Two-dimensional polymer composite membrane as well as preparation method and application thereof
By using trialdehyde phlogenetol and cyanodiamine-containing monomers in lithium extraction in salt lakes, and modifying hydroxylamine, the problem of low separation efficiency of monovalent metal ions in salt lakes is solved, and the problem of low separation efficiency of monovalent metal ions in salt lakes is achieved. It has efficient, energy-saving and environmentally friendly separation effects.
Patent Information
- Application Number
- CN202411093705.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing membrane separation technology is difficult to efficiently separate monovalent metal ions such as Na+, K+ and Li+ in salt lakes, resulting in low separation efficiency during lithium extraction of salt lakes, high process energy consumption and unfriendly environment.
Trialdehyde phlogenes and cyano-containing diamine monomers are used to form a two-dimensional polymer layer through Schiff base reaction, and acyl oxime groups are introduced through hydroxylamine modification to adjust the pore structure and active groups, and increase the monovalent /Separation properties of monovalent metal ions.
It has achieved efficient separation of Na+/Li+ and K+/Li+ during the lithium extraction process of salt lakes, significantly improved K+ penetration rate and selectivity, simple and safe process, suitable for industrial production, energy-saving and environmentally friendly.
Smart Images

Figure CN118925509A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of membrane separation technology, and in particular to a two-dimensional polymer composite membrane and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Lithium resources are known as "white gold" as a key raw material for electronic devices and electric vehicles. Salt lake brine resources contain a large amount of lithium resources, so lithium extraction from salt lakes has important social and economic significance. At present, research on lithium extraction from salt lakes mainly focuses on separating magnesium ions and lithium ions in salt lake brine. According to the different magnesium / lithium ratios in salt lake brine, the lithium extraction technology from salt lakes is also different. The lithium extraction technology from low magnesium / lithium ratio salt lakes mainly uses precipitation method, while the lithium extraction technology from high magnesium / lithium ratio salt lakes mainly uses adsorption method, electrodialysis method, membrane separation technology, and extraction method. Compared with other separation technologies, membrane separation technology has the advantages of high separation efficiency, simple operation, environmental friendliness, and low energy consumption. It has been widely used and studied in the process of lithium extraction from salt lakes.
[0004] At present, magnesium ions can be separated from lithium ions efficiently through membrane separation technology. + , K + , Li + With the same valence and similar hydration radius (Na + : K + : Li + : ), using membrane separation technology to separate monovalent / monovalent metal ions in salt lakes (Na + / Li + or K + / Li + Separation) is a current difficulty in the research of lithium extraction from salt lakes. Therefore, the development of membrane materials for separation (especially efficient separation) is the key to solving the problem. Summary of the invention
[0005] In order to address the deficiencies in the prior art, the purpose of the present invention is to provide a two-dimensional polymer composite membrane and a preparation method and application thereof. The two-dimensional polymer composite membrane prepared by the present invention has high separation performance in the monovalent / monovalent metal ion separation process, especially the modified two-dimensional polymer composite membrane has excellent separation performance.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, a method for preparing a two-dimensional polymer composite membrane comprises the following steps:
[0008] The organic phase is prepared by adding trialdehyde phloroglucinol to an organic solvent, a diamine monomer containing a cyano group is added to an acidic aqueous solution to prepare an aqueous phase, the organic phase and the aqueous phase are separated by a support membrane, and the trialdehyde phloroglucinol in the organic phase and the diamine monomer containing a cyano group undergo a Schiff base reaction on the surface of the support membrane to form a two-dimensional polymer layer, thereby obtaining;
[0009] The cyano-containing diamine monomer is an organic compound containing at least one cyano group and two primary amino groups.
[0010] The present invention adopts trialdehyde phloroglucinol and a diamine monomer containing a cyano group to form a covalent organic framework through a Schiff base reaction, which has a large number of pore structures and active groups such as ketone groups and cyano groups. The organic phase and the aqueous phase are separated by a support membrane, and the Schiff base reaction is carried out on the surface of the support membrane located at the interface between the oil and water phases, so that a two-dimensional polymer layer is grown in situ at the liquid-solid interface. In the process of growing the two-dimensional polymer layer in situ, the pore structure of the two-dimensional polymer layer can be adjusted by adjusting the number of cyano groups of the diamine monomer. It is found through experiments that the separation of monovalent / monovalent metal ions can be achieved by adjusting the pore structure of the two-dimensional polymer layer and the coordination of active groups such as ketone groups and cyano groups.
[0011] In order to further improve the separation effect of monovalent / monovalent metal ions, the present invention can use hydroxylamine to modify the formed two-dimensional polymer layer. In this method, hydroxylamine can react with the cyano group in the two-dimensional polymer layer to produce acyloxime groups. This makes the two-dimensional polymer layer contain oxime groups. Experimental studies have shown that the two-dimensional polymer composite membrane containing oxime groups has a better separation effect of monovalent / monovalent metal ions.
[0012] In another aspect, a two-dimensional polymer composite membrane is obtained by the preparation method described in the first aspect of the present invention.
[0013] Thirdly, a method for separating potassium ions and lithium ions is provided, wherein water and a solution containing potassium ions and lithium ions are placed on both sides of the above-mentioned two-dimensional polymer composite membrane, respectively, and allowed to stand for separation; in this separation process, osmotic pressure is used as the driving force for separation, which is more energy-saving and environmentally friendly compared to electric drive and pressure drive.
[0014] In a fourth aspect, an application of the above-mentioned two-dimensional polymer composite membrane or the method for separating potassium ions and lithium ions in extracting lithium from salt lakes.
[0015] The beneficial effects of the present invention are:
[0016] 1. The present invention selects trialdehyde phloroglucinol and a diamine monomer containing a cyano group to carry out a Schiff base reaction on the surface of a support membrane to form a two-dimensional polymer layer, which can not only adjust the pore structure of the two-dimensional polymer layer, but also introduce active groups such as ketone groups and cyano groups. Through the coordination of physical structure and active groups, the separation of monovalent / monovalent metal ions can be achieved, and the separation of monovalent metal ions in the process of lithium extraction from salt lakes can be achieved. In addition, the present invention converts part of the cyano group into an oxime group through hydroxylamine modification, which can further improve the separation effect of monovalent / monovalent metal ions. + / Li + During the separation process, K + Permeation rate and true K + / Li + The selectivity can reach 306mmol / m 2 ·h and 5.6, which can achieve efficient separation of monovalent metal ions during lithium extraction from salt lakes.
[0017] 2. The two-dimensional polymer composite membrane of the present invention has a simple and safe process in the preparation process, does not involve high temperature, high pressure or high energy consumption such as electricity consumption, has a low preparation cost, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0019] Figure 1 is a schematic diagram of preparing a cyano-containing two-dimensional polymer composite membrane according to Example 1 of the present invention;
[0020] Figure 2 is the FTIR spectrum of the cyano-containing two-dimensional polymer composite membrane TpPa-CN6 of Example 1 of the present invention;
[0021] Figure 3 is the XRD spectrum of the cyano-containing two-dimensional polymer composite membrane TpPa-CN6 of Example 1 of the present invention;
[0022] Figure 4 1 is a SEM image of the cyano-containing two-dimensional polymer composite membrane TpPa-CN6 of Example 1 of the present invention, a is a surface image of the membrane, and b is a cross-sectional image of the membrane;
[0023] Figure 5 is the FTIR spectrum of the acyloxime-containing two-dimensional polymer composite membrane TpPa-AO6 of Example 2 of the present invention;
[0024] Figure 6 is the XRD spectrum of the acyloxime-containing two-dimensional polymer composite film TpPa-AO6 of Example 2 of the present invention;
[0025] Figure 7 This is the SEM spectrum of the acyloxime-containing two-dimensional polymer composite membrane TpPa-AO6 of Example 2 of the present invention, a is a surface view, and b is a cross-sectional view;
[0026] Figure 8 is the FTIR spectrum of the cyano-containing two-dimensional polymer composite membrane TpPa-CN3 of Example 3 of the present invention;
[0027] Fig. 9 is the XRD spectrum of the cyano-containing two-dimensional polymer composite film TpPa-CN3 of Example 3 of the present invention;
[0028] Fig.10 1 is a SEM image of the cyano-containing two-dimensional polymer composite membrane TpPa-CN3 of Example 3 of the present invention, a is a surface image, and b is a cross-sectional image;
[0029] Fig.11 is the FTIR spectrum of the acyloxime-containing two-dimensional polymer composite membrane TpPa-AO3 of Example 6 of the present invention;
[0030] Fig.12 is the XRD spectrum of the acyloxime-containing two-dimensional polymer composite film TpPa-AO3 of Example 6 of the present invention;
[0031] Fig.13 1 is the SEM spectrum of the acyloxime-containing two-dimensional polymer composite membrane TpPa-AO3 of Example 6 of the present invention, a is a surface view, and b is a cross-sectional view;
[0032] Fig.14 is the FTIR spectrum of the two-dimensional polymer composite membrane TpPa-CN0 of Comparative Example 1 of the present invention;
[0033] Fig.15 is the XRD spectrum of the two-dimensional polymer composite membrane TpPa-CN0 of Comparative Example 1 of the present invention;
[0034] Fig.16 1 is a SEM image of the two-dimensional polymer composite membrane TpPa-CN0 of Comparative Example 1 of the present invention, a is a surface image, and b is a cross-sectional image;
[0035] Fig.17 K of the two-dimensional polymer composite membranes prepared in Examples 1, 2, 3, 6 and Comparative Example 1 in a single KCl solution and a LiCl solution + / Li + Separation performance;
[0036] Fig.18 K of the two-dimensional polymer composite membranes prepared in Examples 1, 2, 3, 6 and Comparative Example 1 in a KCl / LiCl mixed solution + / Li +Separation performance;
[0037] Fig.19 This is a performance comparison chart of the acyloximine-based two-dimensional polymer composite membrane prepared in Example 2 and other membranes reported in the literature in K+ / Li+ separation applications. DETAILED DESCRIPTION
[0038] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0039] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0040] Considering that the difficulty of extracting lithium from salt lakes lies in the separation of monovalent / monovalent metal ions by membrane materials, the present invention proposes a two-dimensional polymer composite membrane and a preparation method and application thereof.
[0041] A typical embodiment of the present invention provides a method for preparing a two-dimensional polymer composite membrane, comprising the following steps:
[0042] The organic phase is prepared by adding trialdehyde phloroglucinol to an organic solvent, a diamine monomer containing a cyano group is added to an acidic aqueous solution to prepare an aqueous phase, the organic phase and the aqueous phase are separated by a support membrane, and the trialdehyde phloroglucinol in the organic phase and the diamine monomer containing a cyano group undergo a Schiff base reaction on the surface of the support membrane to form a two-dimensional polymer layer, thereby obtaining;
[0043] The cyano-containing diamine monomer is an organic compound containing at least one cyano group and two primary amino groups.
[0044] In some embodiments, the organic solvent is one or more of mesitylene, 1,4-dioxane, ethyl acetate, tetrahydrofuran, methanol, o-dichlorobenzene or n-butanol, preferably a mesitylene / ethyl acetate mixed solvent. Specifically, the volume ratio of mesitylene to ethyl acetate is 2.5 to 6.5:1.
[0045] In some embodiments, the cyano-containing diamine monomer is 2,5-diaminoterephthalonitrile and / or 2,5-diaminobenzonitrile.
[0046] In some embodiments, the acidic aqueous solution is one or more of hydrochloric acid aqueous solution, acetic acid aqueous solution, trifluoromethanesulfonic acid aqueous solution or p-toluenesulfonic acid aqueous solution, preferably acetic acid aqueous solution. Specifically, the concentration of the acetic acid aqueous solution is 3.5 to 6.5 mol / L.
[0047] The present invention finds that the solvent has a great influence on the density and crystallinity of the finally prepared two-dimensional polymer membrane. When the organic solvent is selected as a mixed solvent of mesitylene / ethyl acetate and the aqueous hydrochloric acid solution is selected as the aqueous acetic acid solution, the two-dimensional polymer has better film-forming property and crystallinity, and thus has better monovalent / monovalent metal ion separation performance.
[0048] In some embodiments, the addition ratio of trialdehyde phloroglucinol to the organic solvent is 0.1-1:30-50, mmol:mL.
[0049] In some embodiments, the addition ratio of the cyano-containing diamine monomer to the acidic aqueous solution is 0.15-1.5:30-50, mmol:mL.
[0050] In some embodiments, the support membrane is a polyacrylonitrile membrane, a polysulfone membrane, a polyethersulfone membrane, an aluminum oxide membrane or a polyimide membrane, preferably a polyacrylonitrile membrane. The present invention does not impose any particular restrictions on the source of the support membrane, and the support membrane can be purchased from commercial sources.
[0051] In some embodiments, the temperature for forming the two-dimensional polymer layer is 30-70°C, more preferably 30-35°C.
[0052] In some embodiments, the time for forming the two-dimensional polymer layer is 2 to 7 days, more preferably 3.5 to 5.5 days.
[0053] In some embodiments, a post-modification process is further included, wherein the post-modification process is: modifying the two-dimensional polymer layer with hydroxylamine to convert the cyano group into an oxime group.
[0054] Specifically, the post-modification process comprises the following steps: placing a support membrane having a two-dimensional polymer layer grown on its surface in a hydroxylamine solution for reaction.
[0055] More specifically, the hydroxylamine in the hydroxylamine solution is a hydroxylamine aqueous solution or hydroxylamine hydrochloride. The hydroxylamine aqueous solution generally has a mass concentration of 45 to 55%. The solvent in the hydroxylamine solution is an alcohol solvent, which may be one or more of methanol, ethanol, isopropanol or n-butanol, and ethanol is further preferred.
[0056] More specifically, the temperature of the post-modification process is 30-80°C, preferably 30-35°C.
[0057] More specifically, the post-modification process lasts for 12 to 72 hours, preferably at 48 to 72°C.
[0058] Another embodiment of the present invention provides a two-dimensional polymer composite membrane obtained by the preparation method described in the first aspect of the present invention.
[0059] A third embodiment of the present invention provides a method for separating potassium ions and lithium ions, wherein water and a solution containing potassium ions and lithium ions are placed on both sides of the two-dimensional polymer composite membrane, respectively, and allowed to stand for separation.
[0060] A fourth embodiment of the present invention provides an application of the above-mentioned two-dimensional polymer composite membrane or the method for separating potassium ions and lithium ions in extracting lithium from salt lakes.
[0061] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0062] Example 1
[0063] A method for preparing a cyano-containing two-dimensional polymer composite film comprises the following steps:
[0064] (1) Weigh 21.0 mg (0.1 mmol) of trialdehyde pyrogallol (Tp), dissolve it in 50 mL of mesitylene / ethyl acetate mixed solution, and ultrasonicate it in an ultrasonic machine for 10 minutes to ensure that the solid is fully dissolved; weigh 23.7 mg (0.15 mmol) of 2,5-diaminoterephthalonitrile (Pa-CN2), dissolve it in 50 mL of acetic acid aqueous solution, and ultrasonicate it in an ultrasonic machine for 10 minutes to ensure that the solid is fully dissolved.
[0065] (2) First, a polyacrylonitrile membrane is used as a support membrane and is vertically sandwiched in the middle of a homemade H-shaped groove. Then, the solutions of the aldehyde monomer and the amine monomer in step (1) are added to both sides of the H-shaped groove respectively.
[0066] (3) placing the H-shaped tank to which the solution was added in step (2) into an oven at 30° C. and reacting for 4 days; after the reaction was completed, a two-dimensional polymer composite membrane containing cyanide groups was obtained, which was recorded as TpPa-CN6 membrane.
[0067] In Example 1 Figure 1 Schematic diagram of the preparation of cyano-containing two-dimensional polymer composite membrane.
[0068] The TpPa-CN6 film prepared in Example 1 was tested by FTIR spectrum. The results are as follows: Figure 2 As shown, it can be seen that the TpPa-CN6 membrane containing cyano groups was successfully prepared.
[0069] The TpPa-CN6 film prepared in Example 1 was subjected to XRD test, and the results are as follows: Figure 3As shown, it can be seen that the synthesized two-dimensional polymer film is highly crystalline.
[0070] The TpPa-CN6 membrane prepared in Example 1 was subjected to SEM testing, and the results were as follows: Figure 4 As shown, its dense structure and film thickness can be seen.
[0071] Example 2
[0072] A method for preparing a two-dimensional polymer composite film containing an acyl oxime group comprises the following steps:
[0073] (1) Weigh 200 μL of a 50% hydroxylamine aqueous solution, add it to 100 mL of ethanol, and ultrasonicate it in an ultrasonic machine for 10 minutes to ensure that the hydroxylamine is fully dissolved in the ethanol.
[0074] (2) The cyano-containing two-dimensional polymer composite membrane prepared in Example 1 is placed in the hydroxylamine solution prepared in step (1) to convert the cyano groups in the two-dimensional polymer composite membrane into oxime groups.
[0075] (3) The hydroxylamine solution containing the two-dimensional polymer composite membrane was placed in an oven at 30° C. and reacted for 72 hours.
[0076] (4) After the reaction is completed, the two-dimensional polymer composite membrane is continuously cleaned with deionized water and ethanol solution to obtain a two-dimensional polymer composite membrane containing acyl oxime groups, which is recorded as TpPa-AO6 membrane.
[0077] The TpPa-AO6 film prepared in Example 2 was subjected to FTIR spectrum test, and the results were as follows: Figure 5 As shown, it can be seen that the cyano groups in the two-dimensional polymer composite film are successfully converted into oxime groups.
[0078] The TpPa-AO6 film prepared in Example 2 was subjected to XRD test, and the results were as follows: Figure 6 As shown, it can be seen that after acylation, the two-dimensional polymer composite film still maintains good crystallinity.
[0079] The TpPa-AO6 membrane prepared in Example 2 was subjected to SEM testing, and the results were as follows: Figure 7 As shown, its dense structure and film thickness can be seen.
[0080] Example 3
[0081] This embodiment is the same as the embodiment 1, except that 2,5-diaminoterephthalonitrile is replaced by an equal molar amount of 2,5-diaminobenzonitrile to obtain a two-dimensional polymer composite film containing cyano groups, which is recorded as TpPa-CN3 film.
[0082] The TpPa-CN3 film prepared in Example 3 was tested by FTIR spectrum. The results are as follows: Figure 8As shown, it can be seen that the TpPa-CN3 membrane containing cyano groups was successfully prepared.
[0083] The TpPa-CN3 film prepared in Example 3 was subjected to XRD test, and the results were as follows: Fig. 9 As shown, it can be seen that the synthesized two-dimensional polymer film is highly crystalline.
[0084] The TpPa-CN3 membrane prepared in Example 3 was subjected to SEM testing, and the results were as follows: Fig.10 As shown, its dense structure and film thickness can be seen.
[0085] Example 4
[0086] This embodiment is the same as embodiment 1, except that the polyacrylonitrile membrane is replaced by a polysulfone membrane.
[0087] Example 5
[0088] This embodiment is the same as the embodiment 1, except that the polyacrylonitrile film is replaced by a polyimide film.
[0089] Example 6
[0090] This embodiment is the same as Embodiment 2, except that the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 1 is replaced by the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 3 to obtain a two-dimensional polymer composite membrane containing oxime groups, which is recorded as TpPa-AO3 membrane.
[0091] The TpPa-AO6 film prepared in Example 6 was subjected to FTIR spectrum test, and the results were as follows: Fig.11 As shown, it can be seen that the cyano groups in the two-dimensional polymer composite film are successfully converted into oxime groups.
[0092] The TpPa-AO6 film prepared in Example 6 was subjected to XRD test, and the results were as follows: Fig.12 As shown, it can be seen that after acylation, the two-dimensional polymer composite film still maintains good crystallinity.
[0093] The TpPa-AO6 membrane prepared in Example 6 was subjected to SEM testing, and the results were as follows: Fig.13 As shown, its dense structure and film thickness can be seen.
[0094] Example 7
[0095] This embodiment is the same as Embodiment 2, except that the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 1 is replaced by the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 4.
[0096] Example 8
[0097] This embodiment is the same as Embodiment 2, except that the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 1 is replaced by the cyanide-containing two-dimensional polymer composite membrane prepared in Embodiment 5.
[0098] Comparative Example 1
[0099] This comparative example is the same as Example 1, except that 2,5-diaminoterephthalonitrile is replaced by an equal molar amount of p-phenylenediamine to prepare a two-dimensional polymer composite membrane, which is recorded as TpPa-CN0.
[0100] The TpPa-CNO film prepared in Comparative Example 1 was subjected to FTIR spectrum test, and the results were as follows: Fig.14 As shown, it can be seen that the TpPa-CN0 membrane containing cyano groups was successfully prepared.
[0101] The TpPa-CNO film prepared in Comparative Example 1 was subjected to XRD test, and the results are as follows: Fig.15 As shown, it can be seen that the synthesized two-dimensional polymer film is highly crystalline.
[0102] The TpPa-CNO membrane prepared in Comparative Example 1 was subjected to SEM testing, and the results were as follows: Fig.16 As shown, its dense structure and film thickness can be seen.
[0103] Application Example 1
[0104] The two-dimensional polymer composite membranes of Examples 1, 2, 3, 6 and Comparative Example 1 were subjected to a monovalent / monovalent metal ion separation test, and the specific test process was as follows:
[0105] Prepare 100 mL of KCl solution (0.1 mol / L) and 100 mL of LiCl solution (0.1 mol / L) as feed solution;
[0106] Place the cyano or acyl oxime-containing two-dimensional polymer composite membrane vertically in the middle of an H-type membrane pool, add 100 mL of KCl solution or LiCl solution (0.1 mol / L) prepared in step (1) to the side facing the two-dimensional polymer layer, and add ultrapure water to the other side of the H-type membrane pool. Stir both sides of the H-type membrane pool at the same time. After 3 hours, take the solution on the ultrapure water side and then use an inductively coupled plasma mass spectrometer to check the K content of the solution. + or Li + concentration, and an ideal monovalent / monovalent metal ion separation test was performed under this system.
[0107] Fig.17 K is the K of the two-dimensional polymer composite membrane containing cyano and acyl oxime groups prepared in Example 1 and Example 2 in a single KCl solution and a LiCl solution. + / Li +Separation performance. From the separation performance diagram, it can be seen that the acyloximate-based two-dimensional polymer composite membrane exhibits a better K + / Li + Separation performance, K + Permeate flux and ideal K + / Li + The selectivity reached 340.2mmol / m 2 ·h and 6.4.
[0108] Application Example 2
[0109] The two-dimensional polymer composite membranes of Examples 1, 2, 3, 6 and Comparative Example 1 were subjected to a monovalent / monovalent metal ion separation test, and the specific test process was as follows:
[0110] (1) preparing 100 mL of KCl / LiCl mixed solution (0.1 mol / L) as feed solution;
[0111] (2) Place the cyano or acyl oxime-containing two-dimensional polymer composite membrane vertically in the middle of an H-type membrane pool, add 100 mL of the KCl / LiCl mixed solution (0.1 mol / L) prepared in step (1) to the side facing the two-dimensional polymer layer, and add ultrapure water to the other side of the H-type membrane pool. Stir both sides of the H-type membrane pool at the same time. After 3 hours, take the solution on the ultrapure water side, and then use an inductively coupled plasma mass spectrometer to check the K content of the solution. + or Li + concentration, and actual monovalent / monovalent metal ion separation tests were carried out under this system.
[0112] Fig.18 K of the two-dimensional polymer composite membrane containing cyano and acyl oxime groups prepared in Examples 1, 2, 3, 6 and Comparative Example 1 in a KCl / LiCl mixed solution + / Li + Separation performance. From the separation performance diagram, it can be seen that the acyloximate-based two-dimensional polymer composite membrane exhibits a better K + / Li + Separation performance, K + Permeation flux and actual K + / Li + The selectivity reached 306mmol / m 2 ·h and 5.6.
[0113] Fig.19 The acyloxime-based two-dimensional polymer composite membrane prepared in Example 2 is comparable to other membranes reported in the literature in terms of K + / Li + Performance comparison chart in separation applications, the results show that the acyl oxime-based two-dimensional polymer composite membrane exhibits excellent comprehensive K + / Li +The separation performance exceeds that reported in current literature, indicating that the membrane has more practical industrial application value.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a two-dimensional polymer composite membrane, comprising: The process is as follows: The organic phase is prepared by adding trialdehyde phloroglucinol to an organic solvent, a diamine monomer containing a cyano group is added to an acidic aqueous solution to prepare an aqueous phase, the organic phase and the aqueous phase are separated by a support membrane, and the trialdehyde phloroglucinol in the organic phase and the diamine monomer containing a cyano group undergo a Schiff base reaction on the surface of the support membrane to form a two-dimensional polymer layer, thereby obtaining; The cyano-containing diamine monomer is an organic compound containing at least one cyano group and two primary amino groups.
2. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The organic solvent is one or more of mesitylene, 1,4-dioxane, ethyl acetate, tetrahydrofuran, methanol, o-dichlorobenzene or n-butanol, preferably a mesitylene / ethyl acetate mixed solvent; preferably, the volume ratio of mesitylene to ethyl acetate is 2.5-6.5:
1.
3. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The diamine monomer containing a cyano group is 2,5-diaminoterephthalonitrile and / or 2,5-diaminobenzonitrile; Or, the acidic aqueous solution is one or more of a hydrochloric acid aqueous solution, an acetic acid aqueous solution, a trifluoromethanesulfonic acid aqueous solution or a p-toluenesulfonic acid aqueous solution, preferably an acetic acid aqueous solution; preferably, the concentration of the acetic acid aqueous solution is 3.5 to 6.5 mol / L; Or, the support membrane is a polyacrylonitrile membrane, a polysulfone membrane, a polyethersulfone membrane, an aluminum oxide membrane or a polyimide membrane, preferably a polyacrylonitrile membrane.
4. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The addition ratio of trialdehyde phloroglucinol and organic solvent is 0.1-1:30-50, mmol:mL; Alternatively, the addition ratio of the cyano-containing diamine monomer and the acidic aqueous solution is 0.15-1.5:30-50, mmol:mL.
5. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The temperature for forming the two-dimensional polymer layer is 30 to 70° C., preferably 30 to 35° C.; Alternatively, the time for forming the two-dimensional polymer layer is 2 to 7 days, more preferably 3.5 to 5.5 days.
6. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The method also includes a post-modification process, which comprises: modifying the two-dimensional polymer layer with hydroxylamine to convert the cyano group into an acyloxime group.
7. The method for preparing a two-dimensional polymer composite membrane according to claim 1, characterized in that: The post-modification process comprises the following steps: placing a support membrane having a two-dimensional polymer layer grown on the surface thereof in a hydroxylamine solution for reaction; Preferably, the hydroxylamine in the hydroxylamine solution is a hydroxylamine aqueous solution or hydroxylamine hydrochloride; preferably, the solvent in the hydroxylamine solution is an alcohol solvent, preferably, the alcohol solvent may be one or more of methanol, ethanol, isopropanol or n-butanol, more preferably ethanol; Preferably, the temperature of the post-modification process is 30 to 80°C, preferably 30 to 35°C; Preferably, the post-modification process lasts for 12 to 72 hours, preferably at 48 to 72°C.
8. A two-dimensional polymer composite membrane, characterized in that: Obtained by the preparation method according to any one of claims 1 to 7.
9. A method for separating potassium ions and lithium ions, characterized in that: Water and a solution containing potassium ions and lithium ions are placed on both sides of the two-dimensional polymer composite membrane according to claim 8, respectively, and allowed to stand for separation.
10. Use of the two-dimensional polymer composite membrane or the method for separating potassium ions and lithium ions according to claim 8 in extracting lithium from salt lakes.
Citation Information
Patent Citations
Method for preparing high-throughput covalent organic framework nano-filtration membrane on basis of interfacial polymerization
CN108889139A
Mixed matrix type cation exchange membrane and preparation method thereof
CN110336052A
Polymeric additives comprising zwitterionic moieties for PVDF-based membranes
CN114828993A
Film formulations comprising carrier
CN114901263A
Composite binder, secondary battery and electric equipment
CN116554815A