High-flux nanofiltration composite membrane and preparation method thereof
By introducing nanofiber intermediate layer and electrostatic spray-assisted interface polymerization technology into the nanofiltration membrane, the problem of insufficient flux and permeability of traditional nanofiltration membranes is solved, and the preparation of nanofiltration membranes with high throughput and high retention is achieved, improving the improvement of nanofiltration membranes The hydrophilicity and separation properties of the membrane are obtained.
Patent Information
- Application Number
- CN202310515983.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The flux of traditional nanofiltration membranes is difficult to increase under the premise of meeting the interception requirements, and the defects of the polyamide separation layer during electrostatic spraying affect the permeability, making it difficult to prepare a highly permeable nanofiltration membrane.
A nanofiber intermediate layer was introduced to modify the macroporous base membrane, and the nanofiber intermediate layer was obtained through electrospinning technology, and electrostatic spray-assisted interface polymerization was performed on its surface to prepare a high-throughput nanofiltration membrane.
While ensuring the divalent cation retention rate, the permeability flux of the nanofiltration membrane is significantly improved, and the hydrophilicity and separation performance of the membrane are enhanced.
Smart Images

Figure CN118925513A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nanofiltration membrane separation technology and water treatment, and specifically relates to a high-throughput nanofiltration composite membrane and a preparation method thereof. Background Art
[0002] Water is the source of life, and the world's demand for clean water resources is growing. As a water purification method, nanofiltration separation technology has the advantages of simple operation, low cost, green energy saving, etc., which has attracted widespread attention from researchers.
[0003] Common nanofiltration membranes are thin film composite membranes (TFC) with a three-layer asymmetric structure consisting of a non-woven fabric support layer, a polyethersulfone / polysulfone base membrane, and a polyamide active separation layer. The traditional polyamide separation layer is obtained by interfacial polymerization on the surface of the base membrane, which plays a key role in the performance of the nanofiltration membrane. At present, a variety of methods for preparing nanofiltration membranes have been developed, but the long-standing trade-off effect between permeability and selectivity in the membrane separation process makes it difficult to improve the flux of the nanofiltration membrane while meeting the interception requirements.
[0004] In order to prepare better nanofiltration membranes, researchers used electrostatic spray-assisted interfacial polymerization technology to obtain a thinner and more uniform polyamide separation layer, improving the performance of the nanofiltration membrane. However, the size of the monomer droplets produced during the electrostatic spray process is much smaller than the pore size of the base membrane, which easily causes interfacial polymerization to occur in the base membrane pores rather than on the membrane surface, resulting in separation layer defects and adversely affecting the permeability of the nanofiltration membrane. On the other hand, it makes it challenging to prepare a nanofiltration membrane with high permeability on a macroporous base membrane. Summary of the invention
[0005] The purpose of the present invention is to introduce a nanofiber intermediate layer to modify the macroporous base membrane, improve the base membrane structure, overcome the permeation-selectivity trade-off limitation in the membrane separation process, and obtain a high permeation flux while ensuring the membrane's retention rate for divalent cations.
[0006] In the present invention, the nanofiber is obtained by electrostatic spinning technology; the polyamide separation layer is prepared by electrostatic spray-assisted interfacial polymerization.
[0007] Compared with the existing membrane separation technology, the outstanding effects of the present invention are:
[0008] Compared with preparing the polyamide separation layer by directly performing interfacial polymerization on the polyethersulfone / polysulfone base membrane, the nanofiber intermediate layer is introduced between the porous base membrane and the polyamide separation layer for modification, which reduces the pore size of the macroporous base membrane surface and prevents polyamide from invading the base membrane; slows down the diffusion rate of the amine monomer, increases the content of the amine monomer on the reaction interface, and promotes the polymerization reaction. At the same time, the increased membrane surface roughness further improves the hydrophilicity of the membrane.
[0009] Another object of the present invention is to provide a preparation technology for the above-mentioned high-flux nanofiltration membrane.
[0010] To achieve the above object, the technical solution implemented by the present invention is:
[0011] In the first step, the polymer is completely dissolved in the solvent to prepare a uniform spinning solution;
[0012] In the second step, the dried base film is fixed on the collector of the electrospinning device, a spinning solution is loaded into one side of the collector, and then a nanofiber intermediate layer is electrospun on the surface of the base film to obtain a composite base film modified by nanofibers;
[0013] The third step is to dissolve the amine monomer in deionized water to obtain an aqueous phase solution; dissolve the acyl chloride monomer in a suitable solvent to obtain an organic phase solution;
[0014] The fourth step is to change the electrospinning device into a multi-nozzle electrostatic spray device, fix the composite base membrane obtained in the second step on the collector, respectively load the aqueous phase solution and the organic phase solution into the syringes on both sides of the collector, and perform electrostatic spray-assisted interfacial polymerization on the surface of the composite base membrane to obtain a polyamide separation layer;
[0015] In the fifth step, the membrane after the electrostatic spraying in the fourth step is removed, and a polyamide composite membrane modified with a nanofiber intermediate layer is obtained through heat treatment, which is a nanofiltration membrane with high flux.
[0016] In the above technical solution, the polymer used to prepare the spinning solution includes but is not limited to one or more of chitosan, polyvinyl alcohol, polyacrylonitrile, polyethyleneimine, polyethylene oxide, cellulose acetate, and polyvinylidene fluoride.
[0017] In the above technical solution, the time for electrospinning nanofibers is 1-60 minutes.
[0018] In the above technical scheme, the amino monomers include but are not limited to phenylenediamine, polyethyleneimine, piperazine and its derivatives; the acyl chloride monomers include but are not limited to isophthaloyl chloride, terephthaloyl chloride, trimesoyl chloride; the solvents include but are not limited to n-hexane, cyclohexane, etc.
[0019] In the above technical solution, the time of electrostatic spray-assisted interfacial polymerization is 1-60 minutes.
[0020] In the above technical solution, the heat treatment conditions are 40-80°C and the time is 1-30min.
[0021] Compared with the prior art, the present invention has the following positive effects: a high-flux nanofiltration membrane is prepared by introducing a nanofiber intermediate layer to modify the base membrane and preparing a polyamide separation layer by electrostatic spraying, thereby ensuring a high retention rate for divalent cations and obtaining a larger permeation flux. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The electrospinning device and its structural diagram
[0023] Figure 2 It is a multi-nozzle electrostatic spray device and its structural diagram
[0024] Among them: 1-power supply, 2-spinning solution injector, 3-drum collector, 4-power supply, 5-aqueous solution injector, 6-drum collector, 7-organic solution injector.
[0025] Figure 3 This is the SEM image of the base film surface
[0026] Figure 4 SEM and AFM images of the nanofiltration membrane surface
[0027] Figure 5 This is the Zeta potential test result of the nanofiltration membrane surface
[0028] Figure 6 is the water contact angle measurement result on the nanofiltration membrane surface
[0029] Figure 7 Examples 1-4 and Comparative Example 1 are performance comparison diagrams of nanofiltration membranes
[0030] Figure 8 Examples 5-8 and Comparative Example 1 are performance comparison diagrams of nanofiltration membranes
[0031] Fig. 9 Examples 9-12 and Comparative Example 2 are performance comparison diagrams of nanofiltration membranes
[0032] Fig.10 Examples 13-16 and Comparative Example 2 are performance comparison diagrams of nanofiltration membranes DETAILED DESCRIPTION
[0033] Specific embodiments of the high-flux nanofiltration composite membrane of the present invention are provided below.
[0034] Example 1
[0035] In the first step, polyvinyl alcohol powder is slowly poured into deionized water, and stirred while heating until it is completely dissolved to obtain a colorless and transparent polyvinyl alcohol spinning solution with a mass fraction of 5%.
[0036] In the second step, the dried commercial polyethersulfone base membrane is fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane is 413nm and the porosity is 18%. The polyvinyl alcohol spinning solution is injected into the syringe on the device, and the spinning process parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning is carried out for 10min, and a polyvinyl alcohol nanofiber intermediate layer is introduced on the surface of the polyethersulfone base membrane to obtain a modified polyvinyl alcohol / polyethersulfone composite base membrane. The average pore size of the composite base membrane is 350nm and the porosity is 14%.
[0037] The third step is to dissolve polyethyleneimine in deionized water to prepare an aqueous phase solution with a mass fraction of 1%; and to ultrasonically disperse trimesoyl chloride in n-hexane to prepare an organic phase solution with a mass fraction of 0.1%.
[0038] In the fourth step, the polyvinyl alcohol / polyethersulfone composite base film is fixed on the collector of the multi-nozzle electrostatic spray device. The syringes on both sides of the collector are respectively filled with aqueous solution and organic solution, and the electrostatic spray parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm away from the collector, organic phase syringe nozzle 6cm away from the collector, humidity 30%. Classical spray-assisted interfacial polymerization is carried out for 40min to prepare a polyamide separation layer.
[0039] In the fifth step, the membrane was removed and placed in an oven for heat treatment at 70°C for 10 minutes to finally obtain a high-flux nanofiltration composite membrane.
[0040] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0041] Example 2
[0042] Compared with Example 1, the difference of Example 2 is
[0043] In the second step, a dried commercial polyethersulfone base membrane was fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane was 413nm and the porosity was 18%. The polyvinyl alcohol spinning solution was injected into the syringe on the device, and the spinning process parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning was performed for 20min to obtain a polyvinyl alcohol / polyethersulfone composite base membrane.
[0044] The composite base membrane modified by the electrospun nanofiber intermediate layer has an average pore size of 343 nm and a porosity of 11%.
[0045] Example 3
[0046] Compared with Example 1, the difference of Example 3 is:
[0047] In the second step, a dried commercial polyethersulfone base membrane was fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane was 413nm and the porosity was 18%. The polyvinyl alcohol spinning solution was injected into the syringe on the device, and the spinning process parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning was performed for 30min to obtain a polyvinyl alcohol / polyethersulfone composite base membrane.
[0048] The composite base membrane modified by the electrospun nanofiber intermediate layer has an average pore size of 332 nm and a porosity of 9%.
[0049] Example 4
[0050] Compared with Example 1, the difference of Example 4 is:
[0051] In the second step, a dried commercial polyethersulfone base membrane was fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane was 413nm and the porosity was 18%. The polyvinyl alcohol spinning solution was injected into the syringe on the device, and the spinning process parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning was performed for 40min to obtain a polyvinyl alcohol / polyethersulfone composite base membrane.
[0052] The composite base membrane modified by the electrospun nanofiber intermediate layer has an average pore size of 289 nm and a porosity of 6%.
[0053] Example 5
[0054] In the first step, polyvinyl alcohol powder is slowly poured into deionized water, and stirred while heating until it is completely dissolved to obtain a colorless and transparent polyvinyl alcohol spinning solution with a mass fraction of 5%.
[0055] In the second step, the dried commercial polyethersulfone base membrane is fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane is 413nm and the porosity is 18%. The polyvinyl alcohol spinning solution is injected into the syringe on the device, and the spinning process parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning is carried out for 20min, and a polyvinyl alcohol nanofiber intermediate layer is introduced on the surface of the polyethersulfone base membrane to obtain a modified polyvinyl alcohol / polyethersulfone composite base membrane. The average pore size of the composite base membrane is 343nm and the porosity is 11%.
[0056] The third step is to dissolve polyethyleneimine in deionized water to prepare an aqueous phase solution with a mass fraction of 1%; and to ultrasonically disperse trimesoyl chloride in n-hexane to prepare an organic phase solution with a mass fraction of 0.1%.
[0057] In the fourth step, the polyvinyl alcohol / polyethersulfone composite base film is fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous phase solution and the organic phase solution are respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm away from the collector, organic phase syringe nozzle 6cm away from the collector, humidity 30%. Classical spray-assisted interfacial polymerization is carried out for 20min to prepare a polyamide separation layer.
[0058] In the fifth step, the membrane was removed and placed in an oven for heat treatment at 70°C for 10 minutes to finally obtain a high-flux nanofiltration composite membrane.
[0059] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0060] Example 6
[0061] Compared with Example 5, the difference of Example 6 is
[0062] In the fourth step, the polyvinyl alcohol / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous phase solution and the organic phase solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 30min to prepare a polyamide separation layer.
[0063] Example 7
[0064] Compared with Example 5, the difference of Example 7 is:
[0065] In the fourth step, the polyvinyl alcohol / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous solution and the organic solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 40min to prepare a polyamide separation layer.
[0066] Example 8
[0067] Compared with Example 5, the difference of Example 8 is:
[0068] In the fourth step, the polyvinyl alcohol / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous phase solution and the organic phase solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 50min to prepare a polyamide separation layer.
[0069] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0070] Comparative Example 1
[0071] As shown in Table 1, the preparation process of the polyamide separation layer of the comparative example is the same as that of Example 1, but the comparative example does not have the step of electrospinning the polyvinyl alcohol nanofiber intermediate layer on the polyethersulfone base membrane.
[0072] Table 1
[0073] first step Step 2 Step 3 Step 4 Step 5 Example 1 - - - - - Comparative Example 1 / / - - -
[0074] - represents that the step is carried out during the preparation process, and / represents that the step is not carried out during the preparation process.
[0075] Example 9
[0076] In the first step, chitosan powder is slowly poured into a 20wt.% acetic acid solution and stirred until it is completely dissolved to obtain a colorless and transparent chitosan spinning solution with a mass fraction of 5%.
[0077] In the second step, the dried commercial polyethersulfone base membrane is fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane is 413nm and the porosity is 18%. The chitosan spinning solution is injected into the syringe on the device, and the spinning process parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning is carried out for 15min, and a chitosan nanofiber intermediate layer is introduced on the surface of the polyethersulfone base membrane to obtain a modified chitosan / polyethersulfone composite base membrane. The average pore size of the composite base membrane is 362nm and the porosity is 16%.
[0078] The third step is to dissolve polyethyleneimine in deionized water to prepare an aqueous phase solution with a mass fraction of 1%; and to ultrasonically disperse trimesoyl chloride in n-hexane to prepare an organic phase solution with a mass fraction of 0.1%.
[0079] The fourth step is to fix the chitosan / polyethersulfone composite base film on the collector of the multi-nozzle electrostatic spray device. The aqueous solution and the organic solution are respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization is carried out for 40min to prepare a polyamide separation layer.
[0080] In the fifth step, the membrane was removed and placed in an oven for heat treatment at 70°C for 10 minutes to finally obtain a high-flux nanofiltration composite membrane.
[0081] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0082] Example 10
[0083] Compared with Example 9, the difference of Example 10 is
[0084] In the second step, a dried commercial polyethersulfone base membrane was fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane was 413nm and the porosity was 18%. The chitosan spinning solution was injected into the syringe on the device, and the spinning process parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning was performed for 30min to obtain a chitosan / polyethersulfone composite base membrane.
[0085] The composite base membrane modified by the electrospun nanofiber intermediate layer has an average pore size of 313 nm and a porosity of 13%.
[0086] Embodiment 11
[0087] Compared with Example 9, the difference of Example 11 is:
[0088] In the second step, a dried commercial polyethersulfone-based membrane was fixed on the drum collector of the electrospinning device.
[0089] The average pore size of the sulfone-based membrane is 413 nm, and the porosity is 18%. The chitosan spinning solution is injected into the syringe on the device, and the spinning process parameters are set as follows: positive voltage 15 kV, negative voltage -3 kV, injection speed 0.6 mL / h, collection drum speed 100 rpm, syringe translation speed 80 mm / min, syringe needle tip distance collector 8 cm, spinning humidity 30%. Electrospinning is performed for 45 minutes to obtain a chitosan / polyethersulfone composite base membrane.
[0090] The composite base membrane modified by the electrospinning nanofiber intermediate layer has an average pore size of 290 nm and a porosity of 10%.
[0091] Example 12
[0092] Compared with Example 9, the difference of Example 12 is:
[0093] In the second step, a dried commercial polyethersulfone base membrane was fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane was 413nm and the porosity was 18%. The chitosan spinning solution was injected into the syringe on the device, and the spinning process parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance 8cm from the collector, and spinning humidity 30%. Electrospinning was performed for 60min to obtain a chitosan / polyethersulfone composite base membrane.
[0094] The composite base membrane modified by the electrospun nanofiber intermediate layer has an average pore size of 212 nm and a porosity of 6%.
[0095] Example 13
[0096] In the first step, chitosan powder is slowly poured into deionized water, and stirred while heating until it is completely dissolved to obtain a colorless and transparent chitosan spinning solution with a mass fraction of 5%.
[0097] In the second step, the dried commercial polyethersulfone base membrane is fixed on the drum collector of the electrospinning device. The average pore size of the commercial polyethersulfone base membrane is 413nm and the porosity is 18%. The chitosan spinning solution is injected into the syringe on the device, and the spinning process parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 0.6mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, syringe needle tip distance collector 8cm, spinning humidity 30%. Electrospinning is carried out for 30min, and a chitosan nanofiber intermediate layer is introduced on the surface of the polyethersulfone base membrane to obtain a modified chitosan / polyethersulfone composite base membrane. The average pore size of the composite base membrane is 313nm and the porosity is 13%.
[0098] The third step is to dissolve polyethyleneimine in deionized water to prepare an aqueous phase solution with a mass fraction of 1%; and to ultrasonically disperse trimesoyl chloride in n-hexane to prepare an organic phase solution with a mass fraction of 0.1%.
[0099] The fourth step is to fix the chitosan / polyethersulfone composite base film on the collector of the multi-nozzle electrostatic spray device. The syringes on both sides of the collector are respectively filled with aqueous solution and organic solution, and the electrostatic spray parameters are set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm away from the collector, organic phase syringe nozzle 6cm away from the collector, humidity 30%. Classical spray-assisted interfacial polymerization is carried out for 20min to prepare a polyamide separation layer.
[0100] In the fifth step, the membrane was removed and placed in an oven for heat treatment at 70°C for 10 minutes to finally obtain a high-flux nanofiltration composite membrane.
[0101] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0102] Embodiment 14
[0103] Compared with Example 13, the difference of Example 14 is
[0104] In the fourth step, the chitosan / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous solution and the organic solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 30min to prepare a polyamide separation layer.
[0105] Embodiment 15
[0106] Compared with Example 13, the difference of Example 15 is:
[0107] In the fourth step, the chitosan / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous solution and the organic solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 40min to prepare a polyamide separation layer.
[0108] Example 16
[0109] Compared with Example 13, the difference of Example 16 is:
[0110] In the fourth step, the chitosan / polyethersulfone composite base film was fixed on the collector of the multi-nozzle electrostatic spray device. The aqueous solution and the organic solution were respectively loaded into the syringes on both sides of the collector, and the electrostatic spray parameters were set as follows: positive voltage 15kV, negative voltage -3kV, injection speed 1.2mL / h, collection drum speed 100rpm, syringe translation speed 80mm / min, aqueous phase syringe nozzle 12cm from the collector, organic phase syringe nozzle 6cm from the collector, humidity 30%. Classical spray-assisted interfacial polymerization was carried out for 50min to prepare a polyamide separation layer.
[0111] In the embodiments, the average pore size is measured by a pore size analyzer; the porosity is measured by a dry-wet weight method.
[0112] Comparative Example 2
[0113] As shown in Table 2, the preparation process of the polyamide separation layer of the comparative example is the same as that of Example 9, but the comparative example 2 does not have the step of electrospinning the chitosan nanofiber intermediate layer on the polyethersulfone based membrane.
[0114] Table 2
[0115] first step Step 2 Step 3 Step 4 Step 5 Example 9 - - - - - Comparative Example 2 / / - - -
[0116] - represents that the step is carried out during the preparation process, and / represents that the step is not carried out during the preparation process.
[0117] Characterization experiments
[0118] SEM Characterization:
[0119] The surface SEM photos of the polyethersulfone base membrane and the composite base membrane after the nanofiber intermediate layer is modified in the embodiment are as follows: Figure 3 As shown, the conventional polyethersulfone base membrane has a large pore size and an uneven pore structure, and the interlaced nanofibers form a network covering the macroporous base membrane to modify the base membrane surface and reduce the surface pore size. This is also proven by the continuously decreasing base membrane pore size and porosity in Examples 1-4 and Examples 9-12.
[0120] The SEM and AFM images of the nanofiltration membrane surfaces prepared in Example 2 / 10 and Comparative Example 1 / 2 are as follows: Figure 4 As shown, compared with the control example, the surface of the nanofiltration membrane prepared in the example can still clearly see the crossed nanofibers, and the surface roughness of the membrane is increased. According to the Wenzel model, the increased surface roughness is conducive to improving the hydrophilicity of the membrane surface.
[0121] Zeta potential test:
[0122] The surface Zeta potential results of the nanofiltration membranes prepared in Example 2 / 10 and Comparative Example 1 / 2 are as follows: Figure 5 As shown in the figure, it shows the change of the surface potential of the nanofiltration membrane before and after the modification of the nanofiber intermediate layer. The introduction of the intermediate layer increases the content of the interfacial amine monomer, which increases the residual amine groups on the membrane surface after the interfacial polymerization reaction and enhances the surface positive charge, which is beneficial to improve the separation ability of the nanofiltration membrane for multivalent cations.
[0123] Hydrophilicity characterization:
[0124] By measuring the water contact angle of the nanofiltration membrane in Example 2 / 10 and Comparative Example 1 / 2, the hydrophilicity of the membrane before and after modification was compared. Figure 6 As shown, the nanofiltration membrane prepared on the base membrane modified with the nanofiber intermediate layer exhibited better hydrophilicity.
[0125] Nanofiltration membrane performance test
[0126] The nanofiltration membranes of Examples 1-4 and Comparative Example 1 were used to test the permeation flux and retention rate of the nanofiltration composite membrane using a pressure-driven cross-flow filtration device. Under the test conditions of an operating pressure of 4 bar, a feed concentration of 500 PPM of magnesium chloride aqueous solution, and a solution temperature of room temperature, the flux and salt rejection rate of the membrane after stabilization for 30 minutes were measured. The results are as follows: Figure 7 shown.
[0127] The nanofiltration membranes of Examples 5-8 and Comparative Example 1 were used to test the permeation flux and retention rate of the nanofiltration composite membrane using a pressure-driven cross-flow filtration device. Under the test conditions of an operating pressure of 4 bar, a feed concentration of 500 PPM of magnesium chloride aqueous solution, and a solution temperature of room temperature, the flux and salt rejection rate of the membrane were measured after stabilization for 30 minutes. The results are as follows: Figure 8 shown.
[0128] The nanofiltration membranes of Examples 9-12 and Comparative Example 2 were used to test the permeation flux and retention rate of the nanofiltration composite membrane using a pressure-driven cross-flow filtration device. Under the test conditions of an operating pressure of 4 bar, a feed concentration of 500 PPM of magnesium chloride aqueous solution, and a solution temperature of room temperature, the flux and salt rejection rate of the membrane after stabilization for 30 minutes were measured. The results are as follows: Fig. 9 shown.
[0129] The nanofiltration membranes of Examples 13-16 and Comparative Example 2 were used to test the permeation flux and retention rate of the nanofiltration composite membrane using a pressure-driven cross-flow filtration device. Under the test conditions of an operating pressure of 4 bar, a feed concentration of 500 PPM of magnesium chloride aqueous solution, and a solution temperature of room temperature, the flux and salt rejection rate of the membrane after stabilization for 30 minutes were measured. The results are as follows: Fig.10 shown.
[0130] Analysis of experimental data shows that:
[0131] The polyamide composite nanofiltration membrane prepared by introducing a nanofiber intermediate layer to modify a macroporous substrate can significantly improve the permeation flux of the membrane and achieve effective separation of divalent cations.
[0132] The performance of the nanofiltration membranes obtained in Examples 1-4 was compared with each other, which showed that the flux of the nanofiltration membranes could be improved by adjusting the time of electrospinning polyvinyl alcohol nanofibers.
[0133] Compared with Examples 1-4, Comparative Example 1 uses a traditional polyethersulfone-based membrane that is not modified with a polyvinyl alcohol nanofiber intermediate layer. During the electrostatic spray-assisted interfacial polymerization process, defects occur in the generated polyamide layer, resulting in a low flux.
[0134] The performance of the nanofiltration membranes obtained in Examples 9-12 was compared with each other, which showed that the flux of the nanofiltration membranes could be improved by adjusting the time of electrospinning chitosan nanofibers.
[0135] Compared with Examples 9-12, in Comparative Example 2, a conventional polyethersulfone-based membrane that was not modified with a chitosan nanofiber intermediate layer was used. During the electrostatic spray-assisted interfacial polymerization process, defects occurred in the generated polyamide layer, resulting in a low flux.
[0136] The above-mentioned embodiments are only preferred solutions of the present invention. It should be noted that ordinary technicians in this technical field can make several improvements and modifications without departing from the concept of the present invention. These improvements and modifications are also within the protection scope of the present invention.
Claims
1. A high-flux nanofiltration composite membrane, comprising a supporting base membrane, a nanofiber intermediate layer and a polyamide separation layer, or a nanofiber layer and a polyamide separation layer, characterized in that: The base membrane is a non-woven fabric or a microfiltration membrane or a macroporous membrane such as polyvinylidene fluoride, polysulfone, polyether sulfone, polyacrylonitrile, polyethylene, polypropylene, etc.
2. The high-flux nanofiltration composite membrane according to claim 1, characterized in that: The nanofiber intermediate layer is prepared by electrostatic spinning; the dense separation layer is a polyamide separation layer prepared by electrospray-assisted interfacial polymerization or interfacial polymerization, or a separation layer of polyvinyl alcohol, cellulose acetate, etc. prepared by coating.
3. The method for preparing a high-flux nanofiltration composite membrane according to claim 1 or 2, characterized in that: The method comprises the following preparation steps: In the first step, the polymer is completely dissolved in the solvent to prepare a uniform spinning solution; In the second step, the dried base film and non-woven fabric are fixed on a collector, or the nanofibers are prepared directly by electrospinning process without using the base film, so as to obtain a base film modified by nanofibers, or a nanofiber layer. The third step is to dissolve the amine monomer in deionized water to obtain an aqueous solution; dissolving the acyl chloride monomer in a suitable solvent to obtain an organic phase solution; Using a multi-nozzle electrostatic spray device, electrostatic spray-assisted interfacial polymerization is performed on the surface of the composite base membrane / nanofiber membrane obtained in the second step to obtain a polyamide separation layer; In the fourth step, the membrane after the electrostatic spraying in the third step is removed, and a high-flux nanofiltration composite membrane is obtained through heat treatment.
4. The method for preparing a high-throughput nanofiltration composite membrane according to claim 3 is characterized in that the raw materials used to prepare the spinning solution in the first step include but are not limited to one or more polymers such as chitosan, polyvinyl alcohol, polyacrylonitrile, polyethylene oxide, cellulose acetate, polyvinylidene fluoride, polyethyleneimine, etc.; the solvent for dissolving the polymer includes but is not limited to one or more of deionized water, acetic acid, ethanol, acetone, etc.
5. The method for preparing a high-flux nanofiltration composite membrane according to claim 3, characterized in that: The time for electrospinning nanofibers in the second step is 1-60 min.
6. The method for preparing a high-flux nanofiltration composite membrane according to claim 3, characterized in that: Amine monomers include but are not limited to m-phenylenediamine, piperazine and its derivatives, polyethyleneimine, etc.; acyl chloride monomers include but are not limited to isophthaloyl chloride, terephthaloyl chloride, trimesoyl chloride; organic phase solvents include but are not limited to n-hexane, cyclohexane, etc.
7. The method for preparing a high-flux nanofiltration composite membrane according to claim 3, wherein the time of electrostatic spray-assisted interfacial polymerization in the third step is 1-60 min.
8. The method for preparing a high-flux nanofiltration composite membrane according to claim 3, wherein the heat treatment conditions in the fifth step are 40-80°C and the time is 1-30 min.