Separator for rechargeable lithium battery and rechargeable lithium battery including same
By using a combination of porous substrate, heat-resistant layer and adhesive layer in the lithium battery separator, the problem of insufficient shape maintenance at high temperature and adhesion at low temperature is solved, and the high-temperature cycle life characteristics and safety improvement of lithium battery is achieved.
Patent Information
- Application Number
- CN202380029443.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing lithium battery separators are difficult to maintain shape under high temperature conditions, resulting in lithium salt precipitation and battery safety problems. They also lack adhesion at low temperature/low pressure, making it difficult to apply to high temperature/high pressure processes.
The separator is composed of a porous substrate, a heat-resistant layer and an adhesive layer. The heat-resistant layer is composed of binders such as polyacrylate and inorganic particles. The adhesive layer contains vinyl aromatic monomers, alkyl acrylates and phosphines. The copolymer of acid ester monomers ensures that the membrane does not shrink at high temperatures and has excellent adhesion.
It realizes the heat resistance and shape of the diaphragm at high temperature, inhibits lithium salt precipitation, improves the safety and cycle life characteristics of the battery, and shows strong adhesion at low temperature/low pressure, suitable for high temperature/high pressure processes .
Smart Images

Figure CN118922996A_ABST
Abstract
Description
Technical Field
[0001] Disclosed are a separator for a rechargeable lithium battery and a rechargeable lithium battery including the separator. Background Art
[0002] The separator used in electrochemical cells is an intermediate film that separates the positive electrode and the negative electrode in the battery and continuously maintains ion conductivity to enable charging and discharging of the battery. However, when the battery is exposed to a high temperature environment due to abnormal behavior, the battery generates heat and starts thermal runaway. Therefore, the separator should have a shutdown function (a function of blocking pores by melting the hot-melt resin) to suppress the ignition of the battery, and should ensure the safety of the battery by maintaining its shape without shrinking even at high temperatures.
[0003] Recently, there has been a demand for higher capacity and higher output of batteries, and there is a trend to apply high nickel-based positive electrode active materials with a nickel content of 80 mol% or more or to manufacture them into a stacked battery structure that is easy to achieve capacity. In addition to high capacity and high output, there is a trend to require battery safety that suppresses battery temperature rise and ignition even at high temperatures.
[0004] For example, when a high-nickel positive electrode active material is used, a large amount of gas may be generated under high temperature conditions, which may lead to problems such as capacity drop or heat generation during the cycle, making it more necessary to ensure battery safety. Specifically, when gas is generated in the battery, the gas is located between the diaphragm and the electrode plate interface, and lithium salts are precipitated, which may cause the pores of the diaphragm to be blocked or short-circuited, and the cycle life may be reduced. Therefore, the diaphragm is required to have ultra-high heat resistance and high adhesion to the electrode plate. Summary of the invention
[0005] Technical issues A separator for a rechargeable lithium battery is provided, which has improved heat resistance and adhesion between the separator and the electrode plate, thereby maintaining the shape of the separator even at high temperatures and inhibiting the precipitation of lithium salts at the interface, thereby providing a separator for a rechargeable lithium battery with improved battery safety and reliability, and a separator for a rechargeable lithium battery that exhibits excellent adhesion even at low temperature / low pressure and can be used for battery types that cannot be applied to high temperature / high pressure processes.
[0006] Technical Solution In an embodiment, a separator for a rechargeable lithium battery includes: a porous substrate; a heat-resistant layer on at least one surface of the porous substrate; and an adhesive layer on the heat-resistant layer, wherein the heat-resistant layer includes a first binder and inorganic particles, the first binder includes at least one selected from polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl alcohol, polysulfonic acid, polyacrylamide, polyamide, polyurea, polyurethane and their copolymers, the adhesive layer includes a second binder, and the second binder includes a copolymer including a first unit derived from a vinyl aromatic monomer, a second unit derived from an alkyl acrylate and a third unit derived from a phosphonate monomer.
[0007] In another embodiment, a rechargeable lithium battery includes a positive electrode, a negative electrode, the aforementioned separator between the positive electrode and the negative electrode, and an electrolyte.
[0008] Beneficial Effects According to the embodiment, the separator for a rechargeable lithium battery achieves ultra-high heat resistance, improves adhesion to the electrode plate, maintains the shape of the separator even at high temperatures, and inhibits lithium salt precipitation at the interface, thereby ensuring the safety and reliability of the battery, and exhibits excellent adhesion even at low temperature / low pressure, so it can be used for battery types that cannot be applied to high temperature / high pressure processes. A rechargeable lithium battery using such a separator can have improved processability, high temperature cycle life characteristics, safety and reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a cross-sectional view schematically showing a rechargeable lithium battery.
[0010] Figure 2 is a graph showing changes in the temperature within the battery of Comparative Example 1 during the high temperature cycle life of the battery.
[0011] Figure 3 is a graph showing changes in the temperature within the battery of Example 1 during the high temperature cycle life of the battery.
[0012] Figure 4 is a graph showing the charge / discharge efficiency of the battery cell of Comparative Example 1.
[0013] Figure 5 is a graph showing the charge / discharge efficiency of the battery cell of Example 1. DETAILED DESCRIPTION
[0014] Hereinafter, specific embodiments will be described in detail so that those skilled in the art can easily implement the specific embodiments. However, the present disclosure may be implemented in many different forms and is not to be construed as limited to the example embodiments set forth herein.
[0015] The terms used herein are only used to describe the embodiments and are not intended to limit the present disclosure. Unless the context clearly indicates otherwise, a singular expression includes a plural expression.
[0016] As used herein, "combinations thereof" refers to mixtures, stacks, composites, copolymers, alloys, blends, reactants, and the like of components.
[0017] Here, it should be understood that terms such as “includes,” “comprising,” or “having” are intended to indicate the presence of the presented features, quantities, steps, elements, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.
[0018] In the drawings, the thickness of layers, films, panels, regions, etc., is exaggerated for clarity, and the same reference numerals represent the same elements throughout the specification. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, the element may be directly on the other element, or there may be intervening elements. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0019] Furthermore, the "layer" here includes not only a shape formed on the entire surface when viewed from a plan view but also a shape formed on a part of the surface.
[0020] In addition, the average particle diameter and the average size can be measured by methods known to those skilled in the art, for example, can be measured by a particle size analyzer, or can be measured by a transmission electron micrograph or a scanning electron micrograph. Alternatively, the average particle diameter value can be obtained by measuring the size using a dynamic light scattering method, performing data analysis, counting the number of particles in each particle size range, and calculating therefrom. As used herein, when no definition is otherwise provided, the average particle diameter can mean the diameter (D50) of particles measured by a particle size analyzer and having a cumulative volume of 50% by volume in a particle size distribution.
[0021] Here, “or” is not to be interpreted as an exclusive meaning, for example, “A or B” is interpreted to include A, B, A+B, etc.
[0022] Diaphragm In an embodiment, a separator for a rechargeable lithium battery is provided, the separator comprising: a porous substrate; a heat-resistant layer on at least one surface of the porous substrate; and an adhesive layer on the heat-resistant layer. The heat-resistant layer and the adhesive layer may be positioned on one surface or both surfaces of the porous substrate. The separator may be referred to as a coated separator.
[0023] The heat-resistant layer includes a first binder and inorganic particles. The first binder includes at least one selected from polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl alcohol, polysulfonic acid, polyacrylamide, polyamide, polyurea, polyurethane and copolymers thereof. The adhesive layer includes a second binder, which includes a copolymer including a first unit derived from a vinyl aromatic monomer, a second unit derived from an alkyl acrylate and a third unit derived from a phosphonate monomer.
[0024] The separator can achieve ultra-high heat resistance by including a heat-resistant layer, and for example, the separator can satisfy a 150°C dry shrinkage rate of less than 5% and a 150°C wet shrinkage rate of less than 15%. Therefore, the separator maintains its shape even under high temperature conditions and does not deteriorate performance, thereby improving the cycle life characteristics and safety of the battery.
[0025] In addition, by including an adhesive layer, the separator can achieve excellent adhesion even at low temperature and low pressure, and can exhibit stable and strong adhesion between the separator and the electrode plate. The adhesive layer applied to most separators exhibits adhesion under high temperature and high pressure conditions while being impregnated with an electrolyte, and the adhesion of the separator-negative electrode is generally lower than that of the separator-positive electrode. On the other hand, the adhesive layer according to the embodiment achieves adhesion even at temperatures (e.g., 10°C to 50°C) in the battery manufacturing process, and even at very low pressures due to thickness changes caused by charging and discharging of the battery, and it can also be applied to battery types that are difficult to apply high temperature and high pressure processes. In addition, by including an adhesive layer, the separator can achieve an adhesion strength of 0.1 gf / mm or more for both the separator-positive electrode and the separator-negative electrode under low temperature and low pressure conditions. Therefore, the long-term cycle life characteristics and safety of the battery can be improved.
[0026] For example, in a high-capacity battery using a high-nickel positive electrode active material, a lot of gas is generated in the battery during operation. However, if there is no adhesion or low adhesion between the separator and the electrode plate, lithium salts will precipitate at the interface, causing a sharp drop in capacity or heat generation. On the other hand, the separator according to the embodiment has very excellent adhesion between the positive electrode and the negative electrode, and can inhibit the precipitation of lithium salts at the interface, thereby improving the cycle life characteristics of the battery and effectively improving safety issues such as fire and thermal runaway.
[0027] porous substrate The polyolefin used as the porous substrate material in the diaphragm may be, for example, a homopolymer (such as polyethylene or polypropylene), a copolymer, or a mixture thereof. Polyethylene may be low-density, medium-density, or high-density polyethylene, and from the viewpoint of mechanical strength, high-density polyethylene may be used. In addition, for the purpose of providing flexibility, two or more types of polyethylene may be mixed. From the viewpoint of achieving both mechanical strength and high air permeability, the weight average molecular weight of polyethylene may be 100,000 g / mol to 12,000,000 g / mol, for example, 200,000 g / mol to 3,000,000 g / mol. Polypropylene may be a homopolymer, a random copolymer, or a block copolymer, and may be used alone or in a mixture of two or more. In addition, stereoregularity is not particularly limited, and isotactic polypropylene, syndiotactic polypropylene, or atactic polypropylene may be used, but inexpensive isotactic polypropylene may be used. In addition, additives (such as polyolefins other than polyethylene or polypropylene) and antioxidants may be added to the polyolefin.
[0028] The porous substrate may include, for example, a polyolefin (such as polyethylene or polypropylene), and may include a multilayer membrane of two or more layers (such as a polyethylene / polypropylene double-layer membrane, a polyethylene / polypropylene / polyethylene three-layer membrane, a polypropylene / polyethylene / polypropylene three-layer membrane), but is not limited thereto, and any material and configuration that can be used as a porous substrate in the art may be possible.
[0029] The porous substrate may include, for example, a diene polymer prepared by polymerizing a monomer composition including a diene monomer. The diene monomer may be a conjugated diene monomer or a non-conjugated diene monomer. For example, the diene monomer may include one or more selected from 1,3-butadiene, isoprene, 2-chloro-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, vinylpyridine, vinyl norbornene, dicyclopentadiene and 1,4-hexadiene.
[0030] The thickness of the porous substrate may be 1 μm to 100 μm, for example, 1 μm to 30 μm, 5 μm to 20 μm, 5 μm to 15 μm, or 5 μm to 10 μm. If the thickness of the porous substrate is less than 1 μm, it may be difficult to maintain the mechanical properties of the separator, and if the thickness of the porous substrate is greater than 100 μm, the internal resistance of the lithium battery may increase.
[0031] The porosity of the porous substrate may be 5% to 95%. If the porosity of the porous substrate is less than 5%, the internal resistance of the lithium battery may increase, and if the porosity is greater than 95%, it may be difficult to maintain the mechanical properties of the porous substrate.
[0032] The pore size of the porous substrate may be 0.01 μm to 50 μm, for example, 0.01 μm to 20 μm or 0.01 μm to 10 μm. If the pore size of the porous substrate is less than 0.01 μm, the internal resistance of the lithium battery may increase, and if the pore size of the porous substrate is greater than 50 μm, it may be difficult to maintain the mechanical properties of the porous substrate.
[0033] Heat resistant layer First binder The first binder includes at least one selected from polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl alcohol, polysulfonic acid, polyacrylamide, polyamide, polyurea, polyurethane and copolymers thereof. The first binder may be applied to the heat-resistant layer together with inorganic particles to provide the separator with high heat resistance.
[0034] Here, acrylic acid has a concept including methacrylic acid and acrylic acid, and polysulfonic acid is a polymer derived from a monomer including a sulfonic acid group, such as polyacrylsulfonic acid, polyacrylamidesulfonic acid, polyvinylsulfonic acid, polyallylsulfonic acid, polystyrenesulfonic acid, polyanetholesulfonic acid, and the like.
[0035] The first binder may include, for example, a homopolymer or copolymer of polyacrylamide, or a copolymer of polyacrylamide and polysulfonic acid.
[0036] For example, the first binder may include a copolymer including a first unit derived from (meth)acrylamide, a second unit derived from a monomer containing a sulfonic acid group, and a third unit derived from (meth)acrylic acid, (meth)acrylate, a monomer containing a nitrile group, a monomer containing an alcohol group, or a combination thereof. The first binder may provide the separator with ultrahigh heat resistance. Here, the unit may be expressed as a repeating unit or a structural unit.
[0037] The first unit derived from (meth)acrylamide can improve the adhesion characteristics with the porous substrate through the acrylamide functional group and form hydrogen bonds with the -OH functional group of the inorganic particles, so the inorganic particles in the heat-resistant layer can be more firmly fixed, thereby enhancing the heat resistance of the separator.
[0038] The second unit derived from the monomer containing the sulfonic acid group includes a bulky functional group, thereby reducing the mobility of the copolymer and enhancing the heat resistance of the separator. Here, the sulfonic acid may include a sulfonate. The sulfonate is a salt composed of a sulfonic acid and a suitable cation, and the cation may be, for example, an alkali metal ion. That is, the sulfonate may be an alkali metal sulfonate.
[0039] The monomer containing a sulfonic acid group may include, for example, (meth)acryloylsulfonic acid, (meth)acryloylalkylsulfonic acid, (meth)acrylamidesulfonic acid, (meth)acrylamidealkylsulfonic acid, vinylsulfonic acid, allylsulfonic acid, styrenesulfonic acid, anetholesulfonic acid or salts thereof. Here, the alkyl group may be a C1 to C20 alkyl group, a C1 to C10 alkyl group or a C1 to C6 alkyl group.
[0040] The (meth)acryloylalkylsulfonic acid may be, for example, 2-sulfoethyl (meth)acrylate, 3-sulfopropyl (meth)acrylate, or the like, and the (meth)acrylamidoalkylsulfonic acid may be, for example, 2-acrylamido-2-methylpropanesulfonic acid.
[0041] The third unit derived from (meth) acrylic acid, (meth) acrylic acid ester, a monomer containing a nitrile group, a monomer containing an alcohol group, or a combination thereof is used to fix the inorganic particles on the porous substrate, and at the same time can provide adhesion, so that the heat-resistant layer can be well adhered to the porous substrate, and can help improve the heat resistance and air permeability of the separator. In addition, the dispersibility of the heat-resistant layer composition can be improved by the acrylic acid group or the alcohol group, and the oxidation resistance of the separator can be increased and the moisture content can be reduced by the nitrile group.
[0042] The (meth)acrylate may include, for example, methyl acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, 2-(perfluoropentyl)ethyl (meth)acrylate, 2-(perfluorohexyl)ethyl (meth)acrylate, 2-(perfluorooctyl)ethyl (meth)acrylate, 2-(perfluorononyl)ethyl (meth)acrylate, 2-(perfluorodecyl)ethyl (meth)acrylate, or a combination thereof.
[0043] The monomer containing a nitrile group may be, for example, acrylonitrile, cyanoalkyl (meth)acrylate, or a combination thereof. Here, the alkyl group may be a C1 to C20 alkyl group, a C1 to C10 alkyl group, or a C1 to C6 alkyl group. The cyanoalkyl (meth)acrylate may be, for example, cyanomethyl (meth)acrylate, cyanoethyl (meth)acrylate, cyanopropyl (meth)acrylate, or cyanooctyl (meth)acrylate.
[0044] The monomer comprising an alcohol group may be, for example, vinyl alcohol or olefin alcohol. The alkene alcohol can be, for example, 2-methyl-3-butene-1-ol, 2-ethyl-3-butene-1-ol, 1,1-diphenyl-3-butene-1-ol, 2-methyl-3-butene-2-ol, 2,2-dimethyl-3-butene-1-ol, 3-methyl-1-pentene-3-ol, 2,4-dimethyl-4-pentene-2-ol, 4-alkenyl-2-pentanol, 4-methyl-4-pentene-2-ol, 2-methyl-4-pentene-2-ol, 2-phenyl-4-pentene-2-ol, 2-allylhexamethylenefluoroisopropanol, 2-hydroxy-5-hexene, 3-butene-2-ol, 3-methyl-5-hexene-3-ol, 2-methyl-2-hydroxy-5-hexene, 1-allylcyclohexanol, 2,3-dimethyl-2-hydroxy-5-hexene, 1-heptene-4-ol, and the like.
[0045] In the first binder, the copolymer may include, for example, 55mol% to 99mol% of the first unit, 0.5mol% to 40mol% of the second unit, and 0.5mol% to 40mol% of the third unit. Alternatively, in the first binder, the copolymer may include 75mol% to 94mol% of the first unit, 1mol% to 10mol% of the second unit, and 5mol% to 15mol% of the third unit. Here, the amount range of each unit is based on 100mol% of the copolymer. When the copolymer includes each unit within the range, the first binder can be very firmly bonded to the inorganic particles in the heat-resistant layer, the heat-resistant layer and the porous substrate can be firmly adhered, and by enabling the heat-resistant layer composition to have appropriate viscosity and dispersibility, the heat resistance, chemical resistance, adhesion and processability of the diaphragm can be finally improved.
[0046] In the first binder, the copolymer may further include other units in addition to the first to third units, for example, the copolymer may further include diene units, styrene units, ester units, carbonate units, and the like.
[0047] In addition, the copolymer in the first binder may be in various forms, such as an alternating polymer in which units are alternately distributed, a random polymer in which units are randomly distributed, or a graft polymer in which some structural units are grafted.
[0048] The weight average molecular weight of the copolymer of the first binder can be 300,000 g / mol to 970,000 g / mol, for example, 350,000 g / mol to 970,000 g / mol, 450,000 g / mol to 970,000 g / mol, or 450,000 g / mol to 700,000 g / mol. In this case, the diaphragm including the first binder in the heat-resistant layer can show excellent adhesion, heat resistance and air permeability. The weight average molecular weight can be the polystyrene conversion average molecular weight measured using gel permeation chromatography.
[0049] The copolymer of the first binder may be prepared by various known methods such as emulsion polymerization, suspension polymerization, bulk polymerization, solution polymerization or block polymerization.
[0050] Based on 100wt% of the heat-resistant layer, the first binder may be present in an amount of 1wt% to 20wt%, for example, 1wt% to 15wt%, 1wt% to 10wt%, or 1wt% to 5wt%. When the first binder is included within this range, adhesion and heat resistance of the heat-resistant layer may be improved at the same time.
[0051] Inorganic particles The inorganic particles can reduce the possibility of short circuit between the positive electrode and the negative electrode, and prevent the separator from shrinking or deforming sharply due to temperature rise. In other words, the heat-resistant layer can improve the heat resistance and safety of the battery by including the inorganic particles.
[0052] The inorganic particles can be metal oxides, semi-metal oxides, or combinations thereof. Specifically, the inorganic particles can include aluminum oxide, titanium dioxide, boehmite, barium sulfate, calcium carbonate, calcium phosphate, amorphous silicon dioxide, crystallized glass particles, kaolin, talc, silicon dioxide-alumina composite oxide particles, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, mica, magnesium oxide, etc.
[0053] The inorganic particles can be, for example, Al2O3, SiO2, TiO2, SnO2, CeO2, NiO, CaO, ZnO, MgO, ZrO2, Y2O3, SrTiO3, BaTiO3, MgF2, Mg(OH)2, or a combination thereof. For example, the inorganic particles can be aluminum oxide, titanium dioxide, boehmite, barium sulfate, or a combination thereof.
[0054] The inorganic particles may be spherical, plate-like, fibrous, etc., but are not limited thereto, and may be in any form available in the art. Examples of plate-like inorganic particles include alumina and boehmite. Plate-like alumina, plate-like boehmite, etc. may improve the heat resistance of the separator, ensure a relatively large number of pores, and improve the physical safety of the lithium battery.
[0055] When the inorganic particles are plate-like or fibrous, the aspect ratio of the inorganic particles can be 1:5 to 1:100, for example, 1:10 to 1:100, 1:5 to 1:50 or 1:10 to 1:50. In addition, the ratio of the length of the major axis to the minor axis on the flat surface of the plate-like inorganic particles can be 1 to 3 or 1 to 2. The aspect ratio and the ratio of the length of the major axis to the minor axis can be measured using an optical microscope. When the aspect ratio and the ratio of the length of the major axis to the minor axis meet the above range, the thermal shrinkage of the diaphragm can be reduced, the relatively improved porosity can be ensured, and the physical stability of the lithium battery can be improved.
[0056] The average particle size of the inorganic particles may be 0.1 μm to 2 μm, 0.1 μm to 1.5 μm, or 0.2 μm to 1.0 μm. The average particle size is measured using a laser scattering particle size distribution meter (e.g., Horiba LA-920), and refers to the median particle size (D50) when the volume is converted to 50% cumulatively from the small particle side. By using inorganic particles having an average particle size within the above range, the bonding force between the heat-resistant layer and the porous substrate can be improved, the appropriate porosity of the separator can be ensured, and the heat resistance and processability of the separator can be improved.
[0057] The weight ratio of the first binder to the inorganic particles in the heat-resistant layer can be 1:20 to 1:40, for example, 1:25 to 1:40 or 1:25 to 1:35. In this case, the heat-resistant layer can achieve very high heat resistance and adhesion. If the weight ratio of the first binder to the inorganic particles is greater than 1:20, the porosity of the coating layer will be reduced due to the excess of the first binder, which will limit the movement of lithium ions, and the moisture absorption of the first binder will increase, resulting in degradation of battery characteristics. In addition, if the weight ratio of the first binder to the inorganic particles is less than 1:40, the heat resistance will be reduced due to the insufficient content of the binder for adhering the inorganic particles.
[0058] Based on 100wt% of the heat-resistant layer, the content of the inorganic particles may be 80wt% to 99wt%, for example, 85wt% to 99wt%, 90wt% to 99wt%, or 95wt% to 99wt%. When the inorganic particles are included in this range, the inorganic particles can achieve high mechanical rigidity and high transmittance of the heat-resistant layer and the separator including the heat-resistant layer.
[0059] The heat-resistant layer may include other binders commonly used in the art in addition to the first binder, and may include organic particles in addition to the above-mentioned inorganic particles.
[0060] The thickness of the heat-resistant layer is not particularly limited, but based on the thickness of the heat-resistant layer formed on one surface of the porous substrate, it can be 5% to 45% by length, or 10% to 30% by length of the thickness of the porous substrate, and can be, for example, 0.1 μm to 5 μm, 0.5 μm to 4 μm, 0.5 μm to 3 μm, or 1 μm to 2 μm. In this case, the heat-resistant layer can achieve excellent heat resistance and adhesion without reducing the air permeability of the separator.
[0061] Adhesive layer The adhesive layer is located on the aforementioned heat-resistant layer. When the heat-resistant layer is located on both surfaces of the porous substrate, the adhesive layer is also provided on both surfaces, and when the heat-resistant layer is located only on one surface of the porous substrate, the adhesive layer may be located only on one surface on which the heat-resistant layer is formed, or on both surfaces, that is, on the surface on which the heat-resistant layer is formed and on the surface on which the heat-resistant layer is not formed. The adhesive layer is located on the outermost surface of the separator and can be used to improve the adhesion between the electrode and the separator.
[0062] The adhesive layer according to the embodiment includes a second binder, the second binder includes a copolymer, the copolymer includes a first unit derived from a vinyl aromatic monomer, a second unit derived from an alkyl acrylate, and a third unit derived from a phosphonate monomer. Such a copolymer can also show excellent adhesion even at low temperature and low pressure, so that it can be used in battery types that are difficult to apply high temperature and high pressure processes, so that they have advantages in the process and even a very small amount can maximize the adhesion between the separator and the electrode plate, improve the heat resistance and adhesion of the separator, and ultimately improve the processability, high temperature cycle life characteristics, safety and reliability of the battery.
[0063] The first unit derived from the vinyl aromatic monomer may increase the adhesion of the adhesive layer and improve the dispersibility and processability of the adhesive layer composition.
[0064] [Chemical formula 1]
[0065] In Chemical Formula 1, R 1 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, L 1 is a substituted or unsubstituted C1 to C6 alkylene group, a substituted or unsubstituted C3 to C10 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, or a combination thereof, a is 0 or 1, * represents the portion of the carbon linked to the benzene ring, R 2is fluorine, substituted or unsubstituted C1 to C6 alkyl, substituted or unsubstituted C6 to C20 aryl, or substituted or unsubstituted C1 to C6 alkenyl, and b is an integer of 0 to 5.
[0066] For example, in Formula 1, R 1 It can be hydrogen or methyl, R 2 It can be fluorine, methyl or ethyl, and b can be 0 or 1.
[0067] The vinyl aromatic monomer may be, for example, styrene, α-methylstyrene, fluorostyrene, vinyltoluene, divinylbenzene, 1,1-diphenylethylene, or a combination thereof.
[0068] The second unit derived from an alkyl acrylate can help improve the adhesion of the adhesive layer and achieve appropriate air permeability and heat resistance. Here, the alkyl group can be an alkyl group having 1 to 20 carbon atoms (i.e., a C1 to C20 alkyl group), and the acrylate includes methacrylate and acrylate. For example, the second unit can be represented by Chemical Formula 2.
[0069] [Chemical formula 2]
[0070] In chemical formula 2, R 3 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, and R 4 It is a C1 to C20 alkyl group.
[0071] In chemical formula 2, R 4 It may be, for example, a C5 to C18 alkyl group or a C6 to C15 alkyl group. In this case, the second binder may achieve appropriate air permeability and heat resistance while exhibiting excellent adhesion under low temperature and low pressure conditions.
[0072] The third unit derived from the phosphonate monomer allows the second binder to achieve excellent adhesion under low temperature and low pressure conditions, and can help the second binder have an appropriate glass transition temperature and swelling degree, and even if a very small amount of the binder is used, excellent adhesion can be achieved and high heat resistance and air permeability can be achieved.
[0073] The phosphonate monomer refers to a monomer including a phosphonate group and a C=C double bond. The phosphonate group can be represented by -P(=O)(OR)(OR'), wherein R and R' are organic groups other than hydrogen. The third unit can be represented by Chemical Formula 3, for example.
[0074] [Chemical formula 3]
[0075] In chemical formula 3, R 5 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, L 2 is a carboxyl group (-C(=O)O-), a carbonyl group (-C(=O)-), an ether group (-O-), a substituted or unsubstituted C1 to C6 alkylene group, a substituted or unsubstituted C3 to C10 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, or a combination thereof, c is 0 or 1, R 6 and R 7 are the same as or different from each other, and are each independently a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.
[0076] As an example, in Chemical Formula 3, R 5 It can be hydrogen or methyl, L 2 can be a carboxyl group, a substituted or unsubstituted C1 to C6 alkylene group, or a combination thereof, and R 6 and R 7 May independently be a C1 to C6 alkyl group.
[0077] The phosphonate-based monomer may be, for example, acrylphosphonate, and in this case, the second binder may achieve excellent adhesion under low temperature and low pressure conditions even in a small amount and may exhibit excellent workability.
[0078] The third unit may be derived from, for example, an acrylphosphonate-based monomer, and may be represented by Chemical Formula 4.
[0079] [Chemical formula 4]
[0080] In chemical formula 4, R 5 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, L 3 is a substituted or unsubstituted C1 to C6 alkylene group, R 6 and R 7 are the same as or different from each other and are each independently a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group, and R 8 It is hydrogen or methyl.
[0081] As an example, the acrylphosphonate monomer may be dimethyl [(acryloxy) methyl] phosphonate, dimethyl [(acryloxy) ethyl] phosphonate, diethyl [(acryloxy) methyl] phosphonate, or diethyl [(acryloxy) ethyl] phosphonate, wherein the acryl group may be replaced by a methacryloyl group. If a third unit derived from such a monomer is included, the second binder may achieve excellent adhesion under low temperature and low pressure conditions even in a small amount, and may exhibit excellent processability.
[0082] In the second binder, the copolymer may include 40wt% to 80wt% of the first unit, 5wt% to 40wt% of the second unit, and 0.1wt% to 20wt% of the third unit. For example, the copolymer of the second binder may include 50wt% to 70wt% of the first unit, 10wt% to 30wt% of the second unit, and 5wt% to 20wt% of the third unit. The amount range of each unit is based on 100wt% of the copolymer. If each unit meets these amount ranges, the second binder can achieve excellent adhesion under low temperature and low pressure conditions even in a small amount without deteriorating the heat resistance and air permeability of the diaphragm, thereby improving processability, cycle life characteristics and safety.
[0083] The second binder may be in the form of particles, and may remain in the form of particles without dissolving in an aqueous solvent. In this case, the average particle size (D50) of the second binder may be 0.1 μm to 1 μm, for example, 0.2 μm to 0.9 μm, 0.2 μm to 0.8 μm, or 0.2 μm to 0.7 μm. When this particle size range is met, the adhesive layer can achieve excellent low-temperature and low-pressure adhesion even at a thin thickness without deteriorating the heat resistance and air permeability of the diaphragm. Here, the average particle size may refer to the diameter (D50) of particles measured by a particle size analyzer and having a cumulative volume of 50% by volume in the particle size distribution.
[0084] For example, the second binding agent can be in the form of particles with core-shell structure, in which case, it is conducive to ensuring appropriate average particle diameter and swelling degree. When the second binding agent has core-shell structure, the shell can be made of a copolymer comprising the aforementioned first unit, the second unit and the third unit. The material of the core is not particularly limited, and can be, for example, acrylic polymer, diene polymer or their copolymer.
[0085] The glass transition temperature of the second binder may be 60° C. to 90° C., for example, 65° C. to 75° C. When the second binder has a glass transition temperature within this range, it is advantageous to achieve adhesion under low temperature and low pressure conditions, and even a small amount may exhibit excellent adhesion without deteriorating the characteristics of the separator.
[0086] The swelling degree of the second binder of the adhesive layer may be 600% to 1000%, for example, 700% to 900%. If the second binder has a swelling degree in this range, excellent adhesion can be maintained during the battery manufacturing process and operation, and the adhesion between the separator and the negative electrode and the separator and the positive electrode can be improved. Here, the swelling degree may refer to the swelling degree after the second binder is left standing in an electrolyte at 60°C for 72 hours.
[0087] The thickness of the adhesive layer is not particularly limited, but based on the thickness of the adhesive layer formed on one surface of the porous substrate, it can be 1% to 15% of the thickness of the porous substrate, or 1% to 10% of the thickness of the porous substrate, and can be, for example, 0.05 μm to 3 μm, or 0.1 μm to 2 μm. The adhesive layer according to the embodiment has such a thin thickness that it does not deteriorate the performance of the separator, and despite the thin thickness, can exhibit excellent adhesion.
[0088] In an embodiment, a method for manufacturing a separator for a rechargeable lithium battery is provided, the method comprising: preparing a porous substrate; coating a heat-resistant layer composition comprising a first binder, inorganic particles and a solvent on at least one surface of the porous substrate; and coating an adhesive layer composition comprising a second binder and a solvent on the heat-resistant layer, and then drying it.
[0089] At this time, the loading amount of the adhesive layer composition can be, for example, 0.05 g / m 2 Up to 0.2g / m 2 , or 0.1g / m 2 Up to 0.2g / m 2 In this case, the adhesive layer can achieve excellent adhesion without deteriorating the characteristics of the separator.
[0090] In the method for manufacturing the diaphragm, the solvent of the heat-resistant layer composition and the solvent of the adhesive layer composition can be an aqueous solvent, and can be independently selected from water, an alcohol solvent and a combination thereof. The alcohol solvent can be, for example, methanol, ethanol, propanol, butanol or a combination thereof. These aqueous solvents are harmless to the body and have excellent drying properties, so that mass production can be achieved without reducing productivity.
[0091] The diaphragm according to the embodiment can achieve ultra-high heat resistance. For example, the dry shrinkage rate of the diaphragm can be less than or equal to 5%, and the dry shrinkage rate in both the horizontal direction and the vertical direction can be less than or equal to 4%, or less than or equal to 3%. Here, the dry shrinkage rate refers to the degree of shrinkage of the diaphragm after standing for 1 hour at 150°C.
[0092] In addition, the separator according to the embodiment can achieve excellent adhesion. For example, the wet adhesion of the separator may be greater than or equal to 0.10 gf / mm, greater than or equal to 0.15 gf / mm, or greater than or equal to 0.20 gf / mm. Generally, the adhesion between the separator and the negative electrode tends to be lower than the adhesion between the separator and the positive electrode, but the separator according to the embodiment can also achieve an adhesion of greater than or equal to 0.10 gf / mm to the negative electrode. Here, the wet adhesion may refer to the peeling force between the separator and the electrode measured after the electrolyte is injected into the battery case and left to stand for 2 hours at 40 ° C and a load of 50 kg.
[0093] In the separator, the heat-resistant layer and the adhesive layer may each independently have a single-layer structure or a multilayer structure. In the multilayer structure, layers selected from organic layers, inorganic layers, and organic / inorganic layers may be arbitrarily arranged. The multilayer structure may be a two-layer structure, a three-layer structure, or a four-layer structure, but is not necessarily limited to these structures, and may be selected according to the desired composite separator properties.
[0094] At the same time, when the heat-resistant layer and the adhesive layer are located on both surfaces of the porous substrate, the amount of the second binder in the adhesive layer on the negative electrode side in contact with the negative electrode may be greater than or equal to the amount of the second binder in the adhesive layer on the positive electrode side in contact with the positive electrode. For example, the amount of the second binder in the adhesive layer on the negative electrode side may be 1.5 times or more (e.g., 2 to 5 times, or 2 to 4 times) the amount of the second binder in the adhesive layer on the positive electrode side. In this case, by improving the problem that the adhesion between the diaphragm and the negative electrode is generally lower than the adhesion between the diaphragm and the positive electrode, the loss or deterioration of the adhesion at the diaphragm-negative electrode interface caused by repeated charge and discharge is suppressed, lithium salt precipitation is prevented, and the safety of the battery is improved.
[0095] Rechargeable lithium battery In an embodiment, a rechargeable lithium battery includes a positive electrode, a negative electrode, the aforementioned separator between the positive electrode and the negative electrode, and an electrolyte.
[0096] Figure 1 is a schematic diagram showing a rechargeable lithium battery according to an embodiment. Figure 1 According to an embodiment, a rechargeable lithium battery 100 includes a battery cell, a battery case 120 accommodating the battery cell, and a sealing member 140 sealing the battery case 120, the battery cell including a positive electrode 114, a negative electrode 112 facing the positive electrode 114, a separator 113 between the positive electrode 114 and the negative electrode 112, and an electrolyte impregnating the positive electrode 114, the negative electrode 112 and the separator 113.
[0097] Positive electrode The positive electrode 114 includes a current collector and a positive electrode active material layer on the current collector, and the positive electrode active material layer includes a positive electrode active material and may optionally include a binder and / or a conductive material. Here, the current collector may be, for example, aluminum foil, but is not limited thereto.
[0098] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions. Examples of the positive electrode active material include a compound represented by any one of the following chemical formulas: Li a A 1-b X b D2 (0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T2 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li aNi 1-b-c Mr b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α≤2); Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2); Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2); Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1); Li a Ni b Co c Mr d G e O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8,0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8,0.001≤b≤0.1); Li a Mr 1-b G b O2(0.90≤a≤1.8,0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8,0.001≤b≤0.1); Li a Mr 1-g G g PO4(0.90≤a≤1.8,0≤g≤0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3 (0≤f≤2); Li a FePO4 (0.90≤a≤1.8).
[0099] In the above chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; and J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0100] The positive electrode active material may be a lithium-metal composite oxide, for example, lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium nickel cobalt oxide (LNCO), lithium nickel cobalt aluminum oxide (LNCAO), lithium nickel cobalt manganese oxide (LNCMO), lithium manganese oxide (LMO), or lithium iron phosphate (LFP).
[0101] A compound having a coating layer on the surface may be used, or a mixture of the above-mentioned compound and a compound having a coating layer may be used. The coating layer may include at least one coating element compound selected from an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound forming the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a combination thereof. As an example, the coating layer may include Li2O-ZrO2 (LZO). The coating layer formation process may use a method that does not adversely affect the physical properties of the positive electrode active material, such as a spraying method, an impregnation method, and the like.
[0102] The positive electrode active material may include, for example, one or more types of lithium-metal composite oxides represented by Chemical Formula 11.
[0103] [Chemical formula 11] Li a M 11 1-y11-z11 M 12 y11 M 13 z11 O2 In Chemical Formula 11, 0.9≤a≤1.8, 0≤y11≤1, 0≤z11≤1, 0≤y11+z11<1, and M 11 、M 12 and M 13 Independently any one selected from elements such as Ni, Co, Mn, Al, Mg, Ti or Fe, and combinations thereof.
[0104] For example, M 11 It can be Ni, and M 12 and M 13 Mn, Al, Mg, Ti or Fe may be independently a metal such as Co, Mn, Al, Mg, Ti or Fe. 11 Can be Ni, M 12 It can be Co, M 13 It may be Mn or Al, but is not limited thereto.
[0105] In an embodiment, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula 12.
[0106] [Chemical formula 12] Li a12 Ni x12 M 14 y12 M 15 1-x12-y12 O2 In Chemical Formula 12, 0.9≤a12≤1.8, 0.3≤x12≤1, 0≤y12≤0.7, and M 14 and M 15 Independently, it is at least one element selected from Al, B, Ba, Ca, Ce, Co, Cr, F, Fe, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W and Zr.
[0107] In Chemical Formula 12, 0.3 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.7, 0.4 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.6, 0.5 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.5, 0.6 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.4, 0.7 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.3, 0.8 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.2, or 0.9 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.1.
[0108] For example, the positive electrode active material may include a lithium nickel cobalt-based oxide represented by Chemical Formula 13.
[0109] [Chemical Formula 13] Li a13 Ni x13 Co y13 M 16 1-x13-y13 O2 In Chemical Formula 13, 0.9 ≤ a13 ≤ 1.8, 0.3 ≤ x13 < 1, 0 < y13 ≤ 0.7, and M 16 is at least one element selected from Al, B, Ba, Ca, Ce, Cr, F, Fe, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W, and Zr.
[0110] In Chemical Formula 13, 0.3 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.7, 0.4 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.6, 0.5 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.5, 0.6 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.4, 0.7 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.3, 0.8 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.2, or 0.9 ≤ x13 ≤ 0.99 and 0.01 ≤ y13 ≤ 0.1.
[0111] Based on the total amount of metals other than lithium, the nickel content in the lithium nickel composite oxide may be greater than or equal to 30 mol%, for example, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol%, or greater than or equal to 90 mol%, and may be less than or equal to 99.9 mol% or less than or equal to 99 mol%.
[0112] As an example, the lithium-nickel composite oxide may be a high-nickel oxide, which includes greater than or equal to 80 mol% or greater than or equal to 90 mol% nickel based on the total amount of metals other than lithium. In this case, there is the advantage of achieving high capacity and high output characteristics, but there is a problem of generating a large amount of gas during battery operation. At this time, the generated gas is located at the interface between the electrode and the diaphragm, causing the precipitation of lithium salts, which can cause a sharp drop in capacity or short circuit and fire. In order to solve this problem, when the diaphragm according to the embodiment is applied, the heat resistance is improved and the adhesion between the diaphragm and the electrode is enhanced, thereby effectively suppressing the precipitation of lithium salts, thereby effectively improving the safety and cycle life characteristics of the battery.
[0113] When a positive electrode using a high-nickel positive electrode active material is combined with a separator according to an embodiment and a battery type that is difficult to apply high temperature and high pressure processes is applied, the effect of the embodiment can be maximized, that is, the effect of improving the heat resistance, safety, processability and cycle life characteristics of the battery.
[0114] The average particle size (D50) of the positive electrode active material may be 1 μm to 25 μm, for example, 4 μm to 25 μm, 5 μm to 20 μm, 8 μm to 20 μm, or 10 μm to 18 μm. The positive electrode active material having a particle size within the range may be mixed in coordination with other components in the positive electrode active material layer and achieve high capacity and high energy density. The average particle size may refer to the diameter (D50) of particles having a cumulative volume of 50% by volume in a particle size distribution as measured by a particle size analyzer.
[0115] The positive electrode active material may be in the form of secondary particles formed by agglomeration of a plurality of primary particles or in the form of a single particle. In addition, the positive electrode active material may have a spherical shape, a shape close to a spherical shape, a polyhedral shape, or an irregular shape.
[0116] The content of the positive electrode active material may be 55 wt % to 99.7 wt %, for example, 74 wt % to 89.8 wt %, based on the total weight of the positive electrode active material layer. Within the above range, the capacity of the rechargeable lithium battery may be maximized and cycle life characteristics may be improved.
[0117] The binder improves the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples thereof may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0118] The amount of the binder in the positive electrode active material layer may be 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.
[0119] A conductive material is included to provide electrode conductivity, and any conductive material can be used as the conductive material unless it causes a chemical change. Examples of conductive materials include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metal-based materials including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof. The amount of the conductive material in the positive electrode active material layer may be 1 wt% to 5 wt% based on the total weight of the positive electrode active material layer.
[0120] Negative electrode A negative electrode for a rechargeable lithium battery includes a current collector and a negative electrode active material layer positioned on the current collector. The negative electrode active material layer includes a negative electrode active material and may further include a binder and / or a conductive material.
[0121] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, or a transition metal oxide.
[0122] The material that reversibly intercalates / deintercalates lithium ions may include, for example, crystalline carbon, amorphous carbon, or a combination thereof as a carbonaceous negative electrode active material. The crystalline carbon may be a non-shaped, or flake, flaky, spherical, or fibrous natural graphite or artificial graphite. The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonization product, calcined coke, etc.
[0123] Lithium metal alloys include alloys of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0124] The material capable of being doped / dedoped with lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may include silicon, silicon-carbon composites, SiO xwhere \(0 \lt x \lt 2\), a Si-Q alloy (where Q is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, Group 15 element, Group 16 element, transition metal, rare earth element, or a combination thereof, but not Si), and the Sn-based negative electrode active material may include Sn, \(SnO_2\), a Sn-R alloy (where R is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, Group 15 element, Group 16 element, transition metal, rare earth element, or a combination thereof, but not Sn). At least one of these materials may be mixed with \(SiO_2\). The elements Q and R may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0125] The silicon-carbon composite may be, for example, a silicon-carbon composite including a core containing crystalline carbon and silicon particles and an amorphous carbon coating layer provided on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon precursor may be coal tar pitch, mesophase pitch, petroleum pitch, coal oil, petroleum heavy oil, or a polymer resin (such as phenolic resin, furan resin, or polyimide resin). In this case, based on the total weight of the silicon-carbon composite, the content of silicon may be 10 wt% to 50 wt%. Additionally, based on the total weight of the silicon-carbon composite, the content of crystalline carbon may be 10 wt% to 70 wt%, and based on the total weight of the silicon-carbon composite, the content of amorphous carbon may be 20 wt% to 40 wt%. Additionally, the thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D50) of the silicon particles may be 10 nm to 20 μm. The average particle size (D50) of the silicon particles may preferably be 10 nm to 200 nm. The silicon particles may be present in an oxidized form, and in this case, the atomic content ratio of Si:O in the silicon particles indicating the degree of oxidation may be 99:1 to 33:67. The silicon particles may be \(SiO_x\) x particles, and in this case, the range of x in \(SiO_x\) x may be greater than 0 and less than 2.
[0126] The Si-based negative electrode active material or the Sn-based negative electrode active material may be mixed with a carbon-based negative electrode active material. When the Si-based negative electrode active material or the Sn-based negative electrode active material is mixed and used with the carbon-based negative electrode active material, the mixing ratio may be a weight ratio of 1:99 to 90:10.
[0127] In the negative electrode active material layer, the negative electrode active material may be included in an amount of 95 wt % to 99 wt % based on the total weight of the negative electrode active material layer.
[0128] In an embodiment, the negative electrode active material layer further includes a binder and optionally may further include a conductive material. Based on the total weight of the negative electrode active material layer, the amount of the binder in the negative electrode active material layer may be 1wt% to 5wt%. In addition, when a conductive material is further included, the negative electrode active material layer may include 90wt% to 98wt% of the negative electrode active material, 1wt% to 5wt% of the binder, and 1wt% to 5wt% of the conductive material.
[0129] The binder is used to adhere the negative electrode active material particles to each other well, and also to adhere the negative electrode active material to the current collector. The binder may be a non-water-soluble binder, a water-soluble binder, or a combination thereof.
[0130] The non-water-soluble binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, ethylene propylene copolymers, polystyrene, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0131] The water-soluble binder can include a rubber binder or a polymer resin binder. The rubber binder can be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and a combination thereof. The polymer resin binder can be selected from polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and a combination thereof.
[0132] When a water-soluble binder is used as a negative electrode binder, a cellulose compound capable of imparting viscosity may be further included. As a cellulose compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose and their alkali metal salts may be mixed and used. The alkali metal may be Na, K or Li. Based on 100 parts by weight of the negative electrode active material, the amount of such a thickener may be 0.1 parts by weight to 3 parts by weight.
[0133] A conductive material is included to provide electrode conductivity, and any conductive material can be used as the conductive material unless it causes a chemical change. Examples of the conductive material include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metal-based materials including metal powder or metal fiber of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0134] The current collector of the negative electrode may include one selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0135] Electrolyte The electrolyte includes a non-aqueous organic solvent and a lithium salt.
[0136] The non-aqueous organic solvent is used as a medium for transporting ions involved in the electrochemical reaction of the battery. The non-aqueous organic solvent may be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent or an alcohol solvent, or an aprotic solvent. Examples of carbonate solvents include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Examples of ester solvents include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolactone, valerolactone, mevalonolactone, caprolactone, etc. The ether solvent may be dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., and the ketone solvent may be cyclohexanone, etc. In addition, the alcohol solvent can be ethanol, isopropanol, etc., and the aprotic solvent can be: nitrile, such as R-CN (wherein R is a C2 to C20 straight chain, branched or cyclic hydrocarbon group, and can include a double bond, an aromatic ring or an ether bond); amide, such as dimethylformamide; dioxolane, such as 1,3-dioxolane; cyclopentane; etc.
[0137] The nonaqueous organic solvent may be used alone or in a mixture, and when the organic solvent is used in a mixture, the mixing ratio may be controlled according to desired battery performance.
[0138] In addition, in the case of carbonate solvents, a mixture of cyclic carbonate and chain carbonate can be used. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the electrolyte can show excellent performance.
[0139] The non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of about 1:1 to about 30:1.
[0140] As the aromatic hydrocarbon solvent, an aromatic hydrocarbon compound represented by Chemical Formula I may be used.
[0141] [Chemical Formula I]
[0142] In Formula I, R 4 To R 9 are the same or different and are selected from hydrogen, halogen, C1 to C10 alkyl, C1 to C10 haloalkyl, and combinations thereof.
[0143] Specific examples of aromatic hydrocarbon solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene and combinations thereof.
[0144] The electrolyte may further include vinylene carbonate or ethylene carbonate compounds of Chemical Formula II to improve the cycle life of the battery.
[0145] [Chemical Formula II]
[0146] In Chemical Formula II, R 10 and R 11 are the same or different and are selected from hydrogen, halogen, cyano, nitro and fluorinated C1 to C5 alkyl, provided that R 10 and R 11 At least one of them is selected from halogen, cyano, nitro and fluorinated C1 to C5 alkyl, but R 10 and R 11 Both are not hydrogen.
[0147] Examples of ethylene carbonate compounds may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the additive for improving the cycle life may be used within an appropriate range.
[0148] The lithium salt dissolved in the nonaqueous organic solvent supplies lithium ions in the battery, enables basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode.
[0149] Examples of lithium salts include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers, for example, integers from 1 to 20), at least one of lithium difluoro(bis(oxalato)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato)borate; LiBOB) and lithium difluoro(oxalato)borate (LiDFOB).
[0150] The lithium salt may be used in a concentration range of 0.1 M to 2.0 M. If the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0151] Rechargeable lithium batteries can be classified as lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries, depending on the presence of a separator and the type of electrolyte used in the battery. Rechargeable lithium batteries can have a variety of shapes and sizes, and include cylindrical, prismatic, coin, or pouch-type batteries, and can be thin film batteries or can be quite bulky in size. The structure and manufacturing methods of lithium ion batteries pertaining to the present disclosure are well known in the art.
[0152] Since the rechargeable lithium battery according to the embodiment achieves high capacity and has excellent storage stability at high temperature, cycle life characteristics, and high rate characteristics, it can be used in electric vehicles (EVs), hybrid electric vehicles (such as plug-in hybrid electric vehicles (PHEVs)), and portable electronic devices.
[0153] Hereinafter, examples and comparative examples of the present invention are described. However, it will be understood that the examples are for illustrative purposes and are not to be construed as limiting the present invention.
[0154] Example 1 1. Manufacturing of diaphragm (1) Preparation of the first binder for the heat-resistant layer Distilled water (6361 g), acrylic acid (72.06 g, 1.0 mol), acrylamide (604.1 g, 8.5 mol), potassium persulfate (2.7 g, 0.01 mol), 2-acrylamido-2-methylpropanesulfonic acid (103.6 g, 0.5 mol) and 5N lithium hydroxide aqueous solution (1.05 equivalents based on the total amount of 2-acrylamido-2-methylpropanesulfonic acid) were placed in a 10L four-necked flask equipped with a stirrer, a thermometer and a condenser, and the internal pressure of the flask was reduced to 10 mmHg with a diaphragm pump, and then, restored to normal pressure with nitrogen, and repeated three times. The reaction solution was controlled to be stable between 65°C and 70°C for 12 hours. The reaction solution was cooled to room temperature and the reaction solution was adjusted to a pH range of 7 to 8 by using a 25% ammonia solution. In this manner, poly(acrylamide-co-2-acrylamide-2-methylpropanesulfonic acid-co-acrylic acid) lithium salt having a molar ratio of acrylamide, 2-acrylamide-2-methylpropanesulfonic acid and acrylic acid of 85:5:10 was prepared to prepare a first binder.
[0155] (2) Formation of heat-resistant layer A heat-resistant layer composition was prepared by mixing the prepared first binder and inorganic particles (boehmite, D50 = 0.3 μm) in an aqueous solvent at a weight ratio of 1:30. The prepared heat-resistant layer composition was coated on both surfaces of an 8 μm thick polyethylene porous substrate (SK Co., air permeability: 120 sec / 100 cc, puncture strength: 480 kgf) by bar coating so that the thickness of each surface was 1.5 μm, and dried.
[0156] (3) Formation of adhesive layer A second binder having a core-shell structure, an average particle size (D50) of 0.5 μm, a glass transition temperature of 65°C, and a swelling degree of 800% was prepared. In the second binder, the core includes a copolymer of an alkyl acrylate and divinylbenzene, and the shell includes a copolymer of 70 wt% styrene, 20 wt% 2-ethylhexyl methacrylate, and 10 wt% acrylphosphonate. An adhesive layer composition was prepared by dispersing the second binder in an aqueous solvent. The adhesive layer composition was coated on the surface of the heat-resistant layer using a rod coating method so that the thickness of each surface was 0.5 μm, and dried, and the loading amount of the adhesive layer composition was set to 0.1 g / m2 .
[0157] Thus, a coated separator having a total thickness of approximately 12 μm was produced.
[0158] 2. Manufacturing of battery cells 96wt% LiNi 0.91 Co 0.05 Al 0.04 An O2 positive electrode active material, 2 wt% of a polyvinylidene fluoride binder, 2 wt% of a carbon nanotube conductive material and an N-methylpyrrolidone solvent were mixed with a mixer to prepare a positive electrode active material layer composition, and the positive electrode active material layer composition was coated on an aluminum foil, and then dried and rolled to manufacture a positive electrode.
[0159] 97 wt % of graphite, 1.5 wt % of styrene butadiene rubber binder, 1.5 wt % of carboxymethyl cellulose and distilled water solvent were mixed to prepare a negative electrode active material layer composition, and the negative electrode active material layer composition was coated on a copper current collector, then dried and pressed to manufacture a negative electrode.
[0160] The coin cell was fabricated by placing the prepared coated separator between the positive electrode and the negative electrode, inserting it into a case, and then injecting an electrolyte solution, which was a solution of 1.1 M LiPF6 dissolved in a solvent mixed with ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:5.
[0161] Example 2 In addition to setting the loading amount of the adhesive layer composition when forming the adhesive layer to 0.15 g / m 2 A separator and a battery cell were manufactured in the same manner as in Example 1 except for the above.
[0162] Example 3 In addition to setting the loading amount of the adhesive layer composition to 0.20 g / m 2 A separator and a battery cell were manufactured in the same manner as in Example 1 except for the above.
[0163] Example 4 A separator and a battery cell were manufactured in the same manner as in Example 1, except that a binder having a core-shell structure in which a shell was made of styrene-co-2-ethylhexyl methacrylate-co-acryloylphosphonate copolymer, an average particle size (D50) of 0.5 μm, a glass transition temperature of 75° C., and a swelling degree of 800% was used as the second binder of the adhesive layer.
[0164] Example 5 In addition to setting the loading amount of the adhesive layer composition when forming the adhesive layer to 0.15 g / m 2 A separator and a battery cell were manufactured in the same manner as in Example 4 except for the above.
[0165] Example 6 In addition to setting the loading amount of the adhesive layer composition to 0.20 g / m 2 A separator and a battery cell were manufactured in the same manner as in Example 4 except for the above.
[0166] Comparative Example 1 A separator and a battery cell were manufactured in the same manner as in Example 3, except that polyvinylidene fluoride (PVdF) was used as the second binder of the adhesive layer.
[0167] Comparative Example 2 A separator and a battery cell were manufactured in the same manner as in Example 3, except that a binder having a core-shell structure in which the shell is made of styrene-co-2-ethylhexyl methacrylate-co-acrylonitrile copolymer and having a glass transition temperature of 65° C. and a swelling degree of 800% was used as the second binder of the adhesive layer.
[0168] Comparison Example 3 A separator and a battery cell were manufactured in the same manner as in Example 3, except that a binder having a core-shell structure in which a shell was made of styrene-co-butyl acrylate-co-acrylonitrile copolymer and having a glass transition temperature of 55° C. and a swelling degree of 400% was used as the second binder of the adhesive layer.
[0169] Comparison Example 4 A separator and a battery cell were manufactured in the same manner as in Example 3, except that a binder having a core-shell structure in which a shell is made of styrene-co-butyl acrylate-co-acrylonitrile copolymer and having a glass transition temperature of 60° C. and a swelling degree of 300% was used as the second binder of the adhesive layer.
[0170] Evaluation Example 1: Evaluation of Dry Shrinkage of Separator The coated separators prepared in Examples and Comparative Examples were cut into a size of (8 cm) × (8 cm) and placed in a convection oven at 150°C for 1 hour, and then the length change rates in the machine direction (MD) and transverse direction (TD) of the coated separators were calculated. The results are shown in Table 1.
[0171] Referring to Table 1, the separators of Examples 1 to 6 showed a very low drying shrinkage of 2.3% or less at high temperatures, demonstrating excellent heat resistance.
[0172] Evaluation Example 2: Evaluation of wet adhesion of separator The battery cells manufactured in the examples and comparative examples were kept at a temperature of 40°C and a load of 50kg for 2 hours, and then a peeling test was performed as follows. After separating the separator from the positive electrode by about 15mm and then fixing the positive electrode to the lower clamp and the separator to the upper clamp, the two clamps were pulled apart in the 180° direction, and the positive electrode and the separator were peeled off at 100mm / min. The force required to peel off 40mm was measured three times and the arithmetic mean was obtained. The peeling test for the separator and the negative electrode was also performed in the same manner, and the results are shown in Table 1.
[0173] Referring to Table 1, in Comparative Examples 1 to 4, the peel strength between the separator and the negative electrode is at a very low level of 0.05 gf / mm, and the bonding strength is very low, while in Examples 1 to 6, it can be seen that the peel strength between the separator and the positive electrode and the peel strength between the separator and the negative electrode are both very high, at 0.1 gf / mm or more, showing excellent adhesion.
[0174] Evaluation Example 3: Evaluation of High-Temperature Cycle Life Characteristics of Battery Cells The battery cells of the examples and comparative examples were charged at 55°C at a constant current of 0.1C to an upper voltage of 4.25V, and then discharged at a constant current of 0.1C until the cut-off discharge voltage was 3.5V to perform initial charge and discharge. Then, charging at 0.5C and discharging at 0.5C were repeated 10 times in the voltage range of 3.5V to 4.25V. The battery temperature was measured after 10 cycles, and the degree of increase compared to the initial temperature was measured and shown in Table 1. In addition, the ratio of the discharge capacity of the 10th cycle to the initial discharge capacity was calculated and shown in Table 1 as efficiency.
[0175] Referring to Table 1, for the battery cells of Comparative Examples 1 to 4, the temperature change was as large as 12°C or more, however, for the battery cells of Examples 1 to 6, the temperature change was as low as 7.5°C or less, confirming that heat generation during battery operation was suppressed. In addition, in the case of the battery cells of Comparative Examples 1 to 4, the capacity retention rate at 10 cycles was 84% or less, while in the case of the battery cells of Examples 1 to 6, the capacity retention rate was as high as 94% or more, indicating that high temperature cycle life characteristics were improved.
[0176] (Table 1)
[0177] Evaluation Example 4: Evaluation of Heat Generation during Cycle of Battery Cells The battery cells of Comparative Example 1 and Example 1 were cycled in the same manner as in Evaluation Example 3, and the temperature inside the battery cells was measured, and the results are shown in FIG. Figure 2and Figure 3 middle. Figure 2 is the result of Comparative Example 1, and Figure 3 This is the result of Example 1.
[0178] Reference Figure 2 The gray curve of temperature is shown in FIG. 1 , and the temperature inside the battery cell exceeds 65° C. during the initial operation of the battery cell, indicating a heating phenomenon. Figure 3 , the battery cells will not overheat during operation.
[0179] Evaluation Example 5: Evaluation of initial charge / discharge efficiency The battery cells of Comparative Example 1 and Example 1 were charged at a constant current of 0.1C to an upper voltage limit of 4.25V at room temperature (25°C), and then discharged at a constant current of 0.1C until the discharge cutoff voltage was 3.5V to perform initial charge and discharge. Then, charging at 0.5C and discharging at 0.5C were repeated 10 times in the voltage range of 3.5V to 4.25V. The charge capacity, discharge capacity, and efficiency as a ratio of discharge capacity to charge capacity of 10 cycles were measured, and the results are shown in Figure 4 and Figure 5 middle. Figure 4 The results of Comparative Example 1 are shown. Figure 5 The results of Example 1 are shown.
[0180] Reference Figure 4 In the case of the battery cell of Comparative Example 1, the initial charge and discharge efficiency is reduced. Figure 5 , compared with Comparative Example 1, the initial charge and discharge efficiency of the battery cell of Example 1 is improved.
[0181] Although the preferred embodiment has been described in detail above, the scope of the present invention is not limited thereto. In addition, various modifications and improvements made by those skilled in the art using the basic concept defined in the claims should also be understood to fall within the scope of the present invention.
[0182] [Explanation of Symbols] 100: Rechargeable lithium battery 112: Negative electrode 113: Diaphragm 114: Positive electrode 120: Battery housing 140: Sealing member.
Claims
1. A separator for a rechargeable lithium battery, the separator for a rechargeable lithium battery comprising: porous substrate, a heat-resistant layer on at least one surface of the porous substrate; as well as an adhesive layer, on the heat-resistant layer, Wherein, the heat-resistant layer comprises a first binder and inorganic particles, The first binder comprises at least one selected from polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl alcohol, polysulfonic acid, polyacrylamide, polyamide, polyurea, polyurethane and copolymers thereof, The adhesive layer includes a second adhesive, and The second binder includes a copolymer including a first unit derived from a vinyl aromatic monomer, a second unit derived from an alkyl acrylate, and a third unit derived from a phosphonate-based monomer.
2. The separator for a rechargeable lithium battery according to claim 1, wherein In the heat-resistant layer, the first binder includes a copolymer including a first unit derived from (meth)acrylamide, a second unit derived from a monomer including a sulfonic acid group, and a third unit derived from (meth)acrylic acid, (meth)acrylate, a monomer including a nitrile group, a monomer including an alcohol group, or a combination thereof.
3. The separator for a rechargeable lithium battery according to claim 2, wherein: In the first binder of the heat-resistant layer, the copolymer includes 55 mol % to 99 mol % of the first unit, 0.5 mol % to 40 mol % of the second unit, and 0.5 mol % to 40 mol % of the third unit.
4. The separator for a rechargeable lithium battery according to claim 3, wherein: In the first binder of the heat-resistant layer, the copolymer includes 75 mol % to 94 mol % of the first unit, 1 mol % to 10 mol % of the second unit, and 5 mol % to 15 mol % of the third unit.
5. The separator for a rechargeable lithium battery according to claim 1, wherein In the heat-resistant layer, a weight ratio of the first binder to the inorganic particles is 1:20 to 1:
40.
6. The separator for a rechargeable lithium battery according to claim 1, wherein The average particle size D50 of the inorganic particles is 0.1 μm to 2 μm.
7. The separator for a rechargeable lithium battery according to claim 1, wherein The thickness of the heat-resistant layer is 0.1 μm to 5 μm.
8. The separator for a rechargeable lithium battery according to claim 1, wherein The first unit in the second binder of the adhesive layer is represented by Chemical Formula 1: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, L 1 is a substituted or unsubstituted C1 to C6 alkylene group, a substituted or unsubstituted C3 to C10 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, or a combination thereof, a is 0 or 1, * represents the portion of the carbon linked to the benzene ring, R 2 is fluorine, substituted or unsubstituted C1 to C6 alkyl, substituted or unsubstituted C6 to C20 aryl, or substituted or unsubstituted C1 to C6 alkenyl, and b is an integer of 0 to 5.
9. The separator for a rechargeable lithium battery according to claim 1, wherein In the first unit of the second binder of the adhesive layer, the vinyl aromatic monomer is styrene, α-methylstyrene, fluorostyrene, vinyltoluene, divinylbenzene, 1,1-diphenylethylene, or a combination thereof.
10. The separator for a rechargeable lithium battery according to claim 1, wherein In the second binder of the adhesive layer, the second unit is represented by Chemical Formula 2: [Chemical formula 2] In the chemical formula 2, R 3 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, and R 4 It is a C1 to C20 alkyl group.
11. The separator for a rechargeable lithium battery according to claim 1, wherein In the second binder of the adhesive layer, the third unit is represented by Chemical Formula 3: [Chemical formula 3] In the chemical formula 3, R 5 is hydrogen, fluorine, substituted or unsubstituted C1 to C6 alkyl, or substituted or unsubstituted C6 to C20 aryl, L 2 is carboxyl -C(=O)O-, carbonyl -C(=O)-, ether -O-, substituted or unsubstituted C1 to C6 alkylene, substituted or unsubstituted C3 to C10 cycloalkylene, substituted or unsubstituted C6 to C20 arylene, or a combination thereof, c is 0 or 1, and R 6 and R 7 are the same as or different from each other, and are each independently a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.
12. The separator for a rechargeable lithium battery according to claim 1, wherein In the third unit of the second binder of the adhesive layer, the phosphonate monomer is acrylphosphonate.
13. The separator for a rechargeable lithium battery according to claim 1, wherein In the second binder of the adhesive layer, the copolymer includes 40 wt % to 80 wt % of the first unit, 5 wt % to 40 wt % of the second unit, and 0.1 wt % to 20 wt % of the third unit.
14. The separator for a rechargeable lithium battery according to claim 1, wherein The second binder of the adhesive layer is in the form of particles and has an average particle size D50 of 0.1 μm to 1 μm.
15. The separator for a rechargeable lithium battery according to claim 1, wherein The second binder of the adhesive layer is in the form of particles having a core-shell structure, and the shell includes the copolymer including the first unit derived from the vinyl aromatic monomer, the second unit derived from the alkyl acrylate, and the third unit derived from the phosphonate monomer.
16. The separator for a rechargeable lithium battery according to claim 1, wherein The second binder of the adhesive layer has a glass transition temperature of 60°C to 90°C.
17. The separator for a rechargeable lithium battery according to claim 1, wherein The swelling degree of the second binder of the adhesive layer is 600% to 1000%, and the swelling degree means the swelling degree of the second binder after being left to stand in an electrolyte at 60° C. for 72 hours.
18. The separator for a rechargeable lithium battery according to claim 1, wherein The thickness of the adhesive layer is 0.05 μm to 3 μm.
19. The separator for a rechargeable lithium battery according to claim 1, wherein The heat-resistant layer and the adhesive layer are located on both surfaces of the porous substrate, and the amount of the second binder in the adhesive layer on the negative electrode side in contact with the negative electrode is greater than or equal to the amount of the second binder in the adhesive layer on the positive electrode side in contact with the positive electrode.
20. A rechargeable lithium battery, comprising: Positive electrode; Negative electrode; The separator according to any one of claims 1 to 19, between the positive electrode and the negative electrode; as well as Electrolyte.
21. The rechargeable lithium battery according to claim 20, wherein: The positive electrode includes a positive electrode active material including a lithium nickel-based composite oxide having a nickel content ratio of greater than or equal to 90 mol % relative to a total content of metals excluding lithium.