Preparation and application of Cu-based spinel oxide catalyst

By dispersing Cu species into spinel lattice, designing CuMgFe-LDH precursor to prepare Cu-based spinel oxide catalysts, solving the problem of poor activity of Cu-based catalysts at high temperatures, and achieving efficient CO2 conversion and stability Suitable for industrial applications.

CN118925726AInactive Publication Date: 2024-11-12BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202410977452.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing Cu-based catalysts have poor high-temperature catalytic activity in the reverse water gas transformation reaction, and are costly, making it difficult to maintain stability at high temperatures, and the CO2 conversion efficiency is less than 60%.

Method used

By dispersing Cu species into spinel lattice, designing a trimetal catalyst, using CuMgFe-LDH as the precursor, preparing Cu-based spinel oxide catalyst through high-temperature calcination, and converting LDH structure into spinel oxide, improving the Cu species dispersion and catalytic activity.

Benefits of technology

The CO2 conversion rate is close to 74% at 800°C, the CO selectivity reaches 100%, and the catalytic activity and stability are maintained at high temperatures. The preparation method is simple and the production cost is low, which is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925726A_ABST
    Figure CN118925726A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a Cu-based spinel oxide catalyst, and CuMgFe-LDH is used as a precursor, and the Cu-based spinel oxide catalyst (CuMgFe-MMO) is obtained through high-temperature calcination. The CuMgFe-MMO catalyst provided by the invention has very high RWGS reaction activity at high temperature, and after the metal proportion of the catalyst is optimized, the CO2 conversion rate at 800 DEG C is close to 74%, and the CO selectivity is close to 100%. Results show that Cu ions in the catalyst are selectively doped into MgFe spinel crystal lattices, part of tetrahedral positions and octahedral positions are occupied, spinel phase crystal lattice distortion is caused by ion radius difference between doped Cu < 2 + > and original cations, and formation of an oxygen defect structure is promoted; oxygen deficiency promotes adsorption and activation of CO2 molecules, Cu serves as an active center of a CO2 hydrogenation reaction, and meanwhile the activity and selectivity of an RWGS reaction are promoted. Besides, Cu is selectively doped into spinel crystal lattices and is dispersed and isolated in the spinel crystal lattices, so that the dispersity of Cu species is improved, and meanwhile, high-temperature sintering of the Cu-based catalyst is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation and application, and discloses a method for preparing a Cu-based spinel oxide catalyst and application of the Cu-based spinel oxide catalyst prepared by the preparation method in a reverse water-gas shift reaction process. Background Art

[0002] The impact of excessive CO2 emissions on climate change due to the combustion of fossil fuels has triggered global research on efficient CO2 capture and utilization technologies. Among them, catalytic CO2 hydrogenation is a very promising method for converting the increasing amount of CO2 emissions into synthesis gas and high-value-added chemicals. The reduction of CO2 to CO and water by hydrogenation, also known as the reverse water gas shift reaction, is considered to be the most common and most promising choice for CO2. The current advanced process for converting CO into high-value-added chemicals has been in existence for a long time, and there has also been relatively mature research on the catalytic conversion of CO. Therefore, the development of reverse water gas shift reaction catalysts with high efficiency, high stability and high selectivity is of great significance to the utilization of CO2 and the regeneration of energy.

[0003] Improving the activity and long-term stability of catalysts is a major challenge faced by the reverse water gas reaction. The catalysts used for the reverse water gas shift reaction that have been extensively studied include but are not limited to four types: non-precious metal catalysts, precious metal catalysts, metal oxides, and transition metal carbide catalysts. Precious metal catalysts are highly active, but their cost is too high; non-precious metal catalysts have lower costs and excellent catalytic performance. Among them, Cu-based catalysts, as proven high-efficiency reverse water gas shift reaction catalysts, have the advantages of high selectivity and low cost. They are often used in CO2 hydrogenation reactions and show high catalytic performance, and are considered to be one of the substitutes for precious metals. However, since Cu-based catalysts are easy to sinter at high temperatures, their high-temperature catalytic activity in the RWGS reaction is poor. Studies have found that in Cu-based catalyst systems, when different precipitants, carriers, and preparation methods are used, the activity of Cu-based catalysts is affected to a certain extent. Common Cu-based catalysts include Cu / CeO2, Cu / Al2O3, and Cu / Zn-Al-O. Due to the limitations of temperature and thermodynamic equilibrium, the CO2 conversion efficiency of the above-mentioned Cu-based catalysts is difficult to exceed 60%. Studies have shown that changing the dispersion form of Cu species, improving the dispersion of Cu species, and adding second and third metal additives to utilize metal-support interactions will be important determinants for improving the high-temperature activity of Cu-based catalysts.

[0004] Based on this, the present invention disperses Cu species into the spinel lattice to design a trimetallic catalyst to improve the catalyst activity. Summary of the invention

[0005] In view of the above-mentioned deficiencies, the object of the present invention is to provide a method for preparing a Cu-based spinel oxide catalyst by high-temperature calcination using CuMgFe-LDH as a precursor and applying it to the reverse water-gas shift reaction under high temperature and normal pressure. It is used to solve the problem of high-temperature stability commonly required by the current reverse water-gas shift catalyst. The CuMgFe-MMO prepared by the present invention has the characteristics of high dispersion of active metal nanoparticles and high high-temperature catalytic activity. The raw materials of the present invention are cheap and easy to obtain, the preparation method is simple, it is conducive to large-scale industrial production, and has significant economic and social benefits.

[0006] To achieve the above object, the present invention provides a method for preparing a Cu-based spinel oxide catalyst and applies the same to the reverse water gas shift reaction, in view of the problems of high temperature sintering and low selectivity in the prior art. The present invention is achieved by the following technical means:

[0007] The present invention discloses a method for preparing a Cu-based spinel oxide catalyst, and the specific steps are as follows:

[0008] (1) Dissolving Cu(NO3)2·3H2O, Mg(NO3)2·6H2O, and Fe(NO3)3·9H2O in deionized water at a predetermined molar ratio, wherein the total concentration of all metal ions is 1 mol / L, and the volume of deionized water used is 50 to 100 ml, to obtain a first solution;

[0009] (2) respectively dissolving NaOH and Na2CO3 in deionized water, wherein the concentration of NaOH is 1.6 to 2 times the concentration of metal ions, the concentration of Na2CO3 is 1.6 to 2 times the concentration of trivalent metal ions, and the volume of deionized water used is 50 to 100 ml, to obtain a second solution;

[0010] (3) pouring the first solution and the second solution into a colloid mill at room temperature, mixing them quickly, and stirring them at a speed of 4000 to 5000 r / min for 3 to 5 minutes to obtain a third product;

[0011] (4) placing the third product in a reaction kettle for hydrothermal crystallization at 100-120° C. for 10-12 hours, followed by washing, drying, and grinding to obtain a CuMgFe-LDH precursor;

[0012] (5) The CuMgFe-LDH precursor is heated from room temperature to 1000° C. in a muffle furnace at a heating rate of 5 to 10° C. / min and maintained for 4 to 6 hours to obtain a Cu-based spinel oxidizing agent.

[0013] The invention also discloses a Cu-based spinel oxide catalyst prepared according to the preparation method.

[0014] The present invention also discloses an application of the Cu-based spinel oxide catalyst in a reverse water-gas shift reaction process.

[0015] Furthermore, the application includes:

[0016] Weigh 20 mg of catalyst and 500 mg of quartz sand, mix them evenly and put them into a quartz tube, then put the quartz tube into a continuous fixed bed reactor and introduce a mixed gas. Under normal pressure, the mixed gas is CO2 and H2 and the balance gas Ar. The catalytic performance is examined at 600-800°C. Finally, at 800°C, the CO2 conversion rate is close to 74%, and the CO selectivity is close to 100%.

[0017] Furthermore, the volume ratio of H2, CO2 and Ar is 3:1:1; the mixed gas flow rate is 80 ml / min (i.e. GHSV = 240000 ml g -1 h -1 ).

[0018] The beneficial effects of the present invention are:

[0019] 1. The present invention uses LDH as a precursor and converts it into spinel oxide through a specific heat treatment process. The catalyst prepared in this way will have the advantages of a large specific surface area and more dispersed active components.

[0020] 2. The content of trivalent cations in the LDH structure is usually half of that of divalent cations, which is different from the ratio in the spinel structure. That is, when LDH is heat-treated to form spinel, excess divalent cations will form their oxides. Since the distribution of divalent and trivalent cations in the LDH layer is orderly and uniform, the distribution of spinel species and oxide species formed after heat treatment is also uniform. Therefore, in the nano-hybrid spinel oxidizer synthesized from the LDH precursor, the spinel and divalent metal oxides are well dispersed and combined at the nanoscale to form a wider interface. The two-phase interface gives the catalyst additional oxygen vacancies, enhancing CO2 adsorption and dissociation; Cu ions are selectively doped into the MgFe spinel lattice, occupying part of the tetrahedral and octahedral sites. The difference in ionic radius between the doped Cu ions and the original cations causes the spinel phase lattice to be distorted, promoting the formation of defective structures.

[0021] 3. Cu, as the active center of CO2 hydrogenation reaction, is selectively doped into the spinel lattice and dispersed and isolated in the spinel lattice, which improves the dispersion of Cu species and inhibits the high-temperature sintering of the catalyst.

[0022] 4. Based on this, it was applied to the high-temperature reverse water-gas shift reaction and showed excellent catalytic activity. At 800°C, the CO2 conversion rate was close to 74%, the CO selectivity reached 100%, and the activity only decreased by 8% after 48 hours of reaction at 800°C. Compared with existing catalysts, it has the advantages of high activity, good selectivity and good stability. The preparation method is simple and the production cost is low, which is conducive to large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope photograph of the Cu-based spinel oxide catalyst obtained in Example 1 of the present invention.

[0024] Figure 2 It is the X-ray diffraction (XRD) diagram of the Cu-based spinel oxide catalyst obtained in Examples 1-3 of the present invention.

[0025] Figure 3 It is a performance comparison diagram of the Cu-based spinel oxide catalysts obtained in Examples 1-3 of the present invention and a stability diagram of the Cu-based spinel oxide catalyst obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0027] Example 1

[0028] A Cu-based spinel oxide catalyst method, the specific steps are as follows:

[0029] First, 100 ml of deionized water is used to prepare a mixed salt solution of copper nitrate, magnesium nitrate solution and ferric nitrate with a total metal ion concentration of 1 mol / L, and the Cu / Mg / Fe molar ratio is 0.5:3:2, which is recorded as the first solution. In addition, 100 ml of deionized water is added with 1.6 times the total molar amount of metal ions NaOH and 2 times the molar amount of trivalent metal ions Na2CO3 to prepare a mixed alkaline solution, which is recorded as the second solution; the first solution and the second solution are simultaneously poured into a colloid mill with a rotation speed of 4000 r / min and rapidly mixed and stirred for 3 minutes to obtain a suspension, which is placed in a closed high-pressure reactor and placed in an oven for hydrothermal crystallization at 120°C for 12 hours. After the reaction is completed, the precipitate is centrifuged to neutrality, dried at 80°C for 12 hours, and ground to obtain CuMgFe-LDH; CuMgFe-LDH is heated from room temperature to 900°C at 5°C / min in a muffle furnace and calcined for 4 hours to obtain a Cu-based spinel oxide catalyst.

[0030] The SEM image of the Cu-based spinel oxide catalyst obtained in this example is attached. Figure 1 .from Figure 1It can be seen that the catalyst nanoparticles are flake structures with a size of about 300 nm, and the particle size distribution is relatively uniform.

[0031] Example 2

[0032] A Cu-based spinel oxide catalyst method, the specific steps are as follows:

[0033] First, 100 ml of deionized water is used to prepare a mixed salt solution of copper nitrate, magnesium nitrate solution and ferric nitrate with a total metal ion concentration of 1 mol / L, and the Cu / Mg / Fe molar ratio is 1:3:2, which is recorded as the first solution. In addition, 100 ml of deionized water is added with 1.6 times the total molar amount of metal ions NaOH and 2 times the molar amount of trivalent metal ions Na2CO3 to prepare a mixed alkaline solution, which is recorded as the second solution; the first solution and the second solution are simultaneously poured into a colloid mill with a rotation speed of 4000 r / min and rapidly mixed and stirred for 3 minutes to obtain a suspension, which is placed in a closed high-pressure reactor and placed in an oven for hydrothermal crystallization at 120°C for 12 hours. After the reaction is completed, the precipitate is centrifuged to neutrality, dried at 80°C for 12 hours, and ground to obtain CuMgFe-LDH; CuMgFe-LDH is heated from room temperature to 900°C at 5°C / min in a muffle furnace and calcined for 4 hours to obtain a Cu-based spinel oxide catalyst.

[0034] Example 3

[0035] MgFe spinel oxide catalyst method, the specific steps are as follows:

[0036] First, 100 ml of deionized water is used to prepare a mixed salt solution of magnesium nitrate solution and ferric nitrate with a total metal ion concentration of 1 mol / L, and the Mg / Fe molar ratio is 2:1, which is recorded as the first solution. In addition, 100 ml of deionized water is added with 1.6 times the total molar amount of metal ions of NaOH and 2 times the molar amount of trivalent metal ions of Na2CO3 to prepare a mixed alkaline solution, which is recorded as the second solution; the first solution and the second solution are simultaneously poured into a colloid mill with a rotation speed of 4000 r / min, and quickly mixed and stirred for 3 minutes to obtain a suspension, which is placed in a closed high-pressure reactor and placed in an oven for hydrothermal crystallization at 120°C for 12 hours. After the reaction is completed, the precipitate is centrifuged to neutrality, dried at 80°C for 12 hours, and ground to obtain MgFe-LDH; MgFe-LDH is heated from room temperature to 900°C at 5°C / min in a muffle furnace and calcined for 4 hours to obtain a spinel oxide catalyst.

[0037] Figure 2 It is the X-ray diffraction (XRD) diagram of the catalyst obtained in Examples 1-3 of the present invention. As shown in the figure, the obtained catalyst has obvious spinel characteristic peaks and MgO characteristic peaks, and the Cu-based spinel oxide catalyst also has a weak CuO characteristic peak.

[0038] Application Examples

[0039] The catalyst obtained in Examples 1-3 was used in the reverse water gas shift reaction process according to the method of the present invention, as follows:

[0040] Weigh 20 mg of catalyst and 500 mg of quartz sand, mix them evenly and put them into a quartz tube. Then put the quartz tube into a continuous fixed bed reactor and introduce a mixed gas. Under normal pressure, the mixed gas is CO2 and H2 and the balance gas Ar. The volume ratio of H2 / CO2 / Ar is 3:1:1, and the mixed gas flow rate is 80 ml / min (GHSV = 240000 ml g -1 h -1 ), and its catalytic performance was investigated under the condition of T = 600-800 ° C. Shimadzu gas chromatography was used for online sampling and detection, CO2, CO and Ar were detected by TCD detector, and hydrocarbons were detected by FID detector.

[0041] Figure 3 The comparative performance diagram of the catalysts obtained in Examples 1-3 of the present invention and the stability diagram of the catalyst obtained in Example 1 are shown in the figure. As shown in the figure, the Cu-based spinel oxide catalyst has a better catalytic performance than the MgFe spinel oxide catalyst at 700-800°C, and the CO2 conversion rate is close to 74% at 800°C, which is close to the equilibrium conversion rate. When the Cu loading continues to increase, the catalytic performance decreases due to the increase in the CuO content in the catalyst, and the sintering resistance decreases; the catalyst obtained in Example 1 is subjected to a reverse water gas shift reaction at 800°C for 48h, and the CO2 conversion rate decreases by about 8%, which has good stability.

[0042] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a Cu-based spinel oxide catalyst, comprising: (1) Dissolving Cu(NO3)2·3H2O, Mg(NO3)2·6H2O, and Fe(NO3)3·9H2O in deionized water respectively to obtain a first solution; (2) dissolving NaOH and Na2CO3 in deionized water respectively to obtain a second solution; (3) rapidly mixing and stirring the first solution and the second solution in a colloid mill at room temperature to obtain a third product; (4) placing the third product in a closed reactor for hydrothermal crystallization, and washing, drying, and grinding to obtain a CuMgFe-LDH precursor; (5) The CuMgFe-LDH precursor is calcined in a muffle furnace to obtain a Cu-based spinel oxide catalyst.

2. The preparation method according to claim 1, wherein: Step (1) The metal ion concentration in the first solution is 0.5 to 1 mol / L; The volume of the deionized water is 50-100 ml.

3. The preparation method according to claim 1, wherein: In step (2), the NaOH concentration is 1.6 to 2 times the metal ion concentration of the first solution, and the Na2CO3 concentration is 1.6 to 2 times the trivalent metal ion concentration of the first solution; The volume of the deionized water is 50-100 ml.

4. The preparation method according to claim 1, wherein: The mixing and stirring in step (3) is carried out at a rotation speed of 4000 to 5000 r / min and a stirring time of 3 to 5 min.

5. The preparation method according to claim 1, wherein: The hydrothermal crystallization temperature of step (4) is 100-120° C., and the hydrothermal crystallization time is 10-12 hours.

6. The preparation method according to claim 1, wherein: The calcination conditions in step (5) are: heating from room temperature to 1000° C. at a heating rate of 5 to 10° C. / min and maintaining for 4 to 6 hours.

7. A Cu-based spinel oxide catalyst prepared according to the preparation method according to any one of claims 1 to 6.

8. Use of the Cu-based spinel oxide catalyst according to claim 7 in a reverse water gas shift reaction process.

9. The use according to claim 8, comprising: Weigh 20 mg of catalyst and 500 mg of quartz sand, mix them evenly and put them into a quartz tube. Then put the quartz tube into a continuous fixed bed reactor and introduce a mixed gas. Under normal pressure conditions, the mixed gas is CO2 and H2 and the balance gas Ar. The catalytic performance is examined at 600-800°C.

10. The use according to claim 9, wherein: The volume ratio of H2, CO2 and Ar is 3:1:1; The mixed gas flow rate is 80 ml / min.

Citation Information

Patent Citations

  • Preparation method and application of three-way catalyst used for reversed water gas shift reaction

    CN109621963A

  • Hydrotalcite-derived iron-containing spinel catalyst, preparation method and application thereof

    CN113908867A

  • Copper-iron alloy catalyst and preparation and application thereof

    CN116060009A

  • CO2 hydrogenation catalysts for the commercial production of syngas

    US20230150823A1

Cited By

  • Doped hydrotalcite derived composite metal oxide catalyst as well as preparation method and application thereof

    CN121467043A