Water pollution treatment agent prepared based on solid waste and preparation method thereof
By preparing defective perovskite/diatomite composite materials with interconnected internal and external micropores, the problems of high water pollution treatment costs and perovskite waste disposal were solved, achieving efficient and stable water pollution treatment results.
Patent Information
- Application Number
- CN202411093308.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing water pollution treatment methods suffer from high costs, high energy consumption, and secondary pollution, and the treatment and recycling of perovskite battery waste has not been effectively resolved.
By using perovskite waste and materials such as carbon powder and diatomaceous earth, a defective perovskite/diatomaceous earth composite material was prepared through steps such as pyrolysis, ball milling, alkaline solution treatment and double-network gel microsphere coating, forming a composite material with interconnected internal and external micropores.
It improves the catalytic activity and adsorption performance of the material, enabling it to effectively adsorb a variety of pollutants. It has superior water pollution treatment capabilities, adapts to extreme environments, and exhibits self-healing and good cycle stability.
Smart Images

Figure BDA0004987175510000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water pollution treatment agents, and in particular to a water pollution treatment agent prepared based on solid waste and a preparation method thereof. Background Art
[0002] With the rapid development of industrialization and urbanization, water pollution has become increasingly serious and has become one of the environmental issues of global concern. Although traditional water pollution treatment methods such as chemical precipitation, adsorption, membrane separation and biological treatment can effectively remove pollutants in water to a certain extent, these methods often have problems such as high cost, high energy consumption and secondary pollution.
[0003] Solid waste can be divided into domestic waste, industrial waste, construction waste, etc. according to its source and composition. Domestic waste mainly includes food residues, paper, plastic, etc.; industrial waste includes wastewater, waste gas, waste residue, etc.; construction waste comes from the process of construction, demolition and decoration. These wastes have complex physical, chemical and biological properties, such as stability, decomposability, toxicity, flammability, solubility, etc., which provide a rich raw material basis for the preparation of water pollution treatment agents.
[0004] Perovskite is a material with disruptive potential in the field of photovoltaic cells. It has the advantages of high conversion efficiency and low cost. However, as the commercialization of perovskite cells progresses, the problem of handling and recycling perovskite waste, namely titanium dioxide powder, has gradually emerged. Perovskite cells contain toxic substances, such as lead, which need to be properly handled to avoid pollution to the environment.
[0005] Therefore, it is necessary to develop a method for preparing a water pollution treatment agent based on perovskite waste, namely titanium dioxide powder, to solve the technical problems. Summary of the invention
[0006] The purpose of the present invention is to provide a water pollution treatment agent prepared based on solid waste and a preparation method thereof, so as to solve the problems existing in the prior art.
[0007] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a water pollution treatment agent based on solid waste, comprising the following preparation steps:
[0008] (1) immersing the waste perovskite, i.e., titanium dioxide powder and carbon powder, in concentrated nitric acid, heating, stirring, and drying; placing the dried mixture in a container, pyrolyzing it at high temperature under a nitrogen atmosphere, and washing and drying it after pyrolysis;
[0009] (2) placing the washed and dried object into a ball mill, washing it with anhydrous ethanol and deionized water, and drying it to obtain a defective perovskite; dissolving the defective perovskite in DMF to prepare a precursor solution;
[0010] (3) soaking diatomite in a sodium hydroxide solution, washing the material with water, mixing it with a precursor solution, adding a porogen, stirring evenly, drying and dehydrating to obtain a defective perovskite / diatomite composite powder containing a porogen, and then sintering at a high temperature and cooling to obtain a defective perovskite / diatomite composite material;
[0011] (4) mixing isopropyl orthosilicate and ethanol, then gradually adding ammonia solution, stirring sufficiently, reacting completely, and centrifuging and washing to obtain silica microspheres having a first network;
[0012] (5) gradually adding acrylamide, an initiator, a crosslinking agent, and a catalyst into a container, mixing and stirring uniformly to obtain a second network precursor solution;
[0013] (6) soaking the silica microspheres in a second network precursor solution, allowing the precursor solution to penetrate into the interior of the silica microspheres, heating and raising the temperature to perform a polymerization reaction to form a second network, thereby obtaining a double network gel microsphere precursor solution;
[0014] (7) Immersing the sintered defective perovskite / diatomaceous earth composite material in a double network gel microsphere precursor solution, stirring evenly, heating to complete the reaction to form a double network gel microsphere coating layer, filtering, and washing with anhydrous ethanol to obtain a water pollution treatment agent prepared based on solid waste.
[0015] Furthermore, the mass proportions of each raw material are: 10 to 20 parts of titanium dioxide powder, 1 to 3 parts of carbon powder, 2 to 3 parts of porogen, 50 to 70 parts of diatomaceous earth, 30 to 40 parts of isopropyl orthosilicate, 30 to 50 parts of acrylamide, 1 to 3 parts of catalyst, 0.3 to 0.5 parts of initiator, and 0.5 to 1 parts of cross-linking agent.
[0016] Furthermore, the porogen is one of didodecyldimethylammonium bromide, sodium dodecylbenzenesulfonate, and dodecyldimethylammonium bromide.
[0017] Furthermore, the catalyst is one or more of triethylamine and ethylenediamine.
[0018] Furthermore, the initiator is one or more of ammonium sulfate, potassium persulfate, and sodium persulfate; and the cross-linking agent is N,N'-methylenebisacrylamide.
[0019] Furthermore, the pyrolysis in step (1) is carried out in a tubular furnace, the heating rate is 8-10°C / min and the pyrolysis temperature is 500°C-550°C; the mass concentration of concentrated nitric acid in step (1) is 30%-35%.
[0020] Furthermore, the ball mill in step (2) is a planetary ball mill with a rotation speed of 400-450 rpm and a ball milling time of 10-12 h; and the high-temperature sintering temperature in step (3) is 480-520° C. and the time is 1-2 h.
[0021] Furthermore, the mass concentration of the ammonia water in step (4) is 20% to 25%; and the particle size of the silica microspheres in step (4) is 350 to 550 nm.
[0022] Furthermore, the polymerization reaction temperature in step (6) is between 55 and 65° C.; and the reaction temperature in step (7) when forming the double network gel microsphere coating layer is between 55 and 65° C.
[0023] Furthermore, a water pollution treatment agent is provided, and the treatment agent is prepared according to the method described.
[0024] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0025] The present invention prepares defective perovskite through two physical and chemical methods, namely pyrolysis and ball milling, controls the reaction conditions to introduce lattice defects to control the photoelectric properties of the perovskite, controls the concentration and distribution of localized electronic states to improve the catalytic activity, forms a synergistic effect with the introduced nano-activated carbon powder, and has a strong catalytic effect and adsorption performance on pollutants.
[0026] The present invention uses an alkaline solution to soak the diatomite, removes surface impurities and performs purification treatment. The corrosion of the alkaline solution can expose more Si-OH groups on the surface, increase the specific surface area and microporosity, and improve the stability of the micropores. The diatomite is then mixed with the defective perovskite, a porogen is added, and high-temperature sintering is performed. After the perovskite is melted, it is dispersed into the microporous structure of the diatomite to form a defective perovskite / diatomite composite material, thereby improving the dispersion of the micropores and enhancing its adsorption performance.
[0027] The present invention uses a double network gel microsphere structure to coat diatomite sintered with defective perovskite, uses isopropyl orthosilicate as the monomer material of the first layer of the network, and the silica microspheres generated by isopropyl orthosilicate after hydrolysis and condensation reaction are cross-linked to form a network. The microspheres have a high specific surface area and a porous structure, which helps to improve the adsorption capacity of the material; acrylamide is used as the monomer material of the second layer of the network structure, while improving the specific surface area and microporous structure, the overall mechanical properties are improved, and the acrylamide-based double network hydrogel has excellent self-healing properties, good cyclic stability, and can maintain efficient pollutant treatment capabilities for a long time. In addition, the porous structure of the double-layer network provides more active sites, which are connected with the micropores of the diatomite to form a composite material with internal and external micropores connected. The micropores are connected, and the layers are progressive, which improves the ability to capture pollutants, can effectively adsorb a variety of pollutants, and degrade by themselves, and has excellent water pollution treatment capabilities. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the water pollution treatment agent prepared in the following examples are as follows:
[0030] COD average value: HJ / T 399-2007;
[0031] Turbidity: HJ 1075-2019;
[0032] Removal rate: 1-(COD 去除 / COD 初始 )*100% (initial sewage: COD average value is 10350mg / l, turbidity is 1045NTU);
[0033] Chemical property stability: The samples were immersed in buffer solutions with pH values of 2 and 12, respectively, and then placed in the initial sewage to test the COD value after treatment and compare it with the COD value of the sample after treatment without immersion treatment.
[0034] Example 1
[0035] (1) 15 parts of titanium dioxide powder and 2 parts of carbon powder were immersed in concentrated nitric acid with a mass concentration of 30%, stirred at 80°C for 2 hours, and dried; the dried mixture was placed in a container, pyrolyzed at 525°C for 2 hours in a nitrogen atmosphere, and washed and dried after pyrolysis;
[0036] (2) placing the washed and dried object in a ball mill for 11 hours, washing with anhydrous ethanol and deionized water, and drying to obtain a defective perovskite; taking 15 parts of the defective perovskite and dissolving it in DMF to prepare a defective perovskite precursor solution;
[0037] (3) 60 parts of diatomite were soaked in a sodium hydroxide solution for 2.5 hours, the material was washed with water and mixed with a defective perovskite precursor solution, 2 parts of dodecyl dimethyl ammonium bromide were added as a porogen, stirred evenly, dried at 60° C. for 10 hours to obtain a defective perovskite / diatomite composite powder containing a porogen, sintered at 500° C. for 1.5 hours, and cooled to obtain a defective perovskite / diatomite composite material;
[0038] (4) 35 parts of isopropyl orthosilicate and 20 parts of ethanol were mixed, and then a 25% ammonia aqueous solution was gradually added dropwise, and the mixture was stirred thoroughly. After reacting for 1.5 hours, the mixture was centrifuged and washed to obtain silica microspheres having a first network;
[0039] (5) gradually adding 40 parts of acrylamide, 0.4 parts of potassium persulfate, 2 parts of ethylenediamine, and 0.5 parts of N,N'-methylenebisacrylamide into a container and mixing and stirring to obtain a second network precursor solution;
[0040] (6) soaking 15 parts of silica microspheres in 25 parts of the second network precursor solution, allowing the precursor solution to penetrate into the interior of the silica microspheres, maintaining the temperature at 60° C., performing a polymerization reaction to form a second network, and obtaining a double network gel microsphere precursor solution;
[0041] (7) Immersing 15 parts of the sintered defective perovskite / diatomaceous earth composite material in 20 parts of the double network gel microsphere precursor solution, stirring evenly, reacting at 60° C. for 1.5 hours to form a double network gel microsphere coating layer, filtering, and washing with anhydrous ethanol to obtain the water pollution treatment agent prepared based on solid waste.
[0042] Example 2
[0043] (1) immersing 10 parts of titanium dioxide powder and 1 part of carbon powder in concentrated nitric acid with a mass concentration of 30%, stirring at 75° C. for 2 hours, and drying; placing the dried mixture in a container, pyrolyzing it at 500° C. for 1 hour in a nitrogen atmosphere, and washing and drying after pyrolysis;
[0044] (2) placing the washed and dried object in a ball mill for 10 hours, washing it with anhydrous ethanol and deionized water, and drying it to obtain a defective perovskite; taking 10 parts of the defective perovskite and dissolving it in DMF to prepare a defective perovskite precursor solution;
[0045] (3) 50 parts of diatomite were soaked in a sodium hydroxide solution for 2 hours, the material was washed with water and mixed with a defective perovskite precursor solution, 2 parts of dodecyl dimethyl ammonium bromide were added as a porogen, the mixture was stirred evenly and dried at 55° C. for 8 hours to obtain a defective perovskite / diatomite composite powder containing a porogen, the powder was sintered at 480° C. for 1 hour, and the defective perovskite / diatomite composite material was obtained after cooling;
[0046] (4) 30 parts of isopropyl orthosilicate and 20 parts of ethanol were mixed, and then a 25% ammonia aqueous solution was gradually added dropwise, and the mixture was stirred sufficiently. After reacting for 1 hour, the mixture was centrifuged and washed to obtain silica microspheres having a first network;
[0047] (5) gradually adding 30 parts of acrylamide, 0.3 parts of potassium persulfate, 1 part of ethylenediamine, and 0.5 parts of N,N'-methylenebisacrylamide into a container and mixing and stirring to obtain a second network precursor solution;
[0048] (6) soaking 10 parts of silica microspheres in 20 parts of the second network precursor solution, allowing the precursor solution to penetrate into the interior of the silica microspheres, maintaining the temperature at 55° C., performing a polymerization reaction to form a second network, and obtaining a double network gel microsphere precursor solution;
[0049] (7) Immersing 10 parts of the sintered defective perovskite / diatomaceous earth composite material in 15 parts of the double network gel microsphere precursor solution, stirring evenly, reacting at 55° C. for 1 hour to form a double network gel microsphere coating layer, filtering, and washing with anhydrous ethanol to obtain the water pollution treatment agent prepared based on solid waste.
[0050] Example 3
[0051] (1) 20 parts of titanium dioxide powder and 3 parts of carbon powder were immersed in concentrated nitric acid with a mass concentration of 35%, stirred at 85°C for 2 hours, and dried; the dried mixture was placed in a container, pyrolyzed at 550°C for 2 hours in a nitrogen atmosphere, and washed and dried after pyrolysis;
[0052] (2) placing the washed and dried object in a ball mill for 12 hours, washing with anhydrous ethanol and deionized water, and drying to obtain a defective perovskite; taking 20 parts of the defective perovskite and dissolving it in DMF to prepare a defective perovskite precursor solution;
[0053] (3) 70 parts of diatomite were soaked in a sodium hydroxide solution for 3 hours, the material was washed with water and mixed with a defective perovskite precursor solution, 3 parts of dodecyl dimethyl ammonium bromide were added as a porogen, stirred evenly, dried at 65° C. for 10 hours to obtain a defective perovskite / diatomite composite powder containing a porogen, sintered at 520° C. for 2 hours, and cooled to obtain a defective perovskite / diatomite composite material;
[0054] (4) 40 parts of isopropyl orthosilicate and 20 parts of ethanol were mixed, and then a 25% ammonia aqueous solution was gradually added dropwise, and the mixture was stirred sufficiently. After reacting for 2 hours, the mixture was centrifuged and washed to obtain silica microspheres having a first network;
[0055] (5) gradually adding 50 parts of acrylamide, 0.5 parts of potassium persulfate, 1 part of ethylenediamine, and 1 part of N,N'-methylenebisacrylamide into a container and mixing and stirring to obtain a second network precursor solution;
[0056] (6) soaking 20 parts of silica microspheres in 30 parts of the second network precursor solution, allowing the precursor solution to penetrate into the interior of the silica microspheres, maintaining the temperature at 65° C., performing a polymerization reaction to form a second network, and obtaining a double network gel microsphere precursor solution;
[0057] (7) Immersing 20 parts of the sintered defective perovskite / diatomaceous earth composite material in 25 parts of the double network gel microsphere precursor solution, stirring evenly, reacting at 65° C. for 2 hours to form a double network gel microsphere coating layer, filtering, and washing with anhydrous ethanol to obtain the water pollution treatment agent prepared based on solid waste.
[0058] Comparative Example 1
[0059] The difference between Comparative Example 1 and Example 1 is that in step (1), step (1) is changed to immersing 15 parts of titanium dioxide powder in concentrated nitric acid with a mass concentration of 30%, stirring at 80°C for 2h, and drying; placing the dried mixture in a container, pyrolyzing it at 525°C for 2h under a nitrogen atmosphere, and washing and drying after pyrolysis; the remaining steps are the same as in Example 1.
[0060] Comparative Example 2
[0061] The difference between Comparative Example 2 and Example 1 lies in step (1) and step (2). Step (1) and step (2) are changed to immerse 15 parts of titanium dioxide powder and 2 parts of carbon powder in concentrated nitric acid, stir at 80°C for 2h, filter, add dimethyl sulfoxide to dissolve, transfer the mixed solution to an autoclave, heat to 175°C, react for 2h to obtain perovskite, take 15 parts of perovskite and dissolve it in DMF to prepare a perovskite precursor solution, and the remaining steps are the same as Example 1.
[0062] Comparative Example 3
[0063] The difference between Comparative Example 3 and Example 1 is that in step (3), 60 parts of diatomite are mixed with the precursor solution, 2 parts of dodecyl dimethyl ammonium bromide are added as a porogen, stirred evenly, dried at 60° C. for 10 h to obtain a defective perovskite / diatomite composite powder containing a porogen, sintered at 500° C. for 1.5 h, and cooled to obtain a defective perovskite / diatomite composite material; the remaining steps are the same as in Example 1.
[0064] Comparative Example 4
[0065] The difference between Comparative Example 4 and Example 1 lies in steps (5), (6) and (7). Steps (5), (6) and (7) are changed to taking 20 parts of commercially available silica microspheres, dissolving them in deionized water, preparing a silica microsphere precursor solution, immersing 15 parts of the sintered perovskite / diatomaceous earth composite material in 20 parts of the silica gel microsphere precursor solution, stirring evenly, reacting at 60° C. for 2 hours to form a silica gel microsphere coating layer, filtering and washing with anhydrous ethanol; the remaining steps are the same as Example 1.
[0066] Effect example
[0067] Table 1 below shows the performance analysis results of water pollution treatment agents prepared based on solid waste using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.
[0068] Table 1
[0069]
[0070] From the data comparison of the comparative examples, it can be found that the present invention uses perovskite waste as raw material, adds carbon powder, uses pyrolysis and ball milling to prepare defective perovskite, and then adds pore-forming agent to diatomite treated with alkaline solution for high-temperature sintering, disperses the defective perovskite in the microporous structure of diatomite, and then uses double-network gel microspheres for coating, uses tetraethyl orthosilicate as the monomer of the first layer network, and uses acrylamide as the monomer of the second layer network to form a composite material with internal and external micropores connected. The water pollution treatment agent prepared from solid waste of the present invention has excellent photocatalytic properties and adsorption properties, can efficiently treat water pollution, can adapt to extreme environments of excessive acidity and alkalinity, and has excellent self-healing properties and good cycle stability, and can maintain efficient pollutant treatment capabilities for a long time.
[0071] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and no mark in the claims should be regarded as limiting the claims involved.
Claims
1. A method for preparing a water pollution treatment agent based on solid waste, It is characterized in that The method comprises the following preparation steps: (1) immersing the waste perovskite, i.e., titanium dioxide powder and carbon powder, in concentrated nitric acid, heating, stirring, and drying; placing the dried mixture in a container, pyrolyzing it at high temperature under a nitrogen atmosphere, and washing and drying it after pyrolysis; (2) placing the washed and dried object into a ball mill, washing it with anhydrous ethanol and deionized water, and drying it to obtain a defective perovskite; dissolving the defective perovskite in DMF to prepare a defective perovskite precursor solution; (3) soaking diatomite in a sodium hydroxide solution, washing the material with water, mixing it with a defective perovskite precursor solution, adding a porogen, stirring evenly, drying and dehydrating to obtain a defective perovskite / diatomite composite powder containing a porogen, and then sintering at a high temperature, and cooling to obtain a defective perovskite / diatomite composite material; (4) mixing isopropyl orthosilicate and ethanol, then gradually adding ammonia solution, stirring sufficiently, reacting completely, and centrifuging and washing to obtain silica microspheres having a first network; (5) gradually adding acrylamide, an initiator, a crosslinking agent, and a catalyst into a container, mixing and stirring uniformly to obtain a second network precursor solution; (6) soaking the silica microspheres in the second network precursor solution, allowing the precursor solution to penetrate into the interior of the silica microspheres, heating and raising the temperature to perform a polymerization reaction to form a second network, thereby obtaining a double network gel microsphere precursor solution; (7) Immersing the sintered defective perovskite / diatomaceous earth composite material in a double network gel microsphere precursor solution, stirring evenly, heating to complete the reaction to form a double network gel microsphere coating layer, filtering, and washing with anhydrous ethanol to obtain a water pollution treatment agent prepared based on solid waste.
2. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The mass proportions of each raw material are: 10-20 parts of titanium dioxide powder, 1-3 parts of carbon powder, 2-3 parts of porogen, 50-70 parts of diatomaceous earth, 30-40 parts of isopropyl orthosilicate, 30-50 parts of acrylamide, 1-3 parts of catalyst, 0.3-0.5 parts of initiator, and 0.5-1 parts of cross-linking agent.
3. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The porogen is one of didodecyl dimethyl ammonium bromide, sodium dodecyl benzene sulfonate and dodecyl dimethyl ammonium bromide.
4. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The catalyst is one or more of triethylamine and ethylenediamine.
5. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The initiator is one or more of ammonium sulfate, potassium persulfate, and sodium persulfate; and the cross-linking agent is N,N'-methylenebisacrylamide.
6. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The pyrolysis in step (1) is carried out in a tubular furnace, the heating rate is 8-10° C. / min and the pyrolysis temperature is 500° C.-550° C.; the mass concentration of concentrated nitric acid in step (1) is 30%-35%.
7. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The ball mill in step (2) is a planetary ball mill with a rotation speed of 400-450 rpm and a ball milling time of 10-12 hours; the high-temperature sintering temperature in step (3) is 480-520° C. and the time is 1-2 hours.
8. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The mass concentration of the ammonia water in step (4) is 20% to 25%; the particle size of the silica microspheres in step (4) is 350 to 550 nm.
9. A method for preparing a water pollution treatment agent based on solid waste according to claim 1, It is characterized in that The polymerization reaction temperature in step (6) is 55-65°C; and the reaction temperature in step (7) when forming the double network gel microsphere coating layer is 55-65°C.
10. A water pollution treatment agent, It is characterized in that The treating agent is prepared according to the method according to any one of claims 1-9.
Citation Information
Patent Citations
Preparation method and use of three-dimensional nano-perovskite-type composite heterogeneous Fenton catalyst
CN103785394A
Porous perovskite type catalyst LaCo0. 7Fe0. 3O3 as well as preparation method and application thereof
CN116196933A
Method for preparation of perovskite quantum dot (PQD) / polymer / ceramic ternary complex
US20200385632A1
Solid-state perovskite cluster and preparation method therefor, and photoelectric device
WO2023070876A1