Rare earth metal modified molecular sieve and preparation method thereof
Through the preparation method of rare earth metal modified molecular sieve, the multi-stage pore structure and domain-limited metal sites are used to solve the problem of insufficient performance of existing molecular sieve adsorption hydrocarbons and oxygen-containing compounds, and achieve efficient adsorption and high temperature stability, satisfying the Fischer-Tropsch synthetic industry demand.
Patent Information
- Application Number
- CN202411272802.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
AI Technical Summary
When existing molecular sieves absorb coal through Fischer-Tropsch to synthesize hydrocarbon products produced by indirect liquefaction, especially oxygen-containing compounds, it is difficult to meet industrial needs.
Using the preparation method of rare earth metal modified molecular sieve, the 13X molecular sieve is mixed with reactants such as rare earth metal salt, aluminum source and alkali source, and crystallization reaction and calcination are carried out to form a molecular sieve precursor loaded with rare earth metal, and pass through multi-stage pore channels. Structural and confined metal sites improve adsorption performance.
It significantly improves the adsorption performance of molecular sieves, can effectively adsorb hydrocarbons and oxygen-containing compounds, meets the needs of Fischer-Tropsch synthesis industry, maintains stability at high temperatures, and extends service life.
Smart Images

Figure CN118925662A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of molecular sieve preparation, and in particular to a rare earth metal modified molecular sieve and a preparation method thereof. Background Art
[0002] The Fischer-Tropsch synthesis process is divided into a low-temperature Fischer-Tropsch synthesis process and a high-temperature Fischer-Tropsch synthesis process according to the reaction temperature. The catalysts, reactors and reaction conditions used in the two processes are obviously different, which determines that the product compositions of the two processes are also very different. The carbon number distribution of the low-temperature Fischer-Tropsch synthesis product is very wide, and the main product is solid wax. The group composition is aliphatic alkanes, a small amount of aliphatic olefins and oxygen-containing compounds, almost no aromatics and cycloalkanes, the mass fraction of α-olefins is 40-60%, and the mass fraction of oxygen-containing compounds is 3-10%. The carbon number distribution of high-temperature Fischer-Tropsch synthesis is narrower, and the main product is liquid oil. The group composition is olefins, a small amount of alkanes, oxygen-containing compounds and aromatics. Compared with low-temperature Fischer-Tropsch synthesis, the group composition of high-temperature Fischer-Tropsch synthesis oil is more complex, and the content of olefins (especially linear α-olefins) and oxygen compounds is higher. High-temperature Fischer-Tropsch synthetic oils contain a large amount of olefins and oxygen-containing compounds. This means that during downstream deep processing, in addition to being converted into liquid fuels such as gasoline and diesel, they can also be separated and extracted to produce a variety of high-value chemicals, such as 1-hexene, 1-octene, detergent-grade olefins, and oxygen-containing chemicals such as alcohols, aldehydes, and ketones.
[0003] Fischer-Tropsch synthetic oils have the characteristics of wide carbon number distribution and complex composition. In addition to hydrocarbon components, they also contain trace amounts of oxygenated compounds, mainly small molecular oxygenated compounds such as alcohols, aldehydes, ketones, acids, and esters. However, since hydrocarbons and oxygenated compounds can form azeotropes, they cannot be effectively separated by simple distillation.
[0004] Molecular sieves have regular crystal structures, adjustable pore systems, and relatively large specific surface areas. At the same time, molecular sieves have large Coulomb fields and polar effects in their crystals, and there are mobile, exchangeable compensating cations on their surfaces. Therefore, molecular sieve-type adsorbents are increasingly being used in the fields of adsorption, separation, and catalysis of Fischer-Tropsch synthetic oils.
[0005] However, the hydrocarbon products produced by indirect liquefaction of coal through Fischer-Tropsch synthesis have different carbon number distributions, and the oxygen-containing compounds in each carbon number product are of various types, with large differences in molecular weight and molecular structure. Therefore, high requirements are placed on the adsorption performance of molecular sieves. However, the performance of molecular sieves in the prior art is poor, and the adsorption effect on the above-mentioned oxygen-containing compounds is poor, which makes it difficult to meet industrial needs. Summary of the invention
[0006] The main purpose of the present invention is to provide a rare earth metal modified molecular sieve and a preparation method thereof, so as to solve the problem of poor adsorption performance of the molecular sieve in the prior art.
[0007] In order to achieve the above-mentioned purpose, according to the first aspect of the present invention, a method for preparing a rare earth metal modified molecular sieve is provided, and the preparation method comprises: S1) mixing a 13X molecular sieve and a first reactant to obtain a molecular sieve precursor; S2) mixing the molecular sieve precursor and a second reactant and performing a first crystallization reaction to obtain a rare earth metal modified molecular sieve; the first reactant comprises: a first aluminum source and a first metal salt; the first metal salt is a rare earth metal salt; the second reactant comprises: a first alkali source, a first silicon source and a supporting agent.
[0008] Further, the first aluminum source includes aluminum oxide; preferably, the rare earth metal salt includes: one or more of rare earth metal acetate, rare earth metal nitrate or rare earth metal sulfate; preferably, the rare earth metal acetate includes one or more of ytterbium acetate, lutetium acetate, thulium acetate, erbium acetate, gadolinium acetate, holmium acetate, titanium acetate or terbium acetate.
[0009] Furthermore, the first reactant also includes a pore-forming agent, a lubricant and a first acid source; preferably, the pore-forming agent includes one or more of sesbania powder, gum arabic, lignin, guar gum or ethyl cellulose; preferably, the lubricant includes a base oil; preferably, the first acid source includes one or more of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid or acetic acid, and more preferably, the first acid source is nitric acid.
[0010] Further, S1) includes S1-a) or S1-b); S1-a) includes: the first reactant includes 13X molecular sieve, a first aluminum source, a rare earth metal salt, a pore-forming agent, a lubricant and an acid source, the first reactant is mixed, a first drying is performed, and a first calcination is performed to obtain a molecular sieve precursor; S1-b) includes ion exchanging the 13X molecular sieve with the rare earth metal salt, and then mixing it with the first aluminum source, the pore-forming agent, the lubricant and the acid source, performing a second drying, and then performing a second calcination to obtain a molecular sieve precursor; preferably, the second drying temperature is 50-120°C, and the second drying time is 0.1-30h; preferably, the second calcination temperature is 400-650°C, and the second calcination time is 0.1-48h; preferably, the ion exchange temperature is 50-120°C, and the time is 0.1-5h. Preferably, the temperature of the first drying is 50-120° C., and the time of the first drying is 0.1-30 h; preferably, the temperature of the first calcination is 400-650° C., and the time of the first calcination is 0.1-48 h.
[0011] Furthermore, the mass ratio of 13X molecular sieve and the first aluminum source is (7-9): (1-3); preferably, the mass of the rare earth metal salt accounts for 2.5-5wt% of the total mass of the first reactant; preferably, the mass of the pore-forming agent accounts for 1-3wt% of the total mass of the first reactant; preferably, the mass of the lubricant accounts for 1-3wt% of the total mass of the first reactant; preferably, the mass of the acid source accounts for 0.5-1.5wt% of the total mass of the first reactant.
[0012] Further, the first alkali source includes one or more of sodium hydroxide, sodium carbonate, calcium hydroxide, potassium hydroxide or ammonia water; preferably, the first silicon source includes one or more of sodium silicate, silica sol, chromatography silica gel, methyl orthosilicate or ethyl orthosilicate; preferably, the supporting agent includes one or more of dihexadecyldimethylammonium chloride, isooctyl alcohol, polyethylene glycol ether, ethanolamine, dodecyldimethylbenzylammonium chloride, octadecyldimethylammonium chloride, hydroxyethylethylenediamine or didecyldimethylammonium chloride.
[0013] Further, S2) includes: mixing the molecular sieve precursor and the second reactant in a mass ratio of 1:20-60, performing a first crystallization reaction, and then performing a third calcination to obtain a rare earth metal modified molecular sieve; preferably, in the second reactant, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (0.1-8): (3-50): (0.5-15); more preferably, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (1-5): (20-40): (1-8); preferably, the temperature of the first crystallization reaction is 90-110°C, and the time of the first crystallization reaction is 4-36h; preferably, the temperature of the third calcination is 300-600°C, and the time of the third calcination is 2-24h.
[0014] Furthermore, the preparation method of 13X molecular sieve includes: a) mixing a second aluminum source, a second metal salt and water to obtain an aluminum source gel system; uniformly mixing a second silicon source and water to obtain a silicon source gel system; mixing the aluminum source gel system and the silicon source gel system to obtain a gel solution; b) mixing the gel solution with a second alkali source to obtain a gel slurry solution; c) subjecting the gel slurry solution to a second crystallization reaction and a third crystallization reaction to obtain a crystallization solution; d) mixing an aluminum-containing solution, a silicon-containing solution and a third alkali source to obtain a gel mother liquor; e) mixing the gel mother liquor with the crystallization solution, performing an aging reaction and a fourth crystallization reaction to obtain a 13X molecular sieve; preferably, the second metal salt includes a metal salt of any one or more of the following elements: calcium, magnesium, cerium, potassium, lanthanum or neodymium.
[0015] Further, the preparation method of 13X molecular sieve includes: a) mixing an aluminum source, a second metal salt and water to obtain an aluminum source gel system; uniformly mixing a second silicon source and water to obtain a silicon source gel system; mixing the aluminum source gel system and the silicon source gel system to obtain a gel solution; c) subjecting the gel slurry solution to a second crystallization reaction and a third crystallization reaction to obtain a crystallized solution; d) mixing an aluminum-containing solution, a silicon-containing solution and a third alkali source to obtain a gel mother liquor; e) mixing the gel mother liquor with the crystallization solution, performing an aging reaction and a fourth crystallization reaction to obtain a 13X molecular sieve; preferably, the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably, the second metal salt includes a metal salt of any one or more of the following elements: calcium, magnesium, cerium, potassium, lanthanum or neodymium; preferably, the metal salt includes one or more of calcium chloride, calcium nitrate, calcium bromide, calcium acetate, calcium phosphate, magnesium acetate, magnesium nitrate, lanthanum nitrate or cerium nitrate; preferably, in a), silicon The preparation method of the silicon source gel system is as follows: the second silicon source and water are uniformly mixed, stirred at 20-60°C for 0.1-12h, and the stirring speed is maintained at 200-800rpm to obtain a silicon source gel system; preferably, the second silicon source includes one or more of sodium silicate, silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash or carbon black; preferably, in b), the pH value of the gel slurry solution is 8.5-12.5; preferably, the second alkali source includes sodium hydroxide, sodium carbonate, hydrogen One or more of calcium oxide, potassium hydroxide or ammonia water; preferably, in c), the molar ratio of each component in the crystallization solution is silicon dioxide: aluminum oxide = 0.01-2.5:1, sodium oxide: silicon dioxide = 0.01-4:1, water: silicon dioxide = 1-40:1; preferably, in e), the aging reaction time is 0.1-24h, and the temperature is 20-100°C; preferably, the fourth crystallization reaction time is 0.1-36h, and the temperature is 60-105°C.
[0016] Furthermore, in c), the second crystallization reaction is performed for 4-24 hours at a temperature of 20-60°C; preferably, the third crystallization reaction is performed for 6-48 hours at a temperature of 60-100°C; preferably, the temperature of the third crystallization reaction is 20-50°C higher than that of the second crystallization reaction.
[0017] Further, d) includes: the concentration of the silicon-containing solution is 10.wt%-98wt%; the concentration of the aluminum-containing solution is 10wt%-98wt%; the concentration of the solution of the third alkali source is 0.5wt%-40wt%; preferably, the silicon-containing solution includes a solution of one or more of the following compounds: one or more of sodium silicate, pseudo-boehmite, silica sol, chromatography silica gel, methyl orthosilicate or ethyl orthosilicate; preferably, the aluminum-containing solution includes a solution of one or more of the following compounds: one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably, the third alkali source includes sodium hydroxide, sodium carbonate, calcium hydroxide, hydroxyl radical, iodine, iodine, sulphuric acid, sulphuric acid, chlorine ... one or more of potassium hydroxide or ammonia water; preferably, the atomic ratio of the components of the gel mother liquor is: silicon dioxide: aluminum oxide = 1-12: 1, sodium oxide: silicon dioxide = 0.25-3: 1, water: silicon dioxide = 5-50: 1; preferably, d) comprises: mixing the oxide with the third alkali source in a mass ratio of 1: 2.5-25 to obtain a gel mother liquor; preferably, the oxide comprises a waste catalyst; preferably, the waste catalyst comprises one or more of a waste ZSM-5 molecular sieve catalyst, a waste MTO catalyst, a waste X-type molecular sieve, fly ash, a waste A-type molecular sieve, a waste FCC catalyst, a waste Y-type molecular sieve or a waste VOC adsorbent.
[0018] Furthermore, the molar ratio of the amount of each component substance in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1: 0.5-10; alumina: MO = 1: 0.001-0.5; alumina: MOH = 1: 5-30; alumina: first acid root metal salt = 1: 0.5-20; alumina: second acid root metal salt = 1: 0.02-5; MO is the oxide of the active metal in the rare earth metal modified molecular sieve, MOH is the hydroxide of the active metal in the rare earth metal modified molecular sieve, and the active The metal includes: any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; the first acid radical metal salt includes salts of any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrates, hydrochlorides, sulfates, phosphates, citrates or acetates; the second acid radical metal salt includes salts of any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetates, nitrates or sulfates.
[0019] In order to achieve the above object, according to the second aspect of the present invention, a rare earth metal modified molecular sieve prepared by the above rare earth metal modified molecular sieve preparation method is provided; the molar ratio of the amount of each component substance in the rare earth metal modified molecular sieve is: aluminum oxide: silicon dioxide = 1: 0.5-10; aluminum oxide: MO = 1: 0.001-0.5; aluminum oxide: MOH = 1: 5-30; aluminum oxide: first acid root metal salt = 1: 0.5-20; aluminum oxide: second acid root metal salt = 1: 0.02-5; MO is the oxide of the active metal in the rare earth metal modified molecular sieve , MOH is the hydroxide of the active metal in the rare earth metal modified molecular sieve, and the active metal includes: any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; the first acid root metal salt includes salts of any one or more elements of calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrates, hydrochlorides, sulfates, phosphates, citrates or acetates; the second acid root metal salt includes salts of any one or more elements of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetates, nitrates or sulfates.
[0020] By applying the technical solution of the present invention, a 13X molecular sieve, a first aluminum source and a rare earth metal are mixed and first calcined to obtain a molecular sieve precursor doped with metal atoms. The molecular sieve precursor is then mixed with a first alkali source, a first silicon source and a supporting agent for first crystallization to obtain the rare earth metal-modified molecular sieve of the present application. Compared with the molecular sieve in the prior art, the rare earth metal-modified molecular sieve of the present application has improved adsorption performance and can meet the adsorption requirements in the Fischer-Tropsch synthesis industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0022] Figure 1 A schematic diagram of the XRD results of the rare earth metal modified molecular sieve according to Example 1 of the present invention is shown.
[0023] Figure 2 A schematic diagram of the SEM results of the rare earth metal modified molecular sieve according to Example 1 of the present invention is shown.
[0024] Figure 3 A schematic diagram of SEM results of the rare earth metal modified molecular sieve according to Example 2 of the present invention is shown.
[0025] Figure 4 A schematic diagram of the SEM results of the rare earth metal modified molecular sieve according to Comparative Example 2 of the present invention is shown. DETAILED DESCRIPTION
[0026] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0027] As mentioned in the background technology, the hydrocarbon products produced by indirect liquefaction of coal through Fischer-Tropsch synthesis have different carbon number distributions, and there are many types of oxygen-containing compounds in the carbon number products, with large differences in molecular weight and molecular structure. However, the molecular sieves in the prior art are difficult to meet the needs of the Fischer-Tropsch synthesis industry due to their poor adsorption performance. Therefore, in this application, the inventors try to load rare earth metals onto the pores of 13X molecular sieves for modification, and perform crystallization reactions to improve the adsorption performance of molecular sieves, which can be applied to the Fischer-Tropsch synthesis industry, and thus propose a series of protection schemes for this application.
[0028] In a first typical embodiment of the present application, a method for preparing a rare earth metal modified molecular sieve is provided, the method comprising: a method for preparing a rare earth metal modified molecular sieve, the method comprising: S1) mixing a 13X molecular sieve and a first reactant to obtain a molecular sieve precursor; S2) mixing the molecular sieve precursor and a second reactant and performing a first crystallization reaction to obtain a rare earth metal modified molecular sieve; the first reactant comprises: a first aluminum source and a first metal salt; the first metal salt is a rare earth metal salt; the second reactant comprises: a first alkali source, a first silicon source and a supporting agent.
[0029] In the present application, 13X molecular sieves, a first aluminum source and a rare earth metal salt are mixed to form a molecular sieve precursor that loads rare earth metal elements in the pores, and then the molecular sieve precursor is crystallized to obtain the molecular sieve of the present application. In the present application, rare earth metal salts, aluminum sources and 13X molecular sieves are reacted to improve the stability of the molecular sieve framework, load rare earth metal elements in the pores, reduce the thermal effect of the molecular sieve, and further improve the anti-phase change performance and anti-carbon deposition ability of the molecular sieve. Moreover, the introduction of rare earth metals can form confined metal sites in the molecular sieve pores, and confined metal sites generally refer to limiting metal atoms to a specific spatial structure, that is, in the present application, rare earth metal atoms are limited to the molecular sieve pores. In the present application, rare earth metal atoms are loaded in the pores of 13X molecular sieves, so that there are cations that balance the negative charge of the framework in the molecular sieve pores, improve the pore structure of the molecular sieve, the surface chemical properties and the cationic electric field in the molecular sieve crystal, so that its adsorption performance is further improved, which is conducive to its subsequent crystallization reaction with the second reactant to further construct a multi-stage pore.
[0030] Moreover, the formation of confined metal sites on the pores of the molecular sieve can further improve the thermal stability of the molecular sieve, protect the metal sites on its pores from sintering or aggregation at high temperatures, maintain the long-term stability of the molecular sieve, and enable it to maintain its adsorption performance during multiple cycles of use, reducing the frequency of replacement.
[0031] The molecular sieve precursor obtained in the present application is subjected to a crystallization reaction with the second reactant, and the pore structure of the molecular sieve is further adjusted so that a clear slit-type pore is formed between adjacent grains of the molecular sieve of the present application, which can improve the selective adsorption performance of the molecular sieve. The molecular sieve of the present application has a high specific surface area, multi-level pores, improved adsorption performance, a wide range of applicable hydrocarbon raw materials, and confined metal sites and slit-type pores. During the application process, it can not affect the properties of the hydrocarbon raw materials themselves in the Fischer-Tropsch industrial synthesis, and can also accurately remove various oxygen compound impurities such as alcohols, aldehydes, ketones, and esters in hydrocarbon substances.
[0032] In a preferred embodiment, the first aluminum source includes alumina; more preferably, the alumina is derived from raw materials such as nano alumina, pseudo-boehmite or boehmite; preferably, the rare earth metal salt includes one or more of rare earth metal acetate, rare earth metal nitrate or rare earth metallic sulfate; preferably, the rare earth metal acetate includes one or more of ytterbium acetate, lutetium acetate, thulium acetate, potassium acetate, magnesium acetate, erbium acetate, gadolinium acetate, holmium acetate, titanium acetate or terbium acetate.
[0033] In this application, rare earth metal salts are selected to modify 13X molecular sieves, and when rare earth elements are loaded in the molecular sieve pores, the defective parts of the silicon-aluminum molecular sieve are filled, and the oxygen atoms in the molecular sieve structure are connected, so as to improve the stability of the molecular sieve framework, and a confined metal site is formed on the pores of the molecular sieve, and the adsorption selectivity and thermal stability of the molecular sieve are improved. The rare earth metal salt in this application is more preferably an acetic acid rare earth metal salt, and acetate ions have good solubility relative to the ions in other rare earth metal salts, can be dissolved in solvents such as water and ethanol, and have a higher melting point and good thermal stability, are more stable in the system, and the reaction is mild, easy to regulate, and can better make rare earth metal atoms loaded in the molecular sieve pores, further promote the molecular sieve The modified molecular skeleton remains stable.
[0034] In a preferred embodiment, the first reactant further comprises a pore former, a lubricant and a first acid source; preferably, the pore former comprises one or more of sesbania powder, gum arabic, lignin, guar gum or ethyl cellulose; preferably, the lubricant comprises but is not limited to base oil; preferably, the base oil comprises but is not limited to mineral base oil; more preferably, the mineral base oil comprises but is not limited to one or more of PAO4, PAO6, or white oil; preferably, the first acid source comprises one or more of nitric acid, acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid or acetic acid; more preferably, the first acid source is nitric acid. Mineral base stock refers to the liquid component that constitutes the finished lubricating oil and grease, which can be a refinery fractionation product or a synthetic oil.
[0035] The above-mentioned first acid source can serve as a binder between the rare earth atoms in the rare earth metal salt and the molecular sieve, and is more preferably nitric acid, which can promote the rare earth atoms to combine with the molecular sieve pores, further improve the adsorption strength of the modified molecular sieve, and can also serve as an auxiliary agent for ion exchange in the subsequent S1-b) to participate in the modification of the molecular sieve, which is beneficial to improve the adsorption performance of the modified 13X molecular sieve.
[0036] In a preferred embodiment, S1) includes S1-a) or S1-b); S1-a) includes: the first reactant includes 13X molecular sieve, a first aluminum source, a rare earth metal salt, a pore-forming agent, a lubricant and an acid source, the first reactant is mixed, a first drying is performed, and then a first calcination is performed to obtain a molecular sieve precursor; S1-b) includes ion-exchanging the 13X molecular sieve with the rare earth metal salt, mixing it with the first aluminum source, the pore-forming agent, the lubricant and the acid source, performing a second drying, and then performing a second calcination to obtain to obtain a molecular sieve precursor; preferably, the first drying temperature is 50-120°C (including but not limited to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110 or 120°C), and the first drying time is 0.1-30h (including but not limited to 0.1, 0.5, 0.8, 1, 23, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30h); preferably, the temperature of the first calcination is 400-650°C (including but not limited to 400°C, 450°C, 500°C, 550°C, 600°C or 650°C), and the time of the first calcination is 0.1-48h (including but not limited to 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, ... 6, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47 or 48h); preferably, the second drying temperature is 50-120°C (including but not limited to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110 or 120°C), and the second drying time is 0.1-30h (including but not limited to 0.1, 0.5, 0.8, 1, 2 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30h); preferably, the temperature of the second calcination is 400-650°C (including but not limited to 400°C, 450°C, 500°C, 550°C, 600°C or 650°C), and the time of the second calcination is 0.1-48h (including but not limited to 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47 or 48h); preferably, the ion exchange temperature is 50-120°C (including but not limited to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C), and the time is 0.1-5h (including but not limited to 0.1, 1, 2, 3, 4 or 5h). .
[0037] In a preferred embodiment, preferably, the mass ratio of 13X molecular sieve and the first aluminum source is (5-10): (1-5), preferably (7-9): (1-3); preferably, the mass of the rare earth metal salt accounts for 2.5-5wt% of the total mass of the first reactant, including but not limited to 2.5, 3, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9 or 5wt%; preferably, the mass of the pore-forming agent accounts for 1-3wt% of the mass of the system, including but not limited to 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1 .9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3wt%; preferably, the mass of the lubricant accounts for 1-3wt% of the mass of the system, including but not limited to 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3wt%; preferably, the mass of the acid source accounts for 0.5-1.5wt% of the mass of the system, including but not limited to 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5. The total mass of the first reactant refers to the mass before drying.
[0038] The present application can load the metal elements in the rare earth metal salt into the pores of the 13X molecular sieve through two parallel schemes. As described in S1-a above, after the 13X molecular sieve is mixed and dried with the first aluminum source, the rare earth metal salt and the pore-forming agent, the rare earth metal elements in the rare earth metal salt are loaded into the molecular sieve pores by high-temperature roasting, and the temperature and time of the roasting are controlled within the above range, so that the rare earth metal elements in the rare earth metal salt are loaded into the molecular sieve pores, and react with the first aluminum source and the pore-forming agent at the same time, and further adjust the silicon-aluminum ratio and polarity of the 13X molecular sieve. Or as described in S1-b above, the 13X molecular sieve is first ion exchanged with the rare earth metal salt, and the time and temperature of the ion exchange are controlled within the above range, so that the rare earth metal elements are loaded into the pores of the 13X molecular sieve; and then mixed and roasted with the first aluminum source, the rare earth metal salt and the pore-forming agent, the stability of the loaded rare earth metal elements is further improved, a multi-level pore molecular sieve is formed, and the specific surface area and pore volume of the molecular sieve are increased. The molecular sieve precursor of the present application can be formed by using the above two methods, and those skilled in the art can select one according to actual production needs.
[0039] In a preferred embodiment, the first alkali source includes one or more of sodium hydroxide, sodium carbonate, calcium hydroxide, potassium hydroxide or ammonia water; preferably, the first silicon source includes one or more of sodium silicate, silica sol, chromatography silica gel, methyl orthosilicate or ethyl orthosilicate; preferably, the supporting agent includes one or more of dihexadecyldimethylammonium chloride, isooctyl alcohol, polyethylene glycol ether, ethanolamine, dodecyldimethylbenzylammonium chloride, octadecyldimethylammonium chloride, hydroxyethylethylenediamine or didecyldimethylammonium chloride.
[0040] In a preferred embodiment, S2) includes mixing the molecular sieve precursor and the second reactant in a mass ratio of 1:20-60 (including but not limited to 1:20, 1:25, 1:30, 1:35, 1:40, 1:4, 1:50, 1:55 or 1:60), performing a first crystallization reaction, and then performing a third calcination to obtain the molecular sieve; preferably, in the second reactant, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (0.1-8): (3-50): (0.5-15); more preferably, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (1-5): (20-40): (1-8); preferably, the temperature of the first crystallization reaction is 85-110°C, including but not limited to 85, 90°C, 95, 100 or 110°C; The time of the first crystallization reaction is 4-36h, including but not limited to 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35 or 36h; preferably, the temperature of the third calcination is 300-600℃, including but not limited to 300℃, 350℃, 400℃, 450℃, 500℃, 550℃ or 600℃, and the time of the third calcination is 2-24h, including but not limited to 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h.
[0041] After forming the above-mentioned molecular sieve precursor, the present application mixes the molecular sieve precursor, alkali, silicon and supporting agent, and performs hydrothermal crystallization reaction again, so that the molecular sieve precursor can be further crystallized, so that the distribution of rare earth metal elements in the pores is more uniform, and it is further fixed in the molecular sieve pores, so that it is not easy to fall during use and regeneration. Moreover, the crystallization reaction can help to form a multi-stage pore molecular sieve, and further in the pores of the rare earth metal elements loaded, a specific specific pore structure and crystal morphology are formed, the porosity is improved, and a slit-type pore is formed inside the molecular sieve, which improves the adsorption selectivity of the molecular sieve in the industrial application of Fischer-Tropsch synthesis. Crystallization reaction is carried out by increasing the alkali source, and the thermal stability of the molecular sieve is further improved, so that it can adapt to the removal of oxygenated compounds in the Fischer-Tropsch synthesis oil at high temperature. After the above-mentioned hydrothermal crystallization reaction, the crystallized molecular sieve precursor is subjected to high temperature roasting again, further widening its specific surface area and pore volume, and promoting its molding.
[0042] The present application precisely regulates the temperature, time, and mass ratio of the above-mentioned crystallization reaction and calcination, so that they can work together to improve the adsorption performance of the molecular sieve and improve its stability. The molecular sieve doped with rare earth metal atoms prepared by the preparation method of the present application has a rich pore structure, increased specific surface area and pore volume, strong thermal stability, and improved performance, so that it can be regenerated multiple times and still have strong activity and a longer service life.
[0043] In a preferred embodiment, the preparation method of 13X molecular sieve includes: a) mixing a second aluminum source, a second metal salt and water to obtain an aluminum source gel system; uniformly mixing a second silicon source and water to obtain a silicon source gel system; mixing the aluminum source gel system and the silicon source gel system to obtain a gel solution; b) mixing the gel solution with a second alkali source to obtain a gel slurry solution; c) subjecting the gel slurry solution to a second crystallization reaction and a third crystallization reaction to obtain a crystallization solution; d) mixing an aluminum-containing solution, a silicon-containing solution and a third alkali source to obtain a gel mother liquor; e) mixing the gel mother liquor with the crystallization solution, performing an aging reaction and a third crystallization reaction to obtain a 13X molecular sieve; preferably, the second metal salt includes a metal salt of any one or more of the following elements: calcium, magnesium, cerium, potassium, lanthanum or neodymium. Preferably, the metal salt includes one or more of calcium chloride, calcium nitrate, calcium bromide, calcium acetate, calcium phosphate, magnesium acetate, magnesium nitrate, lanthanum nitrate or cerium nitrate
[0044] The preparation method of the above-mentioned 13X molecular sieve is a one-pot method for preparing a 13X molecular sieve without impurities, smooth crystals and doped with calcium, magnesium, cerium, potassium, lanthanum or neodymium elements (i.e., the second metal in the present application). The 13X molecular sieve prepared by the method can be better doped with rare earth metal atoms in subsequent reactions. In the preparation process of the 13X molecular sieve of the present application, an aluminum source gel system containing one or more elements of calcium, magnesium, cerium, potassium, lanthanum or neodymium is utilized, and the above-mentioned silicon source gel system is reacted so that the framework of the 13X molecular sieve is doped with the above-mentioned second metal atoms, thereby improving the thermal stability of the molecular sieve framework.
[0045] The present application performs synergistic doping of gradient metal elements on the molecular sieve. When preparing the molecular sieve, a second metal element is doped in the skeleton of the molecular sieve; subsequently, a rare earth metal element is further doped in the pores thereof. The second metal element and the rare earth metal element in the skeleton and the pores cooperate with each other to improve the thermal stability of the molecular sieve, and adjust the positive and negative charge balance and polarity of the molecular sieve. Furthermore, through the above-mentioned first crystallization treatment and first calcination, the metal elements on the pores and the skeleton are not easy to fall off during use, which is conducive to the formation of a molecular sieve that is resistant to high temperatures, has a long service life, and has a strong regeneration ability, and can be applied to the Fischer-Tropsch synthetic oil industry.
[0046] Preferably, in a), the preparation method of the aluminum source gel system is: uniformly mix the second aluminum source, the metal salt and water, stir at 20-60°C for 0.1-12h, and maintain the stirring speed at 200-800rpm to obtain the aluminum source gel system; preferably, the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably, in a), the preparation method of the silicon source gel system is: uniformly mix the second silicon source and water, stir at 20-60°C for 0.1-12h, and maintain the stirring speed at 200-800rpm to obtain the silicon source gel system; preferably, the second silicon source includes sodium silicate, silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, One or more of fly ash or carbon black; preferably, in b), the pH value of the gel slurry solution is 8.5-12.5; preferably, the second alkali source includes one or more of sodium hydroxide, sodium carbonate, calcium hydroxide, potassium hydroxide or ammonia water; preferably, in c), the molar ratio of each component in the crystallization solution is silicon dioxide:alumina=0.01-2.5:1, sodium oxide:silicon dioxide=0.01-4:1, water:silicon dioxide=1-40:1; preferably, in e), the aging reaction time is 0.1-24h, and the temperature is 20-100°C; preferably, the fourth crystallization reaction time is 0.1-36h, and the temperature is 60-105°C.
[0047] In a preferred embodiment, in c), the second crystallization reaction time is 4-24h, and the temperature is 20-60°C; preferably, the third crystallization reaction time is 6-48h, and the temperature is 60-100°C; preferably, the temperature of the third crystallization reaction is 20-50°C higher than the second crystallization reaction temperature.
[0048] In a preferred embodiment, d) includes: the concentration of the silicon-containing solution is 10wt%-98wt%; the concentration of the aluminum-containing solution is 10wt%-98wt%; the concentration of the solution of the third alkali source is 0.5wt%-40wt%; preferably, the silicon-containing solution includes a solution of one or more of the following compounds: one or more of sodium silicate, silica sol, chromatography silica gel, methyl orthosilicate or ethyl orthosilicate; preferably, the aluminum-containing solution includes a solution of one or more of the following compounds: one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably, the third alkali source includes sodium hydroxide, sodium carbonate, calcium hydroxide, calcium hydroxide one or more of potassium or ammonia water; preferably, the molar ratio of the components of the gel mother liquor is: silicon dioxide: aluminum oxide = 0.5-6: 1, sodium oxide: silicon dioxide = 0.5-6: 1, water: silicon dioxide = 10-100: 1; preferably, d) comprises: mixing the oxide with the third alkali source in a mass ratio of 1: 2.5-25 to obtain a gel mother liquor; preferably, the oxide comprises a waste catalyst; preferably, the waste catalyst comprises one or more of a waste ZSM-5 molecular sieve catalyst, a waste MTO catalyst, a waste X-type molecular sieve, fly ash, a waste A-type molecular sieve, a waste FCC catalyst, a waste Y-type molecular sieve or a waste VOC adsorbent.
[0049] In a preferred embodiment, the molar ratio of the amount of each component substance in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1: 0.5-10 (including but not limited to 1: 0.5, 1: 1, 1: 2, 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8, 1: 9 or 1: 10); alumina: MO = 1: 0.001-0.5 (including but not limited to 1: 0.001, 1: 0.002, 1: 0003, 1: 0.004, 1: 1.005, 1: 1.006, 1: 007, 1: 008, 1: 009, 1: 0.1, 1: 0.2, 1: 0.3, 1: 1 :0.4 or 1:0.5); alumina: MOH = 1:5-30 (including but not limited to 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29 or 1:30); alumina: first acid metal salt = 1:0.5-20 (including but not limited to 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6 , 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20); alumina: second acid metal salt = 1:0.02-5 (including but not limited to 1:0.002, 1:0003, 1:0.004, 1:1.005, 1:1.006, 1:007, 1:008, 1:009, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:1, 1:2, 1:3, 1:4 or 1:5); MO is the rare earth metal modified The oxide of the active metal in the molecular sieve, MOH is the hydroxide of the active metal in the rare earth metal modified molecular sieve, the active metal includes: any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; the first acid root metal salt includes salts of any one or more elements of calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrates, hydrochlorides, sulfates, phosphates, citrates or acetates; the second acid root metal salt includes salts of any one or more elements of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetates, nitrates or sulfates.
[0050] In a second typical embodiment of the present application, a rare earth metal modified molecular sieve prepared by any of the above rare earth metal modified molecular sieve preparation methods is provided; the molar ratio of the amount of each component substance in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1: 0.5-10; alumina: MO = 1: 0.001-0.5; alumina: MOH = 1: 5-30; alumina: first acid root metal salt = 1: 0.5-20; alumina: second acid root metal salt = 1: 0.02-5; MO is the oxide of the active metal in the rare earth metal modified molecular sieve, M OH is the hydroxide of the active metal in the rare earth metal modified molecular sieve, and the active metal includes: any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; the first acid radical metal salt includes salts of any one or more elements of calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrates, hydrochlorides, sulfates, phosphates, citrates or acetates; the second acid radical metal salt includes salts of any one or more elements of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetates, nitrates or sulfates.
[0051] The beneficial effects of the present application will be further explained in detail below in conjunction with specific embodiments.
[0052] Example 1
[0053] 1. Dissolve 44g of sodium silicate (SiO2 mass fraction is 28wt%) in 30g of deionized water, and pretreat in a closed reactor at 25°C for 1 hour to obtain a silicon source gel system; dissolve 6.557g of sodium aluminate in 30g of deionized water, and stir at 25°C for 1 hour to obtain an aluminum source gel system; slowly drop the silicon source gel system into the aluminum source gel system, and continue stirring at 80°C for 18 hours to obtain a gel solution;
[0054] 2. Dissolve 14 g of sodium hydroxide in 36 g of deionized water, add the solution to the gel solution, and control the pH value to be maintained at 12 to obtain a gel slurry solution;
[0055] 3. Place the gel slurry solution into a hydrothermal reactor and perform two-stage temperature-controlled crystallization. The first stage crystallization reaction (second crystallization) is at a temperature of 40°C and a time of 12 h, and the second stage crystallization reaction (third crystallization) is at a temperature of 95°C and a time of 24 h to obtain a crystallized solution.
[0056] 4. Mix 58.35g of sodium silicate, 23.6g of sodium aluminate, 11.65NaOH and 400.54g of H2O to obtain a gel mother liquor. Add 25g of the crystallization solution to the gel mother liquor and continue stirring and aging at 60°C for 12h. Place it in a hydrothermal reaction and perform a crystallization reaction again (the fourth crystallization) at a crystallization temperature of 98°C for 24h. Filter and wash the reaction product, control the pH to 7, and dry it at 90°C to obtain a 13X molecular sieve.
[0057] 5. Metal modification
[0058] S1-a) 13X molecular sieve and pseudo-boehmite are uniformly mixed in a mass ratio of 8.5:1.5, and then 3wt% of ytterbium acetate, 2wt% of methyl cellulose, 1.5wt% of PAO4 and a nitric acid solution with a mass concentration of 1.2wt% are added to form a uniform ball, and after drying at 90°C for 5h, it is calcined at 500°C for 6h to obtain a molecular sieve precursor.
[0059] S2) The molecular sieve precursor and the second reactant are mixed at a mass ratio of 1:45, wherein the mass ratio of sodium hydroxide: sodium silicate: dodecyl dimethyl benzyl ammonium chloride in the second reactant is 4:35:6. After mixing, a crystallization reaction (first crystallization reaction) is performed again, the crystallization temperature is 95° C., the time is 12 hours, and after the crystallization reaction is completed, a calcination treatment at 500° C. is performed for 4 hours to obtain a rare earth metal modified molecular sieve.
[0060] The molar ratio of each component in the rare earth metal modified molecular sieve is: alumina (derived from aluminum source): silicon dioxide (derived from silicon source) = 1:2; alumina: MO = 1:0.1; alumina: MOH = 1:15; alumina: first acid metal salt = 1:15; alumina: second acid metal salt = 1:1.5.
[0061] The XRD (X-ray diffraction) diffraction pattern of the rare earth metal-modified molecular sieve of this embodiment is as follows: Figure 1 As shown, SEM (Scanning Electron Microscope, scanning electron microscope) characterization is as follows Figure 2 shown.
[0062] Example 2
[0063] Steps 1-3 in this embodiment are consistent with those in Embodiment 1.
[0064] 4. Mix 8.197 g of sodium aluminate, 53.65 g of sodium silicate, 12.65 NaOH and 260.45 g of H2O to obtain a gel mother liquor. Add 45 g of the crystallization solution to the gel mother liquor and continue stirring and aging at 60°C for 12 h. Place it in a hydrothermal reaction for crystallization reaction at a crystallization temperature of 98°C and a crystallization time of 24 h. Filter and wash the reaction product, control the pH to 7, and dry it at 90°C to obtain a 13X molecular sieve.
[0065] 5. Metal modification
[0066] S1-a) 13X molecular sieve and pseudo-boehmite are mixed uniformly in a mass ratio of 7.8:2.2, and then 3wt% of ytterbium acetate, 1.5wt% of sesbania powder, 0.5wt% of PAO6 and 1.2wt% of nitric acid solution are added, mixed uniformly and rolled into balls, dried at 50°C for 10h, and calcined at 550°C for 5h to obtain a molecular sieve precursor.
[0067] S2) The molecular sieve precursor and the second reactant are mixed in a mass ratio of 1:45, wherein the mass ratio of sodium hydroxide: sodium silicate: octadecyl dimethyl ammonium chloride is 4:35:6. After mixing, a crystallization reaction is carried out at a crystallization temperature of 100°C for 12 hours. After the crystallization reaction is completed, a calcination treatment at 400°C is carried out for 5 hours to obtain a rare earth metal modified molecular sieve.
[0068] The molar ratio of each component in the rare earth metal modified molecular sieve is: alumina: silica = 1:2.5; alumina: MO = 1:0.1; alumina: MOH = 1:6; alumina: first acid radical metal salt = 1:12; alumina: second acid radical metal salt = 1:1.5.
[0069] The SEM characterization of the rare earth metal modified molecular sieve adsorbent of this example is as follows Figure 3 shown.
[0070] Example 3
[0071] Steps 1-4 in this embodiment are consistent with those in Embodiment 1.
[0072] 5. Metal modification
[0073] S1-b) 1.5 wt% lutetium acetate was ion exchanged (loaded) with 13X molecular sieve (solid-liquid ratio of 1:5) under hydrothermal conditions at 80° C. for 3 h to obtain rare earth Lu-13X molecular sieve.
[0074] The Lu-13X molecular sieve and pseudo-boehmite were mixed in a mass ratio of 8:2, and then 2.5wt% of sesbania powder, 2.5wt% of PAO6 and a nitric acid solution with a mass concentration of 1.5wt% were added, mixed evenly and rolled into balls. After drying at 100°C for 3h, the mixture was calcined at 500°C for 5h to obtain a molecular sieve precursor.
[0075] S2) The molecular sieve precursor and the second reactant are mixed in a mass ratio of 1:45, wherein the mass ratio of sodium hydroxide: sodium silicate: octadecyl dimethyl ammonium chloride is 4:35:6, and after mixing, a crystallization treatment is performed at a crystallization temperature of 95°C for 12 hours, and a calcination treatment is performed at 500°C for 4 hours to obtain a rare earth metal modified molecular sieve.
[0076] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1:2; alumina: MO = 1:0.1; alumina: MOH = 1:6; alumina: first acid metal salt = 1:15; alumina: second acid metal salt = 1:2.5
[0077] Example 4
[0078] Steps 1-2 of this embodiment are consistent with those of embodiment 1.
[0079] 3. 10 g of 200 mesh waste ZSM-5 catalyst (the specific composition of the waste ZSM-5 catalyst is SiO2 content of 79%, Al2O3 content of 20%) and 8 g of 10% NaCO3 are mixed evenly, calcined at 650° C. for 120 min, and then the calcined product is dissolved with a 25% nitric acid solution, filtered to obtain an aluminum-containing solution for standby use, filtered to obtain 10 g of filter residue, and the filter residue is mixed evenly with 6 g NaOH and 40 g H2O to obtain a silicon-containing solution by filtration;
[0080] The aluminum-containing solution and the silicon-containing solution are mixed in a mass ratio of 4 to obtain a gel mother solution.
[0081] 4. Add 15 g of the crystallization solution obtained in step 3 to the gel-like mother liquor and continue stirring and aging at 60 ° C for 12 hours. Place it in a hydrothermal reactor with a crystallization temperature of 95 ° C and a crystallization time of 24 hours. Filter and wash the reaction product, adjust the pH to 7, and dry it at 90 ° C to obtain 13X molecular sieve.
[0082] 5. Metal modification
[0083] S1-a) 13X molecular sieve and pseudo-boehmite are mixed uniformly in a mass ratio of 7.5:2.5, 3wt% of ytterbium acetate, 2.5wt% of ethyl cellulose, 1.5wt% of PAO4, and 1.0wt% of nitric acid solution are added, the mixture is mixed uniformly and rolled into a ball, and the mixture is dried at 110°C for 2h and calcined at 650°C for 3h to obtain a molecular sieve precursor.
[0084] S2) The molecular sieve precursor is mixed with the second reactant in a mass ratio of 1:55, and a mixed solution of sodium hydroxide: sodium silicate: octadecyl dimethyl ammonium chloride in a mass ratio of 5:45:5 in the second reactant is subjected to a crystallization reaction at a crystallization temperature of 95°C for 12 hours, and a calcination treatment at 500°C for 4 hours is performed to obtain a rare earth metal modified molecular sieve.
[0085] The ratio of the amount of each component substance in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1:3.5; alumina: MO salt = 1:0.2; alumina: MOH = 1:25; alumina: first acid root metal salt = 1:10; alumina: second acid root metal salt = 1:2.
[0086] Example 5
[0087] The steps of this embodiment are consistent with steps 1 to 4 in embodiment 1.
[0088] 5. Rare earth metal modification
[0089] S1-a) 13X molecular sieve and pseudo-boehmite are mixed in a mass ratio of 8.2:1.8, and then 1.5wt% neodymium acetate, 1.2wt% magnesium acetate, 1.5wt% lignin, 1.5wt% white oil and 1wt% nitric acid solution are added, mixed evenly and rolled into balls, dried at 50°C for 10h, and calcined at 650°C for 3h to obtain a molecular sieve precursor.
[0090] S2) The molecular sieve precursor is mixed with the second reactant in a mass ratio of 1:50, wherein the second reactant has a mixed solution of sodium hydroxide: sodium silicate: octadecyl dimethyl ammonium chloride in a ratio of 5:35:10, and a crystallization reaction is performed again at a crystallization temperature of 95°C for 12 hours, and a calcination treatment is performed at 500°C for 4 hours to obtain a rare earth metal modified molecular sieve.
[0091] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silica = 1: 3.5; alumina: MO = 1: 0.3; alumina: MOH = 1: 30; alumina: first acid root metal salt = 1: 20; alumina: second acid root metal salt = 1: 3.0.
[0092] Example 6
[0093] The same as steps 1-4 in Example 1.
[0094] 5. Rare earth metal modification
[0095] S1-a) 13X molecular sieve and pseudo-boehmite are mixed uniformly in a mass ratio of 7.5:2.5, 0.8wt% of ytterbium acetate, 0.75wt% of gum arabic, 0.75wt% of PAO4 and 1.1wt% of nitric acid solution are added, the mixture is mixed uniformly and rolled into a ball, and the mixture is dried at 120°C for 1h and calcined at 500°C for 8h to obtain a molecular sieve precursor.
[0096] S2) The molecular sieve precursor is mixed with the second reactant in a mass ratio of 1:35, and the mixed solution of the second reactant in a mass ratio of sodium hydroxide: sodium silicate: isooctyl alcohol of 2.5:28:4.5 is crystallized again at a crystallization temperature of 85°C for 15 hours. After the crystallization reaction is completed, a calcination treatment at 500°C is performed for 4 hours to obtain a rare earth metal modified molecular sieve.
[0097] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1:3.5; alumina: MO = 1:0.25; alumina: MOH = 1:25; alumina: first acid root metal salt = 1:12; alumina: second acid root metal salt = 1:1.5.
[0098] Example 7
[0099] The same as steps 1-4 in Example 1.
[0100] 5. Rare earth metal modification
[0101] S1-a) 13X molecular sieve and pseudo-boehmite are uniformly mixed in a mass ratio of 7.8:2.2, 0.75 wt% of cerium acetate, 1.25 wt% of guar gum, 1.25 wt% of white oil and 1.2 wt% of nitric acid solution are added, and the mixture is uniformly rolled into a ball shape, dried at 40° C. for 15 h, and calcined at 700° C. for 1 h to obtain a molecular sieve precursor.
[0102] S2) The molecular sieve precursor and the second reactant are mixed at a mass ratio of 1:44, wherein the mass ratio of sodium hydroxide: sodium silicate: dihexadecyl dimethyl ammonium chloride in the second reactant is 3.5:38:2.5. After mixing, a crystallization reaction is performed at a crystallization temperature of 80° C. for 15 hours, and after the crystallization reaction is completed, a calcination treatment at 500° C. is performed for 4 hours to obtain a rare earth metal modified molecular sieve.
[0103] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silicon dioxide = 1:2.5; alumina: MO = 1:0.25; alumina: MOH = 1:25; alumina: first acid metal salt = 1:15; alumina: second acid metal salt = 1:2.5.
[0104] Example 8
[0105] The same as steps 1-4 of Example 1.
[0106] 5. Rare earth metal modification
[0107] S1-a) 13X molecular sieve and pseudo-boehmite are mixed in a mass ratio of 7.2:2.8, 2.5wt% neodymium acetate, 1.5wt% cerium acetate, 2.5wt% ethyl cellulose, 1.25wt% PAO6 and 1wt% nitric acid solution are added, the mixture is evenly mixed and rolled into a ball, and the other conditions are the same as in Example 1 to obtain a molecular sieve precursor.
[0108] S2) The molecular sieve precursor and the second reactant are mixed at a mass ratio of 1:45, wherein the mass ratio of sodium hydroxide to sodium silicate in the second reactant is 7:38, and after mixing, a crystallization treatment is performed at a crystallization temperature of 110° C. for 10 hours, and a calcination treatment is performed at 500° C. for 4 hours to obtain a rare earth metal modified molecular sieve.
[0109] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silica = 1:3; alumina: MO = 1:0.5; alumina: MOH = 1:25; alumina: first acid root metal salt = 1:18; alumina: second acid root metal salt = 1:2.25.
[0110] Example 9
[0111] The difference from Example 1 is that the temperature of the first crystallization is 135° C. and the crystallization time is 1.6 h.
[0112] Example 10
[0113] The difference from Example 1 is that the temperature of the first crystallization is 60° C. and the crystallization time is 16 h.
[0114] Embodiment 11
[0115] The difference from Example 1 is that the mass ratio of the molecular sieve precursor to the second reactant is 1:15.
[0116] Example 12
[0117] The difference from Example 1 is that the mass ratio of the molecular sieve precursor to the second reactant is 1:80.
[0118] Comparative Example 1
[0119] The only difference between this comparative example and Example 1 is that the molecular sieve precursor is not subjected to the first crystallization treatment, but is directly subjected to the second calcination to obtain the rare earth metal modified molecular sieve of this comparative example.
[0120] The ratio of the amount of each component in the rare earth metal modified molecular sieve is: alumina: silica = 1:4.5; alumina: MO = 1:0.1; alumina: MOH = 1:15; alumina: first acid metal salt = 1:15; alumina: second acid metal salt = 1:1.5. The SEM characterization of the rare earth modified molecular sieve of this comparative example is as follows Figure 4 As shown, it can be seen that the molecular sieve prepared in this comparative example has low crystallinity and relatively poor grain growth integrity.
[0121] Test example
[0122] The BET surface area (Brunauer-Emmett-Teller), pore volume, BJH (Barrett-Joyner-Halenda) average pore width and conversion rate of the rare earth metal-modified molecular sieves of the above embodiments and comparative examples are shown in Table 1; the molecular sieves modified with rare earth metals of the above embodiments and comparative examples are used to adsorb and remove oxides produced in the fractionation process using C6-C8 hydrocarbons as raw materials in the Fischer-Tropsch synthesis process, and the removal rate results are shown in Table 2, and all molecular sieves are operated for 25 cycles; the molecular sieves modified with rare earth metals of the above embodiments and comparative examples are used to adsorb and remove oxides produced in the oil washing process of naphtha in the Fischer-Tropsch synthesis process using naphtha as raw material, and the removal rate results are shown in Table 3, and all molecular sieves are operated for 20 cycles.
[0123] The method for detecting and calculating the removal rate is as follows: dynamic adsorption is carried out using a fixed bed evaluation device with a filling capacity of 10-200g (manufacturer: Tianjin Pengxiang Technology Co., Ltd., number: 20200706PX042), and the above raw materials are transported to the adsorbent bed from bottom to top through a metering pump at a flow rate of 0.5-4.5ml / min, and the oxygen-containing compound content of the reactor outlet material is collected for detection until the adsorption reaches saturation and the adsorbent is regenerated. The regenerated adsorbent is subjected to an adsorption experiment again, with "adsorption-regeneration-adsorption" as a cycle.
[0124] A gas chromatograph was used to test the content of oxygen-containing compounds before and after adsorption. A polar column was used as the chromatographic column. The gas chromatograph temperature program was set as follows: an initial temperature of 50°C, maintained for 5 min, increased to 80°C at 2°C / min, maintained for 5 min, increased to 100°C at 5°C / min, and increased to 240°C at 20°C / min and maintained for 5 min.
[0125] Calculation method: Removal rate = initial oxide concentration (ppm) / concentration after adsorption (ppm).
[0126] Table 1
[0127]
[0128] Among them, micropores refer to pores with a pore diameter of less than 2 nm, and mesopores refer to pores with a pore diameter of 2 to 50 nm.
[0129] Table 2
[0130] Rare earth metal modified molecular sieves Removal rate (%) Example 1 99.99 Example 2 99.95 Example 3 99.56 Example 4 99.12 Example 5 98.45 Example 6 98.05 Example 7 97.86 Example 8 97.08 Example 9 96.45 Example 10 96.05 Embodiment 11 95.67 Example 12 95.45 Comparative Example 1 93.45
[0131] Table 3
[0132] Rare earth metal modified molecular sieves Removal rate (%) Example 1 99.88 Example 2 99.33 Example 3 98.52 Example 4 98.23 Example 5 96.45 Example 6 95.59 Example 7 94.62 Example 8 94.38 Example 9 93.76 Example 10 93.12 Embodiment 11 92.58 Example 12 91.16 Comparative Example 1 90.25
[0133] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: in the present application, a 13X molecular sieve with controllable crystal form and doped with metal elements on the skeleton is prepared by a dynamic multi-stage crystallization one-pot method, and a molecular sieve adsorbent precursor with rare earth metal atoms loaded in the pores is prepared by using the 13X molecular sieve together with a first aluminum source and rare earth metal acetate. After the molecular sieve precursor is subjected to a crystallization reaction, the rare earth metal-modified molecular sieve in the present application can be obtained, and the specific surface area and pore volume are increased, the pore width is uniform, and the silicon source conversion rate is high. Compared with the molecular sieves in the prior art, when used in the Fischer-Tropsch synthesis process, the molecular sieve of the present application has good adsorption performance and stronger regeneration ability.
[0134] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a rare earth metal modified molecular sieve, characterized in that: The preparation method comprises: S1) mixing 13X molecular sieve and the first reactant to obtain a molecular sieve precursor; S2) mixing the molecular sieve precursor and the second reactant and performing a first crystallization reaction to obtain the rare earth metal-modified molecular sieve; The first reactant includes: a first aluminum source and a first metal salt; The first metal salt is a rare earth metal salt; The second reactant includes: a first alkali source, a first silicon source and a supporting agent.
2. The preparation method according to claim 1, characterized in that: The first aluminum source comprises aluminum oxide; Preferably, the rare earth metal salt comprises: one or more of rare earth metal acetate, rare earth metal nitrate or rare earth metal sulfate; Preferably, the rare earth metal element in the rare earth metal salt includes one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium; Preferably, the rare earth metal acetate salt includes one or more of ytterbium acetate, lutetium acetate, thulium acetate, erbium acetate, gadolinium acetate, holmium acetate, titanium acetate or terbium acetate.
3. The preparation method according to claim 1, characterized in that: The first reactant also includes a pore former, a lubricant, and a first acid source; Preferably, the pore-forming agent comprises one or more of sesbania powder, gum arabic, lignin, guar gum or ethyl cellulose; Preferably, the lubricant comprises a base oil; Preferably, the first acid source includes one or more of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid or acetic acid; more preferably, the first acid source is nitric acid.
4. The preparation method according to claim 3, characterized in that: Said S1) includes S1-a) or S1-b); The S1-a) comprises: the first reactant comprises the 13X molecular sieve, the first aluminum source, the rare earth metal salt, the pore former, the lubricant and the acid source, the first reactant is mixed, a first drying is performed, and a first calcination is performed to obtain the molecular sieve precursor; The step S1-b) comprises: mixing the 13X molecular sieve with the rare earth metal salt for ion exchange, and then mixing with the first aluminum source, the pore-forming agent, the lubricant and the acid source, performing a second drying, and then performing a second calcination to obtain the molecular sieve precursor; Preferably, the temperature of the first drying is 50-120°C, and the time of the first drying is 0.1-30h; Preferably, the temperature of the first calcination is 400-650°C, and the time of the first calcination is 0.1-48h; Preferably, the temperature of the second drying is 50-120°C, and the time of the second drying is 0.1-30h; Preferably, the temperature of the second calcination is 400-650°C, and the time of the second calcination is 0.1-48h; Preferably, the ion exchange is carried out at a temperature of 50-120° C. and for a time of 0.1-5 h.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the 13X molecular sieve to the first aluminum source is (5-10): (1-5); Preferably, the mass of the rare earth metal salt accounts for 2.5-5wt% of the total mass of the first reactant; Preferably, the mass of the pore former accounts for 1-3wt% of the total mass of the first reactant; Preferably, the mass of the lubricant accounts for 1-3wt% of the total mass of the first reactant; Preferably, the mass of the acid source accounts for 0.5-1.5 wt % of the total mass of the first reactant.
6. The preparation method according to claim 1, characterized in that: The first alkali source includes one or more of sodium hydroxide, sodium carbonate, calcium hydroxide, potassium hydroxide or ammonia water; Preferably, the first silicon source includes one or more of sodium silicate, silica sol, chromatography silica gel, methyl orthosilicate or ethyl orthosilicate; Preferably, the supporting agent includes one or more of dihexadecyldimethylammonium chloride, isooctyl alcohol, polyethylene glycol ether, ethanolamine, dodecyldimethylbenzylammonium chloride, octadecyldimethylammonium chloride, hydroxyethylethylenediamine or didecyldimethylammonium chloride.
7. The preparation method according to claim 1 or 6, characterized in that: The step S2) comprises: mixing the molecular sieve precursor and the second reactant at a mass ratio of 1:20 to 60, performing the first crystallization reaction, and then performing a third calcination to obtain the rare earth metal modified molecular sieve; Preferably, in the second reactant, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (0.1-8): (3-50): (0.5-15); more preferably, the mass ratio of the first alkali source, the first silicon source and the supporting agent is (1-5): (20-40): (1-8); Preferably, the temperature of the first crystallization reaction is 85-110° C., and the time of the first crystallization reaction is 4-36 h; Preferably, the temperature of the third calcination is 300-600° C., and the time of the third calcination is 2-24 hours.
8. The preparation method according to claim 1, characterized in that: The preparation method of the 13X molecular sieve comprises: a) mixing a second aluminum source, a second metal salt and water to obtain an aluminum source gel system; uniformly mixing a second silicon source and water to obtain a silicon source gel system; and mixing the aluminum source gel system and the silicon source gel system to obtain a gel solution; b) mixing the gel solution with a second alkali source to obtain a gel slurry solution; c) subjecting the gel slurry solution to a second crystallization reaction and a third crystallization reaction to obtain a crystallized solution; d) mixing the aluminum-containing solution, the silicon-containing solution and the third alkali source to obtain a gel mother solution; e) mixing the gel mother solution with the crystallization solution, performing an aging reaction and a fourth crystallization reaction to obtain the 13X molecular sieve; Preferably, the second metal salt comprises a metal salt of any one or more of the following elements: calcium, magnesium, cerium, potassium, lanthanum or neodymium.
9. The preparation method according to any one of claims 1, characterized in that The molar ratio of each component in the rare earth metal modified molecular sieve is: Alumina:silicon dioxide = 1:0.5-10; Alumina: MO = 1: 0.001-0.5; Alumina: MOH = 1: 5-30; Alumina: first acid metal salt = 1: 0.5-20; Alumina: second acid metal salt = 1: 0.02-5; The MO is an oxide of an active metal in the rare earth metal modified molecular sieve, and the MOH is a hydroxide of an active metal in the rare earth metal modified molecular sieve. The active metal includes: any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; The first acid metal salt comprises a salt of any one or more elements selected from calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrate, hydrochloride, sulfate, phosphate, citrate or acetate; The second acid metal salt includes salts of any one or more elements selected from ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetate, nitrate or sulfate.
10. A rare earth metal modified molecular sieve prepared by the method for preparing a rare earth metal modified molecular sieve according to any one of claims 1 to 9; the molar ratio of each component in the rare earth metal modified molecular sieve is: aluminum oxide: silicon dioxide = 1: 0.5-10; Alumina: MO = 1: 0.001-0.5; Alumina: MOH = 1: 5-30; Alumina: first acid metal salt = 1: 0.5-20; Alumina: second acid metal salt = 1: 0.02-5; The MO is an oxide of an active metal in the rare earth metal modified molecular sieve, and the MOH is a hydroxide of an active metal in the rare earth metal modified molecular sieve. The active metals include: Any one or more of ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, and Any one or more of calcium, magnesium, cerium, potassium, lanthanum or neodymium; The first acid metal salt comprises a salt of any one or more elements selected from calcium, magnesium, cerium, potassium, lanthanum or neodymium, each independently selected from nitrate, hydrochloride, sulfate, phosphate, citrate or acetate; The second acid metal salt includes salts of any one or more elements selected from ytterbium, lutetium, thulium, erbium, gadolinium, holmium, titanium or terbium, each independently selected from acetate, nitrate or sulfate.
Citation Information
Cited By
Renewable adsorbent for naphtha purification as well as preparation method and application thereof