Method for preparing battery-grade metal salt solution by taking waste ternary lithium battery as raw material

By using HPB119 boron removal resin and acidic alkaline treatment, boron ions in ternary lithium batteries are efficiently removed, solving the problem of boron affecting the purity of metal salt solutions, and achieving efficient and economical preparation of battery-grade metal salt solutions.

CN118925284APending Publication Date: 2024-11-12ZHEJIANG TIANNENG NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410992947.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing ternary lithium-ion battery recycling process, boron is difficult to effectively remove, affecting the purity of the metal salt solution, and the existing methods are complex and uneconomical.

Method used

The boron-containing metal salt solution is adsorbed and removed by HPB119 type boron removal resin. Through wet treatment and resin column adsorption process, combined with acidic and alkaline desorption and regeneration, it can effectively remove boron ions and prepare battery-grade metal salt solution. .

Benefits of technology

It achieves high boron removal efficiency and easy operation, and reduces the boron content to ≤2mg/L, ensuring high purity of the metal salt solution, and the resin can be reused, reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of recycling treatment of waste lithium ion batteries, in particular to a method for preparing a battery-grade nickel / cobalt solution by taking waste ternary lithium batteries as raw materials. The method provided by the invention comprises the following steps: carrying out wet treatment on the waste ternary lithium battery positive electrode material to obtain a boron-containing metal salt solution; the boron content in the boron-containing metal salt solution is 0.01 to 0.05 g / L; metal elements in the boron-containing metal salt solution comprise one or more of nickel, cobalt and manganese; carrying out adsorption boron removal on the boron-containing metal salt solution by adopting boron removal resin to obtain a battery-grade metal salt solution; metal elements in the battery-grade metal salt solution comprise one or more of nickel, cobalt and manganese; and the model of the boron removal resin is HPB119. The boron ions in the solution can be effectively removed through the resin boron removal method, meanwhile, the method has high adsorption performance, the treatment capacity is large, operation is easy, convenient and efficient, and new impurities cannot be introduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycling and processing waste lithium-ion batteries, and in particular to a method for preparing a battery-grade metal salt solution using waste ternary lithium batteries as raw materials. Background Art

[0002] With the rapid development of the new energy vehicle industry, the demand for power batteries continues to grow, and the production and use of lithium-ion batteries, as the mainstream type of power batteries, have also shown explosive growth. However, the service life of lithium-ion batteries is limited, and the treatment and recycling of a large number of retired batteries has become an urgent problem to be solved.

[0003] Waste lithium-ion batteries contain a large amount of valuable metals, such as nickel, cobalt, manganese, etc. These metals have important application value in battery manufacturing. Therefore, recycling waste lithium-ion batteries can not only achieve the recycling of resources, but also reduce the exploitation of primary resources, which has important economic and environmental significance. However, in order to improve the life, capacity and safety performance of positive electrode materials, some ternary positive electrode material manufacturers on the market often dope positive electrode materials. Boron, as a low-cost non-metallic element, is often used to modify positive electrode materials. Boron doping can reduce the surface energy of the crystal surface of the precursor material, thereby promoting the directional growth of the grains and forming needle-shaped primary particles. When the internal needle-shaped primary particles are radially distributed, a continuous lithium ion transmission channel can be formed in the radial direction. During the cycle, this structure can reduce the unevenness of the charge distribution inside the secondary particles, which is conducive to weakening stress accumulation, reducing microcracks, and improving the charge and discharge cycle stability of the positive electrode material; at the same time, boron doping can refine the primary particles, help form a radial microstructure, reduce stress accumulation, and effectively inhibit the generation of microcracks, so that the positive electrode material has good rate performance and cycle performance.

[0004] At present, the mainstream process for recycling ternary waste lithium-ion batteries is to leach the battery black powder into a mixed metal salt solution, then separate it through a variety of extractants, and purify it step by step into high-purity nickel salt solution, cobalt salt solution, manganese salt solution and other raw materials. After being leached in the leaching process, boron enters the extraction process. In the extraction process, most of the boron will enter the raffinate, and a small amount will enter the stripping solution, affecting the purity of the mixed metal salt solution. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a battery-grade metal salt solution using waste ternary lithium batteries as raw materials. The method has the advantages of high boron removal efficiency and simple operation, and can effectively prepare a battery-grade metal salt solution.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a battery-grade metal salt solution using waste ternary lithium battery positive electrode materials as raw materials, comprising the following steps:

[0008] Wet-processing the waste ternary lithium battery positive electrode material to obtain a boron-containing metal salt solution; the boron content in the boron-containing metal salt solution is 0.01 to 0.05 g / L; the metal element in the boron-containing metal salt solution includes one or more of nickel, cobalt and manganese;

[0009] Adsorbing and removing boron from the boron-containing metal salt solution using a boron removal resin to obtain a battery-grade metal salt solution; the metal elements in the battery-grade metal salt solution include one or more of nickel, cobalt and manganese;

[0010] The model of the boron removal resin is HPB119.

[0011] Preferably, the wet treatment includes crushing, screening, leaching, extracting, degreasing and fine filtering the waste ternary lithium battery positive electrode material in sequence.

[0012] Preferably, the adsorption is performed by passing the boron-containing metal salt solution into a resin column filled with the boron-removing resin.

[0013] Preferably, the flow rate of the boron-containing metal salt solution is 2 to 5 BV / h, the adsorption capacity is 30 to 50 BV, and the adsorption amount is 1 to 1.5 g / L.

[0014] Preferably, the boron content in the battery-grade metal salt solution is ≤2 mg / L.

[0015] Preferably, after the boron removal by adsorption is completed, the process further comprises desorbing the boron removal resin obtained by the adsorption, or sequentially desorbing and regenerating the resin.

[0016] Preferably, the desorption is to elute the adsorbed boron removal resin with a desorption liquid, and the desorption liquid is an acidic solution;

[0017] The acidic solution is a sulfuric acid solution with a mass concentration of 5% to 10%.

[0018] Preferably, the flow rate of the desorption liquid is 1 to 3 BV / h, and the desorption amount is 1 to 3 BV.

[0019] Preferably, the regeneration is to remove the boron from the desorbed boron removal resin using a regeneration liquid, and the regeneration liquid is an alkaline solution;

[0020] The alkaline solution is a sodium hydroxide solution with a mass concentration of 1% to 5%.

[0021] Preferably, the regeneration flow rate is 1 to 3 BV / h, and the regeneration dosage is 1 to 2 BV.

[0022] The present invention provides a method for preparing a battery-grade metal salt solution using waste ternary lithium battery positive electrode materials as raw materials, comprising the following steps: wet-processing the waste ternary lithium battery positive electrode materials to obtain a boron-containing metal salt solution; the boron content in the boron-containing metal salt solution is 0.01-0.05 g / L; the metal elements in the boron-containing metal salt solution include one or more of nickel, cobalt and manganese; using a boron removal resin to adsorb and remove boron from the boron-containing metal salt solution to obtain a battery-grade metal salt solution; the metal elements in the battery-grade metal salt solution include one or more of nickel, cobalt and manganese; the model of the boron removal resin is HPB119. The boron removal resin model HPB119 used in the present invention is a macroporous polystyrene skeleton modified with a high molecular polymer having a selective coordination function for boron ions, and its coordination group can form a very stable complex with boron, but is inert to other anions, and this characteristic is used to selectively remove boron ions in the solution. The resin boron removal method can effectively remove boron ions in the solution, and at the same time has high adsorption performance, large processing capacity, simple and efficient operation, and will not introduce new impurities. DETAILED DESCRIPTION

[0023] The present invention provides a method for preparing a battery-grade metal salt solution using waste ternary lithium battery positive electrode materials as raw materials, comprising the following steps:

[0024] Wet-processing the waste ternary lithium battery positive electrode material to obtain a boron-containing metal salt solution; the boron content in the boron-containing metal salt solution is 0.01 to 0.05 g / L; the metal element in the boron-containing metal salt solution includes one or more of nickel, cobalt and manganese;

[0025] Adsorbing and removing boron from the boron-containing metal salt solution using a boron removal resin to obtain a battery-grade metal salt solution; the metal elements in the battery-grade metal salt solution include one or more of nickel, cobalt and manganese;

[0026] The model of the boron removal resin is HPB119.

[0027] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0028] In the present invention, the wet treatment preferably includes crushing, screening, leaching, extraction, degreasing and fine filtering the waste ternary lithium battery positive electrode material in sequence; the present invention has no special restrictions on the crushing, screening, leaching, extraction, degreasing and fine filtering process, and can be carried out using a process well known to those skilled in the art. In the present invention, the filtration accuracy of the fine filtration is preferably ≤0.3μm; the filtration accuracy can ensure good water quality of the stock solution, avoid clogging subsequent adsorption materials, and affect the boron removal effect.

[0029] In the present invention, the boron content in the boron-containing metal salt solution is 0.01-0.05 g / L; the metal elements in the boron-containing metal salt solution include one or more of nickel, cobalt and manganese.

[0030] After obtaining the boron-containing metal salt solution, the present invention uses a boron removal resin to adsorb and remove boron from the boron-containing metal salt solution to obtain a battery-grade metal salt solution; the metal elements in the battery-grade metal salt solution include one or more of nickel, cobalt and manganese; the model of the boron removal resin is HPB119.

[0031] In the present invention, the adsorption process is preferably to pass the boron-containing metal salt solution through a resin column filled with a boron removal resin. In the present invention, the flow rate of the boron-containing metal salt solution is preferably 2 to 5 BV / h, more preferably 2 to 4 BV / h, and most preferably 2 to 3 BV / h; the adsorption capacity is preferably 30 to 50 BV, more preferably 35 to 50 BV, and most preferably 40 to 50 BV; the adsorption amount is preferably 1 to 1.5 g / L, more preferably 1.1 to 1.4 g / L, and most preferably 1.2 to 1.3 g / L. In the present invention, the adsorption capacity is understood as the volume of the treated boron-containing metal salt solution accounting for the multiple of the volume of the resin filled in the resin column. The adsorption amount is understood as the adsorption amount of boron by the boron removal resin, that is, the mass of boron adsorbed per liter of boron removal resin.

[0032] In the present invention, the boron content in the battery-grade metal salt solution is preferably ≤2 mg / L.

[0033] In the present invention, the effluent obtained after the adsorption is completed is preferably sampled and tested regularly to determine the boron concentration in the effluent. Desorption and regeneration are performed in a timely manner after the boron exceeds the standard. In the actual production operation, two groups of resin columns are used in parallel, one group is desorbed and regenerated after adsorption is saturated, and then switched to the other group for normal production.

[0034] After the adsorption is completed, the present invention preferably further comprises desorbing the adsorbed boron removal resin obtained by the adsorption, or sequentially desorbing and regenerating the resin.

[0035] Before the desorption, the present invention also preferably includes washing the boron removal resin with pure water; the present invention has no special limitation on the washing process, and the washing process can be carried out by a process well known to those skilled in the art. In the present invention, the washing process can avoid the waste of high-value nickel and cobalt metals during the desorption process.

[0036] In the present invention, the desorption is preferably carried out by eluting the adsorbed boron removal resin with a desorption liquid, and the desorption liquid is preferably an acidic solution; the acidic solution is preferably a sulfuric acid solution with a mass concentration of 5% to 10%, more preferably a sulfuric acid solution with a mass concentration of 6% to 9%, and most preferably a sulfuric acid solution with a mass concentration of 7% to 8%. In the present invention, the flow rate of the desorption liquid is preferably 1 to 3BV / h, more preferably 1.5 to 2.5BV / h, and most preferably 1.8 to 2.2BV / h; the desorption amount is preferably 1 to 3BV, more preferably 1.5 to 2.5BV, and most preferably 1.8 to 2.2BV. In the present invention, the desorption amount is understood as the multiple of the volume of the acid solution used in the desorption process to the volume of the loaded boron removal resin.

[0037] Before the regeneration, the present invention also preferably includes washing the boron removal resin with pure water; the present invention has no special limitation on the washing process, and the washing process can be performed using a process well known to those skilled in the art. In the present invention, the washing process can prevent residual acid from consuming the alkaline solution required for subsequent regeneration.

[0038] In the present invention, the regeneration is preferably to remove boron from the desorbed boron removal resin using a regeneration liquid, and the regeneration liquid is preferably an alkaline solution; the alkaline solution is preferably a sodium hydroxide solution with a mass concentration of 1% to 5%, more preferably a sodium hydroxide solution with a mass concentration of 2% to 4%, and most preferably a sodium hydroxide solution with a mass concentration of 2.5% to 3.5%. In the present invention, the regeneration flow rate is preferably 1 to 3BV / h, more preferably 1 to 2.5BV / h, and most preferably 1 to 1.5BV / h; the regeneration amount is preferably 1 to 2BV, more preferably 1.2 to 1.8BV, and most preferably 1.4 to 1.6BV. In the present invention, the regeneration amount is understood as the volume of the alkaline solution used in the regeneration process as a multiple of the volume of the loaded boron removal resin.

[0039] After the regeneration is completed, the present invention also preferably includes washing the boron removal resin with pure water until it is neutral, so as to avoid the residual alkaline solution used in the regeneration causing the regenerated resin to contaminate the original solution (the boron-containing metal salt solution to be adsorbed) after use.

[0040] After the desorption and / or regeneration is completed, the present invention also preferably includes post-treatment of the desorption liquid obtained by the desorption and / or the regeneration liquid obtained by the regeneration; the post-treatment preferably includes mixing the desorption liquid and / or the regeneration liquid with lime milk, pressing, and obtaining boron slag. In the present invention, the mass concentration of the lime milk is preferably 10% to 20%, more preferably 12% to 18%, and most preferably 14% to 16%. In the present invention, the pH value of the mixed solution obtained after the mixing is preferably 9 to 11, more preferably 9.5 to 10.5, and most preferably 9.8 to 10.2. In the present invention, the mixing temperature is preferably 60 to 90°C, more preferably 65 to 85°C, and most preferably 70 to 80°C; the mixing time is preferably 0.5 to 1h, more preferably 0.6 to 0.9h, and most preferably 0.7 to 0.8h.

[0041] In the present invention, the lime milk is preferably replaced by lime milk with magnesium sulfate solution added; in the present invention, the magnesium sulfate solution in the lime milk with magnesium sulfate solution added is preferably a byproduct from the extraction process in the wet treatment of waste ternary lithium batteries. The concentration of the magnesium sulfate solution is preferably 20-40 g / L, more preferably 40 g / L; the mass concentration of the lime milk in the lime milk with magnesium sulfate solution added is preferably 10%-20%, more preferably 20%; the mass ratio of magnesium sulfate solution to lime milk in the lime milk with magnesium sulfate solution added is preferably (1.6-2):1, more preferably 2:1. In the present invention, the pH value of the mixed solution obtained after mixing is preferably 9-11, more preferably 9.5-10.5, and most preferably 9.8-10.2. In the present invention, the mixing temperature is preferably 60-90°C, more preferably 65-85°C, and most preferably 70-80°C; the mixing time is preferably 0.5-1h, more preferably 0.6-0.9h, and most preferably 0.7-0.8h. In the present invention, magnesium sulfate solution is added to lime milk, and the generated magnesium hydroxide is used as colloidal precipitation, which has strong adsorption performance to enhance the effect of boron precipitation.

[0042] The boron removal resin in the method of the present invention can be reused after regeneration. After the resin is saturated with adsorption, it is desorbed and regenerated by acid and alkali. The regenerated resin also has a strong adsorption capacity. At the same time, acid and alkali are also common industrial reagents, cheap and easy to obtain, and the use concentration is very low, which is friendly to employees and the environment.

[0043] The method for preparing a battery-grade metal salt solution using waste ternary lithium batteries as raw materials provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0044] Example 1

[0045] Pretreatment: Used lithium-ion batteries were crushed, screened, leached, extracted, degreased and finely filtered to obtain 3L of cobalt sulfate solution (boron content of 0.038g / L);

[0046] Adsorption process: the cobalt sulfate solution was passed through a resin column filled with a boron removal resin (HPB119 high adsorption capacity special resin produced by Jiangsu Haipu Functional Materials Co., Ltd.) at a flow rate of 2BV / h (the liquid volume through the column was 30BV, the adsorption capacity was 1.14g / L, and the time was 15h) to obtain adsorbed water (boron content was 1.6mg / L);

[0047] Desorption process: 2BV of pure water is passed through the resin column after adsorption saturation, and the water after washing is colorless. Then 2BV of dilute sulfuric acid (mass concentration is 10%) is passed through at a flow rate of 1BV / h for desorption for 2h, and then 2BV of pure water is passed through. The pH of the water after washing is neutral, and the desorbed resin column and desorption liquid are obtained;

[0048] Regeneration process: The desorbed resin column is passed through 2BV of 1% sodium hydroxide solution at a flow rate of 1BV / h for 2 hours, and then 2BV of pure water is passed through. The pH of the water after washing is neutral, and the regenerated resin column and regeneration liquid are obtained;

[0049] The cobalt sulfate solution was passed through the regenerated resin column at a flow rate of 3 BV / h (the liquid volume passing through the column was 30 BV) to obtain adsorbed water (boron content was 0.8275 mg / L);

[0050] Desorption liquid treatment: the desorption liquid (boron content is 1.03 g / L) and the regeneration liquid are mixed, and lime milk with a mass concentration of 20% is added to adjust the pH value of the desorption liquid and the regeneration liquid to 9, react for 0.5 h, filter, and obtain boron slag; the obtained filtrate (boron content is 0.93 g / L) is used for wastewater treatment.

[0051] Example 2

[0052] Pretreatment: Used lithium-ion batteries are crushed, screened, leached, extracted, degreased and finely filtered to obtain 5L of cobalt sulfate solution (boron content of 0.016g / L);

[0053] Adsorption process: the cobalt sulfate solution was passed through a resin column filled with a boron removal resin (HPB119 high adsorption capacity special resin produced by Jiangsu Haipu Functional Materials Co., Ltd.) at a flow rate of 2BV / h (the liquid volume through the column was 40BV, the adsorption capacity was 0.64g / L, and the time was 20h) to obtain adsorbed water (boron content was 0.09mg / L);

[0054] Desorption process: 2BV of pure water is passed through the resin column after adsorption saturation, and the water after washing is colorless. Then 2BV of dilute sulfuric acid (mass concentration is 6%) is passed through at a flow rate of 1BV / h for desorption for 2h, and then 2BV of pure water is passed through. The pH of the water after washing is neutral, and the desorbed resin column and desorption liquid are obtained;

[0055] Regeneration process: The desorbed resin column is passed through 2BV of 5% sodium hydroxide solution at a flow rate of 1BV / h for 2 hours, and then 2BV of pure water is passed through. The pH of the water after washing is neutral, and the regenerated resin column and regeneration liquid are obtained;

[0056] The cobalt sulfate solution was passed through the regenerated resin column at a flow rate of 3 BV / h (the liquid volume passing through the column was 54 BV) to obtain adsorbed water (boron content was 0.74 mg / L);

[0057] Desorption liquid treatment: the desorption liquid (boron content is 1.03 g / L) and the regeneration liquid are mixed, and lime milk with a mass concentration of 25% is added, and the pH value of the desorption liquid and the regeneration liquid is adjusted to 11, and the reaction is carried out for 0.5 h. The reaction is filtered to obtain boron slag; the obtained filtrate (boron content is 0.57 g / L) is used for wastewater treatment.

[0058] Example 3

[0059] Pretreatment: Used lithium-ion batteries were crushed, screened, leached, extracted, degreased and finely filtered to obtain 5L of cobalt sulfate solution (boron content of 0.026g / L);

[0060] Adsorption process: the cobalt sulfate solution was passed through a resin column filled with a boron removal resin (HPB119 high adsorption capacity special resin produced by Jiangsu Haipu Functional Materials Co., Ltd.) at a flow rate of 3BV / h (the liquid volume through the column was 45BV, the adsorption capacity was 1.17g / L, and the time was 15h) to obtain adsorbed water (boron content was 0.91mg / L);

[0061] Desorption process: 3BV of pure water is passed through the resin column after adsorption saturation, and the water after washing is colorless. Then 3BV of dilute sulfuric acid (mass concentration is 8%) is passed through at a flow rate of 1BV / h for desorption for 3h, and then 1BV of pure water is passed through. The pH of the water after washing is neutral, and the desorbed resin column and desorption liquid are obtained;

[0062] Regeneration process: The desorbed resin column is passed through 1.5 BV of a 3.5% sodium hydroxide solution at a flow rate of 1.5 BV / h for 1 hour, and then 2 BV of pure water is passed through. The pH of the water after washing is neutral, and a regenerated resin column and regeneration liquid are obtained;

[0063] Passing the cobalt sulfate solution into the regenerated resin column at a flow rate of 3 BV / h (the liquid volume passing through the column is 40 BV) to obtain adsorbed water (boron content is 1.05 mg / L);

[0064] Treatment of desorption liquid: After the desorption liquid (boron content is 1.03 g / L) and the regeneration liquid are mixed, magnesium sulfate solution (a by-product from the extraction process in the wet treatment of waste ternary lithium batteries, the concentration of the magnesium sulfate solution is 40 g / L) is added, and then lime milk is added to the obtained mixed solution (magnesium content is 4.95 g / L, boron content is 0.824 g / L) to adjust the pH value of the desorption liquid and the regeneration liquid to 9, react for 0.5h, filter, and obtain boron slag; the obtained filtrate (boron content is 0.058 g / L) is subjected to wastewater treatment.

[0065] Example 4

[0066] Pretreatment: Used lithium-ion batteries are crushed, screened, leached, extracted, degreased and finely filtered to obtain 5L of cobalt sulfate solution (boron content of 0.030g / L);

[0067] Adsorption process: the cobalt sulfate solution was passed through a resin column filled with a boron removal resin (HPB119 high adsorption capacity special resin produced by Jiangsu Haipu Functional Materials Co., Ltd.) at a flow rate of 2BV / h (the liquid volume through the column was 40BV, the adsorption capacity was 1.2g / L, and the time was 20h) to obtain adsorbed water (boron content was 0.76mg / L);

[0068] Desorption process: 1BV of pure water is passed through the resin column after adsorption saturation, and the water after washing is colorless. Then 2BV of dilute sulfuric acid (mass concentration is 8%) is passed through at a flow rate of 1BV / h for desorption for 2h, and then 1BV of pure water is passed through. The pH of the water after washing is neutral, and the desorbed resin column and desorption liquid are obtained;

[0069] Regeneration process: The desorbed resin column is passed through 1.5 BV of 3.5% sodium hydroxide solution at a flow rate of 1.5 BV / h for 1 hour, and then 1 BV of pure water is passed through. The pH of the water after washing is neutral, and the regenerated resin column and regeneration liquid are obtained;

[0070] The cobalt sulfate solution was passed through the regenerated resin column at a flow rate of 40 BV / h (the liquid volume passing through the column was 40 BV) to obtain adsorbed water (boron content was 0.92 mg / L);

[0071] Desorption liquid treatment: the desorption liquid (boron content is 1.03 g / L) and the regeneration liquid are mixed, lime milk is added to adjust the pH value to 11, the reaction is carried out for 0.5 h, and the boron slag is obtained by filtering; the obtained filtrate (boron content is 0.018 g / L) is used for wastewater treatment.

[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a battery-grade metal salt solution using waste ternary lithium battery positive electrode materials as raw materials, characterized in that: The following steps are involved: Wet-processing the waste ternary lithium battery positive electrode material to obtain a boron-containing metal salt solution; the boron content in the boron-containing metal salt solution is 0.01 to 0.05 g / L; the metal element in the boron-containing metal salt solution includes one or more of nickel, cobalt and manganese; Adsorbing and removing boron from the boron-containing metal salt solution using a boron removal resin to obtain a battery-grade metal salt solution; the metal elements in the battery-grade metal salt solution include one or more of nickel, cobalt and manganese; The model of the boron removal resin is HPB119.

2. The method according to claim 1, characterized in that The wet treatment includes crushing, screening, leaching, extracting, degreasing and fine filtering the waste ternary lithium battery positive electrode material in sequence.

3. The method according to claim 1, characterized in that The adsorption is performed by passing the boron-containing metal salt solution into a resin column filled with the boron removal resin.

4. The method according to claim 3, characterized in that The flow rate of the boron-containing metal salt solution is 2-5 BV / h, the adsorption capacity is 30-50 BV, and the adsorption amount is 1-1.5 g / L.

5. The method according to any one of claims 1 to 4, characterized in that: The boron content in the battery-grade metal salt solution is ≤2 mg / L.

6. The method according to claim 5, characterized in that After the boron removal by adsorption is completed, the process further includes desorbing the boron removal resin obtained by the adsorption, or desorbing and regenerating the resin in sequence.

7. The method according to claim 6, characterized in that The desorption is to elute the adsorbed boron removal resin with a desorption liquid, and the desorption liquid is an acidic solution; The acidic solution is a sulfuric acid solution with a mass concentration of 5% to 10%.

8. The method according to claim 7, characterized in that The flow rate of the desorption liquid is 1-3 BV / h, and the desorption amount is 1-3 BV.

9. The method according to claim 6, characterized in that The regeneration is to remove boron from the desorbed boron removal resin using a regeneration liquid, wherein the regeneration liquid is an alkaline solution; The alkaline solution is a sodium hydroxide solution with a mass concentration of 1% to 5%.

10. The method according to claim 6 or 9, characterized in that The regeneration flow rate is 1-3 BV / h, and the regeneration dosage is 1-2 BV.

Citation Information

Patent Citations

  • Battery-grade nickel salt and preparation method thereof

    CN113149091A

  • Recycling method of lithium battery positive plate

    CN114188627A

  • Method for preparing lithium battery negative electrode material by using waste power battery

    CN115360452A

  • Method for removing boron

    JP2002361236A

  • Process for preparing a high-purity nickel sulphate solution