated. The results are shown in Table 1. In addition, using the slurry composition obtained in this way, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0273] (Example 6)

[0274] The various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that a particulate polymer prepared as follows was used as the binder material B. The results are shown in Table 1.

[0275] <Manufacture of adhesive material B>

[0276] 70 parts of ion exchange water, 0.15 parts of sodium lauryl sulfate (manufactured by Kao Chemical Co., Ltd., product name "EMAL (registered trademark) 2F") as an emulsifier, and 0.5 parts of ammonium persulfate were respectively supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen, and the temperature was raised to 60°C.

[0277] In another container, 50 parts of ion exchange water, 0.5 parts of sodium dodecylbenzene sulfonate as a dispersant, 79.0 parts of n-butyl acrylate as a (meth)acrylate monomer, 2.5 parts of methacrylic acid as an acidic group-containing monomer, 3.5 parts of N-hydroxymethyl acrylamide as a crosslinking monomer, and 15.0 parts of acrylonitrile as a nitrile-containing monomer are mixed to obtain a monomer composition. The monomer composition is continuously added to the above reactor for 4 hours to perform polymerization. During the addition process, the reaction is carried out at 60°C. After the addition is completed, the reaction is terminated by further stirring at 70°C for 3 hours to prepare an aqueous dispersion containing the binder material B.

[0278] (Example 7)

[0279] The various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that a particulate polymer prepared as follows was used as the binder material B. The results are shown in Table 1.

[0280] <Manufacture of adhesive material B>

[0281] The composition of the monomer composition used in the preparation of the adhesive material B was changed as shown in Table 1. Specifically, the amounts of n-butyl acrylate and acrylonitrile were reduced as shown in Table 1, and 15 parts of glycidyl methacrylate were added as a crosslinking monomer in addition to 3.5 parts of N-methylol acrylamide. A water dispersion containing the adhesive material B was prepared in the same manner as in Example 6 except for the above.

[0282] (Example 8)

[0283] The various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that a polymer prepared as follows was used as the binder material A. The results are shown in Table 1.

[0284] <Preparation of bonding material A>

[0285] The same procedure as in Example 1 was followed except that 1.82 g of sodium thiosulfate was used as a reducing agent instead of ascorbic acid and 455 g of sodium hydroxide was used as an alkali metal compound to obtain a copolymer of vinyl alcohol / lithium methyl acrylate neutralized product as a binder material A. 1 H-NMR measurement confirmed the presence of vinyl alcohol units and methyl acrylate units having a sodium salt group.

[0286] (Examples 9-10)

[0287] The various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that the blending amounts of the adhesive material A were changed as shown in Table 1. The results are shown in Table 2.

[0288] (Example 11)

[0289] The results are shown in Table 2, except that polyvinyl acetate (manufactured by TECHNO CHEMICAL CO., LTD., polyvinyl acetate) which is a homopolymer was used as the particulate polymer, various operations, measurements, and evaluations were carried out in the same manner as in Example 1.

[0290] (Comparative Example 1)

[0291] The results are shown in Table 2, except that the particulate polymer was not blended, various operations, measurements, and evaluations were carried out in the same manner as in Example 1.

[0292] (Comparative Example 2)

[0293] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2, and a granular polymer having a glass transition temperature higher than 95° C. was prepared and used. Various operations, measurements and evaluations were carried out in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core part was partially covered by the shell part. The results are shown in Table 2.

[0294] (Comparative Example 3)

[0295] The various operations, measurements and evaluations were carried out in the same manner as in Example 1 except that a polymer synthesized as follows was added (in Table 2, for convenience of description, the addition is shown in the column of the binder A) instead of the binder A. The results are shown in Table 2.

[0296] <Synthesis of polymer to be added instead of binder material A>

[0297] In a 10L flask with a rubber stopper, add 2660g of ion exchange water and 42g of anhydrous sodium sulfate, and replace the interior of the flask with nitrogen at a flow rate of 100mL / min. Next, add 3.5g of partially saponified polyvinyl alcohol (saponification degree 90%) as a dispersant and 3.5g of lauroyl peroxide as a polymerization initiator, and raise the internal temperature to 60°C. Then, mix 179g of methyl acrylate as an ethylenically unsaturated carboxylic acid ester monomer and 720g of vinyl acetate as a vinyl ester, and add dropwise to the flask using a dropping funnel over 4 hours, keeping the internal temperature at 65°C for 2 hours. After 2 hours, filter out the solid from the reaction solution, wash with methanol, and dry at 70°C for 8 hours to obtain a polymer containing vinyl acetate units and methyl acrylate units. The obtained polymer is subjected to 1 However, no vinyl alcohol unit and alkali metal salt group were detected by H-NMR.

[0298] (Comparative Example 4)

[0299] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2 so that the glass transition temperature was 20° C., and various operations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core part was partially covered by the shell part. In addition, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.

[0300] In addition, in Tables 1 and 2 shown below,

[0301] "ST" represents styrene unit,

[0302] "EDMA" means ethylene glycol methacrylate units,

[0303] "GMA" means glycidyl methacrylate unit,

[0304] "NMA" means N-methylol acrylamide unit,

[0305] "MAA" means methacrylic acid units,

[0306] "2EHA" means 2-ethylhexyl acrylate units,

[0307] "BA" represents n-butyl acrylate unit,

[0308] "AN" stands for acrylonitrile unit,

[0309] "MMA" means methyl methacrylate units,

[0310] "IA" represents itaconic acid unit,

[0311] "BD" represents 1,3-butadiene units,

[0312] "βHEA" represents 2-hydroxyethyl acrylate units.

[0313] [Table 1]

[0314]

[0315] [Table 2]

[0316]

[0317] As can be seen from Tables 1 to 2, in Examples 1 to 11, a slurry composition for a functional layer comprising a granular polymer and a binder material A was used, the glass transition temperature of the granular polymer being above 30°C and below 95°C, and the binder material A comprising at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group, thereby obtaining a functional layer having excellent anti-adhesion properties and a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics.

[0318] On the other hand, it can be seen that in Comparison Example 1 in which the specified granular polymer is not formulated, Comparison Examples 2 and 4 in which a granular polymer is formulated but its glass transition temperature is outside the above range, and Comparison Example 3 in which the adhesive material A does not have hydroxyl groups and alkali metal salt groups, a non-aqueous secondary battery with excellent anti-blocking functional layer and excellent electrolyte injection properties and high-temperature cycle characteristics cannot be obtained.

[0319] Industrial Applicability

[0320] According to the present invention, a slurry composition for a nonaqueous secondary battery functional layer can provide a functional layer having excellent anti-blocking properties and a secondary battery having both high electrolyte injection properties and high-temperature cycle characteristics.

[0321] Furthermore, according to the present invention, it is possible to provide a separator for a non-aqueous secondary battery which can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0322] Furthermore, according to the present invention, a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics can be provided.

[0323] Furthermore, according to the present invention, the slurry composition for a non-aqueous secondary battery functional layer of the present invention can be produced efficiently.

Claims

1. A slurry composition for a non-aqueous secondary battery functional layer, comprising a granular polymer and a binder material A, The particulate polymer has at least one glass transition temperature in the temperature range of 30° C. or more and 95° C. or less, The bonding material A includes at least one of a hydroxyl group and an acidic functional group and an alkali metal salt group.

2. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The bonding material A is a copolymer of vinyl alcohol and an alkali metal neutralized product of an olefinically unsaturated carboxylic acid.

3. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The yellowness index of a 3 mass % aqueous solution of the adhesive material A is 14.0 or less.

4. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The volume average particle size of the particulate polymer is 0.25 μm or more and 5 μm or less.

5. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The particulate polymer has a core-shell structure.

6. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The slurry composition for a non-aqueous secondary battery functional layer further includes heat-resistant particles.

7. A separator for a non-aqueous secondary battery, comprising a separator substrate and a functional layer formed on at least a portion of at least one surface of the separator substrate, The functional layer is a dried product of the slurry composition for a non-aqueous secondary battery functional layer according to any one of claims 1 to 6.

8. A non-aqueous secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, The separator is the separator for a non-aqueous secondary battery according to claim 7.

9. A method for producing a slurry composition for a non-aqueous secondary battery functional layer, wherein the slurry composition for a non-aqueous secondary battery functional layer is the slurry composition for a non-aqueous secondary battery functional layer according to any one of claims 1 to 6, and the method comprises the following steps: A monomer composition containing at least one of a vinyl ester monomer and an ethylenically unsaturated carboxylic acid ester monomer is polymerized to obtain a polymer, and the polymer is further saponified in the presence of an alkali metal compound and a reducing agent to obtain a saponified product of the polymer as the binder material A.