Raney nickel catalyst for producing reduced indigo and production method of reduced indigo
Through the improved Renney nickel catalyst preparation method, the problems of high cost, large energy consumption and poor catalyst circulation performance in indigo reduction technology are solved, and a low-cost, efficient indigo reduction and safe production process are achieved.
Patent Information
- Application Number
- CN202410979533.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing indigo reduction technology has problems such as high cost, large energy consumption, poor environmental protection performance and poor catalyst circulation performance. Especially the cost of precious metal catalysts is high and the number of cycles is limited, and the high pressure required for Renney nickel catalysts poses safety risks.
Using an improved Renney nickel catalyst preparation method, by mixing nickel powder and molybdenum powder, ball milling in a ball mill and tempering, followed by activation with sodium hydroxide solution to form an alloy catalyst with good hydrogen adsorption capacity, and React with indigo powder, sodium hydroxide and potassium hydroxide in an autoclave, and is treated with nitrogen replacement and low-pressure hydrogen to reduce the reaction pressure.
It significantly reduces the cost of catalysts, improves the cycling performance and safety of catalysts, reduces energy consumption, extends the service life of the catalyst, and achieves efficient indigo reduction, reducing equipment requirements and production risks.
Smart Images

Figure CN118925746A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fine chemicals, and in particular to a Raney nickel catalyst for producing reduced indigo and a production method of reduced indigo. Background Art
[0002] At present, indigo is mainly sold in powder form in China, and the dye bath is prepared by chemical reduction method before printing and dyeing. Its disadvantages are coarse particles, wide particle size distribution range, large amount of dust generated during the production process, slow and uneven reduction rate during use, and it must be reduced with insurance powder (or other reducing agents) to make a dye bath, which is easy to cause uneven dyeing and affect the quality of printing and dyeing. A large amount of dye-containing wastewater is generated during the printing and dyeing process, and the treatment cost is high.
[0003] Since indigo is insoluble in water, it is usually dyed with reduced indigo leuco salt and then oxidized to make it color. The main technical routes for the reduction of indigo currently include: bacterial reduction, chemical reduction, catalytic hydrogenation reduction and electrochemical reduction.
[0004] Bacterial reduction method: Before the invention of chemical reduction method, indigo was usually reduced by fermentation process, which completely relied on the action of bacteria. Therefore, it required a long reduction time and harsh environmental conditions, and because it involved biological process, the consistency of reduction could not be guaranteed.
[0005] Chemical reduction method: Hydrosulfite is the most commonly used chemical reducing agent in the indigo industry, but it produces a lot of difficult-to-treat wastewater, so it has shortcomings in environmental protection. At the same time, some newly developed reducing agents are also used in the indigo reduction industry, such as α-hydroxyketone, thiourea, glucose, etc. Similarly, these reducing agents still have many unavoidable shortcomings, which limits the application of chemical reduction in green chemical industry.
[0006] Electrochemical reduction method: Indigo can be reduced directly or indirectly by dispersing it in a suitable solution. It can also be reduced by using the active hydrogen produced during the electrolysis of water. However, in order to achieve large-scale production of liquid reduction of indigo, the current density must be increased by increasing the electrode area and the current, which undoubtedly increases a lot of energy consumption and reduces economic efficiency.
[0007] Catalytic hydrogenation reduction method: Catalytic hydrogenation generally produces water as a product, and does not produce other by-products, which has good atom economy. In addition, the process conditions of indigo catalytic hydrogenation are mild, and the energy consumption is low, which has the prospect of development and application.
[0008] At present, the catalytic hydrogenation catalysts for pre-reducing liquid indigo can be divided into precious metal catalysts and Raney nickel catalysts. For precious metal catalysts, the patent: Method for preparing indigo by catalytic hydrogenation in a fluidized bed (CN 114644585A) points out that the precious metal-loaded catalyst can be cycled up to 50 times through a fluidized bed process, but the precious metal catalyst still has the problem of high cost, and in the cycle, the precious metal-loaded catalyst needs to be added to further increase the cost. It is estimated that according to its method, about 360g of catalyst is required per ton of 40% liquid indigo product, and the cost exceeds 3,000 yuan / ton of product.
[0009] CN 102516817 B discloses an environmentally friendly preparation method of indigo white solution, which uses Raney nickel for catalytic hydrogenation. A higher hydrogen pressure is required to achieve a better reaction effect. The pressure range is 1.5 MPa-5.5 MPa, which poses a safety hazard.
[0010] That is to say, although precious metal catalysts have higher cycle performance, their cost is still high. Although Raney nickel is relatively cheap, it requires a large pressure and has poor cycle performance. Therefore, we hope to prepare a Raney nickel catalyst with good reduction performance, high safety and good cycle performance through Raney nickel modification.
[0011] CN 103480394 A discloses a method for preparing a novel modified Raney nickel catalyst. The Raney nickel is prepared by an impregnation method. From the XRD diagram of the catalyst prepared by this method, it can be seen that the peak of molybdenum is not obvious, which may be because only a small amount of molybdenum is attached to the surface of the catalyst, so it cannot achieve a good catalytic effect.
[0012] CN 104056641 B discloses a preparation method and application of a slurry bed sulfur-resistant methanogenic Raney nickel catalyst. The specific steps of the invention are as follows: (1) pretreatment: uniformly mix nickel powder and molybdenum powder, soak them in a dilute acid solution for 5-60 minutes, then soak them in anhydrous ethanol for 5-30 minutes, then wash them with deionized water for 2-4 times, and dry them at 50-110°C for 1-8 hours for use; soak aluminum powder in an organic solvent for 5-30 minutes, then wash them with deionized water for 2-4 times, and dry them at 50-110°C for 1-8 hours for use; (2) preparation of nickel-molybdenum-aluminum alloy powder: uniformly mix nickel powder, molybdenum powder and aluminum powder, and Melt in a high-temperature furnace with a magnetic field, cool to room temperature under the protection of inert gas, grind the nickel-molybdenum-aluminum alloy powder into 80-200 mesh particles for use; (3) Preparation of Raney nickel catalyst: Place a stainless steel container containing NaOH solution in an ultrasonic constant temperature water bath, adjust the temperature of the constant temperature water bath and the ultrasonic intensity, add the prepared nickel-molybdenum-aluminum alloy powder to the above NaOH solution while stirring, and then stir at a constant temperature of 0-70°C for 3-12h. After the reaction is completed, remove the upper alkali solution, rinse repeatedly with deionized water until neutral, and then rinse with anhydrous ethanol 2-4 times to obtain the Raney nickel catalyst. The Raney nickel prepared by this method is used for slurry bed methanation reaction and can show good sulfur resistance. The sulfur content of the synthesis gas is between 300-6000ppm, and it has good catalytic activity and selectivity. Summary of the invention
[0013] In order to solve the above technical problems, the first purpose of the present invention is to provide a Raney nickel catalyst for producing reduced indigo. The second purpose is to provide a production method of reduced indigo, the preparation process of the Raney nickel catalyst is simple, the energy consumption is low, and the prepared Raney nickel can enhance the adsorption behavior of hydrogen, thereby enhancing the catalytic effect and having good cycle performance.
[0014] To achieve the above first object, the present invention provides the following technical solution: A Raney nickel catalyst for producing reduced indigo, characterized in that it is prepared according to the following steps:
[0015] (1) nickel powder and molybdenum powder were mixed evenly, soaked in dilute acid for 10-15 min, then washed with deionized water until neutral, and dried in a vacuum dryer to constant weight;
[0016] (2) mixing aluminum powder with dried molybdenum powder and nickel powder, and milling the mixture in a planetary ball mill at a speed of 500-1000 rpm for 30-40 min;
[0017] (3) placing the ball-milled mixed powder in a muffle furnace and setting the temperature to 250-300° C. for tempering to further stabilize the crystal phase;
[0018] (4) The alloy powder after tempering treatment is refluxed with sodium hydroxide solution for activation, the upper alkali solution is removed and the powder is washed with clean water until it is neutral to obtain an activated Raney nickel catalyst.
[0019] In the above scheme: in the Raney nickel catalyst, the mass percentage of molybdenum is 3-6%, the mass percentage of nickel is 50%, and the rest is aluminum.
[0020] In the above scheme: after ball milling, the powder particle size is 0.1-1 μm.
[0021] In the above scheme: the dilute acid is one of dilute hydrochloric acid, dilute sulfuric acid and dilute nitric acid.
[0022] In the above scheme: in step (4), the mass concentration of the sodium hydroxide solution is 20-25%, and the reflux time is 45-60 min.
[0023] During ball milling, the metal powder is severely deformed by the collision of the steel balls in the ball mill and cold welded to form a lamellar structure alloy. As the ball milling collision continues, the lamellar structure becomes more and more refined. Due to the presence of a large number of crystal defects introduced by deformation and a large number of interfaces introduced by cold welding, as well as the temperature rise caused by the ball milling collision, the diffusion capacity of the components is greatly enhanced. The generation of crystal defects can enhance the adsorption behavior of hydrogen, thereby enhancing the catalytic effect.
[0024] It can be seen from XRD that the catalysts prepared by the impregnation method and the method of the present invention both have obvious nickel metal peaks, but only the catalyst of the alloy method of the present invention has an obvious molybdenum metal peak, which indicates that molybdenum exists in the catalyst in the form of a solid solution; while the peak of molybdenum in the impregnation method catalyst is not obvious, indicating that only a small amount of molybdenum is attached to the catalyst surface by impregnation. The Raney nickel prepared by the present invention has a different structure from the Raney nickel prepared by the impregnation method.
[0025] The second object of the present invention is achieved by: a method for producing reduced indigo, characterized in that it is produced according to the following method:
[0026] (1) weighing indigo powder, sodium hydroxide, potassium hydroxide, and a dispersant, and adding them into water or a pre-reduced indigo solution to prepare a dispersion, adding the dispersion into a high-pressure reactor, and adding the prepared Raney nickel catalyst and a defoaming agent;
[0027] (2) After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced until the air in the autoclave is completely replaced;
[0028] (3) introducing hydrogen into the autoclave to a pressure of 0.2-0.8 MPa, stirring, heating, and after the reaction is complete, separating the material through a magnetic separator to recover the catalyst, and pressing the pre-reduced indigo into a container for storage;
[0029] (4) The magnetically separated catalyst is washed with water, then washed with N,N-dimethylformamide, and then put into step 1 for recycling.
[0030] The dispersant can be a nonionic surfactant or an amphoteric surfactant, and the added amount is generally 1-5% of the mass of the indigo powder.
[0031] In the above scheme: the amount of sodium hydroxide added is 15-28% of the mass of indigo; the amount of potassium hydroxide added is 3-10% of the mass of indigo; the amount of water added is 150-350% of the mass of indigo; the amount of Raney nickel catalyst added is 3-10% of the mass of indigo; the defoaming agent is one or more of silicone, polyether, and polyether-modified polysiloxane defoaming agents, and the added amount is 0.1-0.5% of the mass of indigo.
[0032] In the above scheme: in step (3), the stirring speed should be 500-1500 rpm, the reaction temperature should be 80-90°C, and the reaction time should be 2-5 hours.
[0033] In the above scheme: in step (4), new Raney nickel catalyst with a mass percentage of 0.2-1% of indigo is added after every two cycles.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The reaction pressure can be reduced to as low as 0.2-0.8 MPa, greatly reducing the requirements for equipment and production risks.
[0036] (2) The present invention can dissolve and elute the indigo attached to the catalyst pores by N,N-dimethylformamide, greatly extending the service life of the catalyst. In the experiment, more than 20 cycles can be performed, thereby reducing the catalyst cost per ton of product to less than 20% of that of the noble metal-supported catalyst.
[0037] (3) In the Raney nickel catalyst of the present invention, the metallic molybdenum in the alloy will not be etched by sodium hydroxide like aluminum, but will enter the nickel lattice. The addition of molybdenum changes the catalytic lattice structure, increases the number of active sites of the Raney nickel and the hydrogen adsorption capacity.
[0038] (4) Under pure sodium hydroxide conditions, vigorous stirring will produce a large amount of foam, which will affect the contact between the catalyst and the indigo dispersion, thereby hindering the further progress of the reaction; the generation of foam during the reaction can be avoided by adding potassium hydroxide and hydroxy silicone oil defoaming agent.
[0039] By partially replacing sodium hydroxide with potassium hydroxide, the crystallization of indigo salt can be avoided at low temperatures. When the addition amount is less than 3%, the product will become solid after being placed in a 0-degree environment for 24 hours; this phenomenon will not occur when the addition amount of potassium hydroxide is higher than 3%. In addition, in order to control costs, the addition amount of potassium hydroxide should not be too high. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The XRD diagram of Raney nickel prepared by Example 1 of the present invention and the impregnation method. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0042] Example 1
[0043] Preparation of Raney nickel catalyst:
[0044] (1) Mix nickel powder and molybdenum powder evenly, soak them in dilute hydrochloric acid for 10-15 minutes, then wash them with deionized water until they are neutral, and dry them in a vacuum dryer to constant weight. The mass percentage of molybdenum is 3%, the mass percentage of nickel is 50%, and the rest is aluminum.
[0045] (2) Mix aluminum powder with dried molybdenum powder and nickel powder, and put them into a planetary ball mill for grinding at a speed of 500-1000 rpm for 30-40 minutes. After ball milling, the powder particle size is 0.1-1 μm.
[0046] (3) The ball-milled mixed powder is placed in a muffle furnace, the temperature is set to 250° C., and tempered for 20-40 min to further stabilize the crystal phase.
[0047] (4) The alloy powder after tempering treatment is activated by refluxing a sodium hydroxide solution with a mass concentration of 21% for 45-60 minutes, removing the upper alkali solution and washing with clean water until neutral, thereby obtaining an activated Raney nickel catalyst.
[0048] Example 2
[0049] 200 g of indigo powder, 56 g of sodium hydroxide, 6 g of potassium hydroxide, and 4 g of dispersant NNO were weighed, put into 400 g of water, mixed into a liquid, and then added into a 2 L high pressure reactor, and 0.2 g of silicone defoamer and 9 g of Raney nickel catalyst of Example 1 were added.
[0050] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 2.5 hours, and the pressure is reduced to 0.1MPa.
[0051] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained, and the catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0052] The obtained pre-reduced indigo was a reddish brown liquid with a concentration of 29.5% and a reduction rate of 97.7%.
[0053] Example 3
[0054] 200 g of indigo powder, 30 g of sodium hydroxide, 20 g of potassium hydroxide, and 2 g of dispersant NNO were weighed, put into 400 g of water, mixed into a liquid, and then added into a 2L high-pressure reactor, and 1 g of defoamer and 6 g of the Raney nickel catalyst of Example 1 were added.
[0055] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.2MPa hydrogen, close the air inlet valve, adjust the stirring speed to 500rpm, and then raise the temperature to 85°C. When the temperature in the autoclave reaches 85°C, add the hydrogen pressure to 0.3MPa and keep the valve open for continuous ventilation. Record the reaction time, speed, temperature and changes. After 3-4 hours of reaction, stop the reaction.
[0056] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained, and the catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0057] The obtained pre-reduced indigo was a clear reddish brown liquid with a concentration of 29.4% and a reduction rate of 97.3%.
[0058] Example 4
[0059] In order to obtain a higher concentration of pre-reduced liquid indigo and further reduce transportation costs, the secondary feeding method can be used to increase the product concentration. First, take 200g of indigo powder, 56g of sodium hydroxide, 6g of potassium hydroxide, and 4g of dispersant NNO, put them into 400g of water and mix them into a liquid, then add 2L of high-pressure reactor, add 0.2g of defoamer and 9g of Raney nickel catalyst of Example 1. After the high-pressure reactor is completely sealed, the air in the reactor is evacuated with a vacuum pump, and nitrogen is introduced. This cycle is repeated 3 times until the air in the reactor is completely replaced. After 0.8MPa of hydrogen is introduced, the air inlet valve is closed, and the temperature is raised to 85°C after the stirring speed is adjusted to 900rpm. When the temperature in the kettle reaches 85°C, the reaction time, speed, temperature and pressure changes are recorded. After the pressure no longer changes, the reaction is stopped.
[0060] Open the reactor and add 160g indigo powder, 35g sodium hydroxide, 5g potassium hydroxide, and 3g dispersant NNO again. After the high-pressure reactor is completely sealed, the air in the reactor is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated 3 times until the air in the reactor is completely replaced. After 0.8MPa hydrogen is introduced, the air inlet valve is closed, the stirring speed is adjusted to 900rpm, and the temperature is raised to 85°C. When the temperature in the reactor reaches 85°C, the reaction time, speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped.
[0061] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained, and the catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0062] The obtained pre-reduced indigo was a clear reddish brown liquid with a concentration of 40.5% and a reduction rate of 98.3%.
[0063] Example 5 is a repeated application test of Example 2. Table 1 lists the relationship between the number of cycles and the catalyst cost per ton of product. As the number of cycles increases, the average catalyst consumption per time decreases monotonically. After every two cycles, 0.2-1% of the mass of indigo is added to the new Raney nickel catalyst.
[0064] The average catalyst cost per ton of product was calculated based on the average catalyst consumption per ton of product and the unit price of Raney nickel catalyst of 200 to 250 yuan per kilogram.
[0065]
[0066]
[0067] Example 6
[0068] 200 g of indigo powder, 50 g of sodium hydroxide, 10 g of potassium hydroxide, and 10 g of dispersant NNO were weighed, put into 700 g of water, mixed into a liquid, and then added into a 2 L high pressure reactor, and 0.6 g of silicone defoamer and 20 g of the Raney nickel catalyst of Example 1 were added.
[0069] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.5 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 1500 rpm, and the temperature is raised to 90°C. When the temperature in the autoclave reaches 90°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped, and the reaction time recorded is 2 hours.
[0070] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained. The catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0071] The pre-reduced indigo is a reddish brown liquid with a concentration of 20.6% and a reduction rate of 97.4%.
[0072] Example 7
[0073] 200 g of indigo powder, 40 g of sodium hydroxide, 20 g of potassium hydroxide, and 5 g of dispersant NNO were weighed, added into 350 g of water, mixed into a liquid, and then added into a 2 L high pressure reactor, and 0.6 g of silicone defoamer and 9 g of Raney nickel catalyst of Example 1 were added.
[0074] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 80°C. When the temperature in the autoclave reaches 80°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The reaction time is recorded as 5 hours.
[0075] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained. The catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0076] The pre-reduced indigo is a reddish brown liquid with a concentration of 32.5% and a reduction rate of 98.1%.
[0077] Example 8
[0078] Preparation of Raney nickel catalyst:
[0079] (1) Nickel powder and molybdenum powder are mixed evenly, soaked in dilute sulfuric acid for 10-15 minutes, then washed with deionized water until neutral, and dried in a vacuum dryer to constant weight. The mass percentage of molybdenum is 6%, the mass percentage of nickel is 50%, and the rest is aluminum.
[0080] (2) Mix aluminum powder with dried molybdenum powder and nickel powder, and put them into a planetary ball mill for grinding at a speed of 500-1000 rpm for 30-40 minutes. After ball milling, the powder particle size is 0.1-1 μm.
[0081] (3) The ball-milled mixed powder is placed in a muffle furnace, the temperature is set to 300° C., and tempered for 20-40 minutes to further stabilize the crystal phase.
[0082] (4) The alloy powder after tempering treatment is activated by refluxing a sodium hydroxide solution with a mass concentration of 21% for 45-60 minutes, removing the upper alkali solution and washing with clean water until neutral, thereby obtaining an activated Raney nickel catalyst.
[0083] Weigh 200 g of indigo powder, 56 g of sodium hydroxide, 6 g of potassium hydroxide, and 4 g of dispersant NNO, put them into 400 g of water and mix them into a liquid, then add them into a 2L high-pressure reactor, add 0.2 g of silicone defoamer and 9 g of the Raney nickel catalyst of this example.
[0084] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped, and the reaction time recorded is 2 hours.
[0085] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained. The catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0086] The obtained pre-reduced indigo was a reddish brown liquid with a concentration of 30.0% and a reduction rate of 98.2%.
[0087] Comparative Example 1
[0088] 200 g of indigo powder, 62 g of sodium hydroxide, and 4 g of dispersant NNO were weighed, added to 400 g of water, mixed into a liquid, added to a 2 L high pressure reactor, and 9 g of the Raney nickel catalyst of Example 1 was added.
[0089] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 7 hours.
[0090] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo sodium salt product is obtained.
[0091] In the experiment of Comparative Example 1, after the reaction was completed, a large amount of foam was observed when the autoclave was opened, and the product was a slightly viscous liquid with a reduction rate of 90.2. Further, after the products of Comparative Example 1 and Example 2 were placed in a refrigerator at -10°C for 24 hours, the product of Comparative Example 1 became solid and lost fluidity, while the product of Example 1 remained in a liquid state with good fluidity.
[0092] Comparative Example 2
[0093] 200 g of indigo powder, 56 g of sodium hydroxide, 6 g of potassium hydroxide, and 4 g of dispersant NNO were weighed, added to 400 g of water, mixed into a liquid, added to a 2 L high pressure reactor, and 9 g of the Raney nickel catalyst of Example 1 was added.
[0094] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 6 hours.
[0095] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo sodium potassium salt product is obtained.
[0096] In the experiment of Comparative Example 2, after the reaction was completed, a small amount of foam was observed floating on the surface of the product and adhering to the stirring rod when the autoclave was opened. After being placed in a refrigerator at -10°C for 24 hours, the product still remained in a liquid state with good fluidity.
[0097] The obtained pre-reduced indigo was a reddish brown liquid with a concentration of 30.0% and a reduction rate of 96.5%.
[0098] Comparative Example 3
[0099] 200 g of indigo powder, 62 g of sodium hydroxide, 0.2 g of defoamer, and 4 g of dispersant NNO were weighed, added to 400 g of water, mixed into a liquid, added to a 2 L high pressure reactor, and 9 g of the Raney nickel catalyst of Example 1 was added.
[0100] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 6.5 hours.
[0101] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo sodium salt product is obtained.
[0102] In the experiment of Comparative Example 3, after the reaction was completed, the autoclave was opened and foam was observed to be attached to the stirring rod. The obtained pre-reduced indigo was a reddish brown liquid with a concentration of 30.0% and a reduction rate of 96.8%. Furthermore, after being placed in a refrigerator at -10°C for 24 hours, the product became solid and lost fluidity.
[0103] Comparative Example 4
[0104] 200 g of indigo powder, 56 g of sodium hydroxide, 4 g of potassium hydroxide, and 2 g of dispersant NNO were weighed, put into 400 g of water, mixed into a liquid, and then added into a 2 L high pressure reactor, and 1 g of defoamer and 6 g of the Raney nickel catalyst of Example 1 were added.
[0105] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.2MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 500rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the hydrogen pressure is supplemented to 0.3MPa, and the valve is kept open for continuous ventilation. Record the reaction time, speed, temperature and changes. After 5 hours of reaction, stop the reaction.
[0106] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product and a catalyst are obtained, and the catalyst is washed with water and N,N-dimethylformamide respectively and then recovered.
[0107] The obtained pre-reduced indigo was a clear reddish brown liquid with a concentration of 30.2% and a reduction rate of 96.9%. Furthermore, after being placed in a refrigerator at -10°C for 24 hours, the product became solid and lost fluidity.
[0108] Comparative Example 5
[0109] 200 g of indigo powder, 56 g of sodium hydroxide, 6 g of potassium hydroxide, and 4 g of dispersant NNO were weighed, added to 400 g of water, mixed into a liquid, and then added to a 2 L high pressure reactor, 0.2 g of silicone defoamer and 9 g of Raney nickel catalyst prepared by the impregnation method disclosed in CN 103480394A were added.
[0110] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 7 hours, and the pressure is reduced to 0.5MPa.
[0111] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo sodium salt product is obtained.
[0112] In the comparative example experiment, after the reaction was completed, the autoclave was opened and the product was found to be relatively viscous. Further, the product of comparative example 5 was tested and its reduction rate was 60.8%.
[0113] Comparative Example 6
[0114] 200 g of indigo powder, 56 g of sodium hydroxide, 6 g of potassium hydroxide, and 4 g of dispersant NNO were weighed, added to 400 g of water, mixed into a liquid, and then added to a 2 L high pressure reactor, 0.2 g of silicone defoamer and 9 g of the Raney nickel catalyst prepared in Example 1 of CN 104056641B were added.
[0115] After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced. This cycle is repeated three times until the air in the autoclave is completely replaced. After introducing 0.8 MPa hydrogen, the air inlet valve is closed, the stirring speed is adjusted to 900 rpm, and the temperature is raised to 85°C. When the temperature in the autoclave reaches 85°C, the reaction time, rotation speed, temperature and pressure changes are recorded. When the pressure no longer changes, the reaction is stopped. The recorded reaction time is 5 hours.
[0116] After the materials in the kettle are pressed into a magnetic separator, a pre-reduced liquid indigo product is obtained.
[0117] In the comparative example experiment, after the reaction was completed, the autoclave was opened and the product was found to be relatively viscous. Further, the product of comparative example 6 was tested and its reduction rate was 81.2%.
[0118] The present invention is not limited to the embodiments. For example, the concentration of sodium hydroxide used for activation can be appropriately adjusted to 20%-25%.
Claims
1. A Raney nickel catalyst for producing reduced indigo, It is characterized in that Prepare according to the following steps: (1) nickel powder and molybdenum powder were mixed evenly, soaked in dilute acid for 10-15 min, then washed with deionized water until neutral, and vacuum dried to constant weight; (2) mixing aluminum powder with dried molybdenum powder and nickel powder, and milling the mixture in a planetary ball mill at a speed of 500-1000 rpm for 30-40 min; (3) placing the ball-milled mixed powder in a muffle furnace and setting the temperature to 250-300° C. for tempering to further stabilize the crystal phase; (4) The alloy powder after tempering treatment is refluxed with sodium hydroxide solution for activation, the upper alkali solution is removed and the powder is washed with clean water until it is neutral to obtain an activated Raney nickel catalyst.
2. The Raney nickel catalyst for producing reduced indigo according to claim 1, Features: In the Raney nickel catalyst, the mass percentage of molybdenum is 3-6%, the mass percentage of nickel is 50%, and the rest is aluminum.
3. The Raney nickel catalyst for producing reduced indigo according to claim 1 or 2, Features: After ball milling, the powder particle size is 0.1-1 μm.
4. The Raney nickel catalyst for producing reduced indigo according to claim 3, Features: The dilute acid is one of dilute hydrochloric acid, dilute sulfuric acid, and dilute nitric acid.
5. The Raney nickel catalyst for producing reduced indigo according to claim 5, Features: In step (4), the reflux time is 45-60 min.
6. A method for producing reduced indigo, It is characterized in that Produced as follows: (1) weighing indigo powder, sodium hydroxide, potassium hydroxide, and a dispersant, and adding them into water or a pre-reduced indigo solution to prepare a dispersion, adding the dispersion into a high-pressure reactor, and adding the Raney nickel catalyst prepared according to any one of claims 1 to 5 and a defoaming agent; (2) After the autoclave is completely sealed, the air in the autoclave is evacuated with a vacuum pump and nitrogen is introduced until the air in the autoclave is completely replaced; (3) introducing hydrogen into the autoclave to a pressure of 0.2-0.8 MPa, stirring, heating, and after the reaction is complete, separating the material through a magnetic separator to recover the catalyst, and pressing the pre-reduced indigo into a container for storage; (4) The magnetically separated catalyst is washed with water, then washed with N,N-dimethylformamide, and then put into step 1 for recycling.
7. The method for producing reduced indigo according to claim 6, Features: The amount of sodium hydroxide added is 15-28% of the mass of indigo; the amount of potassium hydroxide added is 3-10% of the mass of indigo; the amount of water added is 150-350% of the mass of indigo; the amount of Raney nickel catalyst added is 3-10% of the mass of indigo; the defoamer is one or more of silicone, polyether, and polyether-modified polysiloxane defoamers, and the amount added is 0.1-0.5% of the mass of indigo.
8. The method for producing reduced indigo according to claim 7, Features: In step (3), the stirring speed should be 500-1500 rpm, the reaction temperature should be 80-95°C, and the reaction time should be 2-5 hours.
9. The method for producing reduced indigo according to claim 8, Features: In step (4), after every two cycles, new Raney nickel catalyst with a mass percentage of 0.2-1% of indigo is added.
Citation Information
Patent Citations
Method for producing raney nickel catalyst
CN101402046A
Method for preparing indigo white solution
CN102516817A
Novel modified Raney nickel catalyst, its preparation method and application
CN103480394A
Preparation method and application of slurry reactor sulfur-resistant methanation Raney nickel catalyst
CN104056641A
Catalyst used for synthesis of hexanediamine
CN106807395A