In-situ preparation method of Bi4Ti3O12-BiPO4 composite photocatalyst

By growing BiPO4 in situ on the surface of Bi4Ti3O12, a tight Z-Scheme heterojunction interface is formed, which solves the problems of low efficiency and poor stability of traditional photocatalysts in NOx treatment, and achieves efficient NOx removal and by-product inhibition.

CN118925759APending Publication Date: 2024-11-12SHANDONG ALUMINUM WORKS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031341.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional photocatalysts have limited their application in NOx governance due to their narrow light absorption range, low separation efficiency and poor stability of photogenerated electron-hole pairs, especially in building efficient heterojunction interfaces.

Method used

By designing and optimizing the in-situ preparation method of Bi4Ti3O12-BiPO4 composite photocatalyst, the epitaxial growth of BiPO4 on the surface of Bi4Ti3O12 is realized, and a tight Z-Scheme heterojunction interface is formed, thereby improving the separation and transfer efficiency of photogenerated carriers.

Benefits of technology

The NOx removal efficiency of the photocatalyst is significantly improved, and the NO to NO3- is deeply oxidized, while the production of toxic byproducts NO2 is inhibited, the photocatalytic performance is enhanced and the generation of byproducts is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925759A_ABST
    Figure CN118925759A_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ preparation method of a Bi4Ti3O12-BiPO4 (Bi4Ti3O12-BiPO4) composite photocatalyst. Relates to the technical field of photocatalyst preparation. The preparation method comprises the following steps: (1) preparing Bi4Ti3O12; (2) preparing a sodium dihydrogen phosphate solution; (3) preparing Bi4Ti3O12-BiPO4: mixing the Bi4Ti3O12 prepared in the step (1) with deionized water, performing ultrasonic treatment for 30 minutes, mixing with the sodium dihydrogen phosphate solution prepared in the step (2), stirring for 30 minutes, and performing hydro-thermal treatment, washing and drying to obtain Bi4Ti3O12-BiPO4. The invention provides a preparation method for in-situ compounding Bi4Ti3O12 and BiPO4, a Z-Scheme Bi4Ti3O12-BiPO4 heterojunction with a close contact interface is generated, and the Bi4Ti3O12-BiPO4 heterojunction can be used for preparing Bi4Ti3O12-BiPO4. The photocatalyst has the effect of promoting photo-generated charge separation and transfer, so that the photocatalytic efficiency is greatly improved, the preparation process is simple, the property is stable, and the catalyst can be applied to the fields of photocatalytic oxidation of NO and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalyst preparation, and specifically to a Bi4Ti3O 12 -In situ preparation method of BiPO4 composite photocatalyst. Background Art

[0002] In recent years, with the rapid development of social economy, environmental pollution and energy shortage have become two major problems that plague mankind. Among them, air pollution is an important part of environmental pollution. Nitrogen oxides (NO x ) Pollution not only destroys the natural environment that is closely related to human life, but also poses a huge threat to human health. Therefore, it is urgent to develop a green and environmentally friendly NO x Treatment solution: Photocatalysis uses inexhaustible solar energy to oxidize NO at room temperature x It can not only manage the environment without causing secondary pollution, but also save energy. It is an important and promising technology.

[0003] However, the application of traditional photocatalysts in the field of photocatalysis is limited by the narrow light absorption range, low separation efficiency of photogenerated electron-hole pairs, and poor stability. In order to overcome these defects, researchers have developed a series of modification measures for traditional photocatalysts, including morphology regulation, doping, surface modification and loading, construction of heterojunctions, etc. Among them, the construction of heterojunctions can not only realize the flexible regulation of the band structure of composite materials, but also effectively improve the separation and transfer efficiency of photogenerated carriers, and is considered to be an efficient photocatalyst improvement strategy. Among them, the Z-Scheme heterojunction has become the most favored heterostructure by researchers because it promotes the transfer of photogenerated electrons and holes while retaining the high redox potential of the two semiconductor materials. At the same time, the interface quality is also extremely important for the enhancement of photocatalytic activity. The close interface contact between two or more materials is one of the important factors to improve the separation efficiency of photogenerated carriers. Epitaxial growth is considered to be an effective strategy to construct a close contact heterojunction interface. Summary of the invention

[0004] The object of the present invention is to provide a Bi4Ti3O 12 -BiPO4 composite photocatalyst in situ preparation method, in order to solve the above problems raised in the background technology. Therefore, the present invention aims to provide a Bi4Ti3O 12 -BiPO4 composite photocatalyst in situ preparation method, by Bi4Ti3O 12 -BiPO4 catalyst synthesis conditions were designed and optimized, and finally a BiPO4 epitaxially grown on Bi4Ti3O 12Z-Scheme heterojunction catalysts on the surface of the nanostructured carbon nanotubes and applied them to room temperature photocatalytic oxidation of NO x .

[0005] In order to solve the above technical problems, the present invention provides the following technical means: a Bi4Ti3O 12 -The in-situ preparation method of BiPO4 composite photocatalyst comprises the following steps:

[0006] (1) Preparation of Bi4Ti3O 12 : Dissolve bismuth nitrate pentahydrate, tetrabutyl titanate and sodium hydroxide in deionized water, stir for 15 to 30 minutes, ultrasonicate for 15 to 30 minutes, stir for 30 to 60 minutes, then perform hydrothermal treatment, wash and dry to obtain Bi4Ti3O 12 ;

[0007] (2) preparing sodium dihydrogen phosphate solution;

[0008] (3) Preparation of Bi4Ti3O 12 -BiPO4: Bi4Ti3O prepared in step (1) 12 After being mixed with deionized water, the mixture is ultrasonicated for 30 to 60 minutes, and then mixed with the sodium dihydrogen phosphate solution prepared in step (2) and stirred for 30 to 60 minutes, and then subjected to hydrothermal treatment, and then washed and dried to obtain Bi4Ti3O 12 -BiPO4.

[0009] In the above steps:

[0010] The sodium dihydrogen phosphate in step (2) can be replaced by trisodium phosphate, disodium hydrogen phosphate or phosphoric acid. Different phosphoric acids or phosphate solutions have different effects on Bi4Ti3O during the hydrothermal treatment in step (3). 12 Different etching degrees result in different amounts of BiPO4 generated.

[0011] The concentration range of the sodium dihydrogen phosphate solution in step (2) is 0.25-1.0 mol / L. The change in the concentration of the sodium dihydrogen phosphate solution will lead to the 12 The difference in the amount of BiPO4 generated on the surface.

[0012] Step (3) Bi4Ti3O 12 The usage is 0.5-1.25 g, Bi4Ti3O 12 Effect of the usage amount on Bi4Ti3O 12 -BiPO4 composites had no significant effect on the formation of BiPO4.

[0013] The reaction time of the hydrothermal treatment in step (3) is 12-24 hours. The change of the hydrothermal treatment reaction time has an effect on the 12-BiPO4 composites had no significant effect on the formation of BiPO4.

[0014] Beneficial effects of the present invention:

[0015] By etching with sodium dihydrogen phosphate, Bi4Ti3O 12 BiPO4 was in situ grown on the surface. Due to this special in situ preparation method, a closely contacted heterojunction interface was formed between the two semiconductors, which was beneficial to the transmission and transfer of photogenerated carriers between the two semiconductors. The prepared catalyst showed good photocatalytic performance.

[0016] Bi4Ti3O 12 It forms a close contact Z-Scheme heterojunction with BiPO4, which can efficiently separate photogenerated electrons and holes, and has a high redox ability, which is conducive to the deep oxidation of NO to NO3 - , greatly enhancing the ability of photocatalytic removal of NO while inhibiting the production of toxic byproduct NO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solution of the present invention, the following is a brief introduction to the drawings required for use in the implementation mode. It is obvious that the drawings described below are only some implementation modes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The Bi4Ti3O obtained in Example 1 12 -Photocatalytic NO oxidation performance of BiPO4 catalyst.

[0019] Figure 2 The Bi4Ti3O obtained in Example 1 12 - NO2 byproduct accumulation plot for BiPO4 catalyst.

[0020] Figure 3 The Bi4Ti3O obtained in Example 1 12 Scanning electron microscopy image of the catalyst.

[0021] Figure 4 The Bi4Ti3O obtained in Example 1 12 -Scanning electron microscopy image of BiPO4 catalyst. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below by specific implementation methods. Those skilled in the art should understand that the embodiments are only part of the embodiments of the present invention, and the present invention also includes any combination of the specific embodiments.

[0023] An embodiment of the present invention provides a Bi4Ti3O 12 -The in-situ preparation method of BiPO4 composite photocatalyst comprises the following steps:

[0024] (1) Preparation of Bi4Ti3O 12 : Dissolve bismuth nitrate pentahydrate, tetrabutyl titanate and sodium hydroxide in deionized water, stir for 15 minutes, ultrasonicate for 15 minutes, stir for 30 minutes, then perform hydrothermal treatment, wash and dry to obtain Bi4Ti3O 12 ;

[0025] (2) preparing sodium dihydrogen phosphate solution;

[0026] (3) Preparation of Bi4Ti3O 12 -BiPO4: Bi4Ti3O prepared in step (1) 12 After being mixed with deionized water, the mixture was ultrasonicated for 30 minutes, and then mixed with the sodium dihydrogen phosphate solution prepared in step (2) and stirred for 30 minutes, and then subjected to hydrothermal treatment. After washing and drying, Bi4Ti3O 12 -BiPO4.

[0027] The sodium dihydrogen phosphate in step (2) can be replaced by trisodium phosphate, disodium hydrogen phosphate or phosphoric acid, preferably sodium dihydrogen phosphate.

[0028] The concentration range of the sodium dihydrogen phosphate solution in step (2) is 0.25-1.0 mol / L, preferably 0.5 mol / L.

[0029] Step (3) Bi4Ti3O 12 The usage amount is 0.5-1.25 grams, preferably 1.0 grams.

[0030] The reaction time of the hydrothermal treatment in step (3) is 12-24 hours, preferably 20 hours.

[0031] The following non-limiting examples may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way:

[0032] Example 1

[0033] (1) Preparation of Bi4Ti3O 12 : 1.6 g of bismuth nitrate pentahydrate, 0.84 g of tetrabutyl titanate, and 6 g of sodium hydroxide were dissolved in 30 ml of deionized water, stirred for 15 minutes, ultrasonicated for 15 minutes, stirred for 30 minutes, and then hydrothermally treated at 180 degrees Celsius for 20 hours in a 50 ml hydrothermal kettle, washed with deionized water and anhydrous ethanol, and dried at 60 degrees Celsius to obtain Bi4Ti3O 12 ;

[0034] (2) preparing a sodium dihydrogen phosphate solution with a concentration of 0.5 mol / L;

[0035] (3) Preparation of Bi4Ti3O 12 -BiPO4: Bi4Ti3O prepared in step (1) 12 1.0 g was mixed with 30 ml of deionized water and ultrasonicated for 30 minutes, then mixed with 10 ml of sodium dihydrogen phosphate solution prepared in step (2) and stirred for 30 minutes, and then hydrothermally treated at 180 degrees Celsius for 24 hours in a 50 ml hydrothermal kettle, washed with deionized water and anhydrous ethanol respectively, and dried at 60 degrees Celsius to obtain Bi4Ti3O 12 -BiPO4.

[0036] The catalytic performance of the catalyst obtained in this example is as follows Figure 1 and Figure 2 shown.

[0037] Example 2

[0038] In this embodiment, the concentration of the sodium dihydrogen phosphate solution in Example 1 is replaced from 0.5 mol / L to 0.25 mol / L, and the other conditions are exactly the same as those in Example 1.

[0039] The catalytic performance of the catalyst obtained in this example is as follows Figure 1 and Figure 2 shown.

[0040] Example 3

[0041] In this embodiment, the concentration of the sodium dihydrogen phosphate solution in Example 1 is replaced from 0.5 mol / L to 0.75 mol / L, and the other conditions are exactly the same as those in Example 1.

[0042] The catalytic performance of the catalyst obtained in this example is as follows Figure 1 and Figure 2 shown.

[0043] Example 4

[0044] In this embodiment, the concentration of the sodium dihydrogen phosphate solution in Example 1 is replaced from 0.5 mol / L to 1.0 mol / L, and the other conditions are exactly the same as those in Example 1.

[0045] The catalytic performance of the catalyst obtained in this example is as follows Figure 1 and Figure 2 shown.

[0046] Example 5

[0047] In this embodiment, the sodium dihydrogen phosphate in Example 1 is replaced by trisodium phosphate, and other conditions are exactly the same as those in Example 1.

[0048] Example 6

[0049] In this embodiment, the sodium dihydrogen phosphate in Example 1 is replaced by disodium hydrogen phosphate, and other conditions are exactly the same as those in Example 1.

[0050] Example 7

[0051] In this embodiment, the sodium dihydrogen phosphate in Example 1 is replaced by phosphoric acid, and other conditions are exactly the same as those in Example 1.

[0052] Example 8

[0053] In this example, the Bi4Ti3O 12 The usage amount was replaced by 0.5 g from 1.0 g, and the other conditions were exactly the same as those in Example 1.

[0054] Example 9

[0055] In this example, the Bi4Ti3O 12 The usage amount was replaced by 1.0 g to 1.5 g, and the other conditions were exactly the same as those in Example 1.

[0056] Example 10

[0057] In this example, the time of the hydrothermal treatment in step (3) in Example 1 is replaced from 20 hours to 12 hours, and the other conditions are exactly the same as those in Example 1.

[0058] Embodiment 11

[0059] In this example, the time of the hydrothermal treatment in step (3) in Example 1 is replaced from 20 hours to 24 hours, and the other conditions are exactly the same as those in Example 1.

[0060] Example 12

[0061] In this comparative example, the Bi4Ti3O 12 Replaced with BiVO4, other conditions are exactly the same as those in Example 1. Wherein, the preparation method of BiVO4 is as follows: 3 mmol of bismuth nitrate pentahydrate is dissolved in 15 ml of 2 mol / L nitric acid solution, stirred to dissolve to obtain solution A; 3 mmol of ammonium metavanadate is dissolved in 15 ml of 2 mol / L sodium hydroxide solution, and stirred continuously to obtain solution B; solution A is slowly added to solution B to obtain a mixed solution, and the pH of the mixed solution is adjusted to 10 with a 2 mol / L sodium hydroxide solution, and after stirring for 30 minutes, the mixed solution is transferred to a reactor, and hydrothermally reacted at 120 degrees Celsius for 12 hours; after the reaction is completed, the product is centrifuged and washed, and dried at 60 degrees Celsius to obtain BiVO4.

[0062] According to the test results ( Figure 1 , Figure 2) It can be seen that the best embodiment of the present invention is embodiment 1. The Bi4Ti3O synthesized in embodiment 1 12 -The photocatalytic oxidation efficiency of BiPO4 catalyst for NO with an initial concentration of 500 ppb (parts per billion) was 73.05%, exceeding that of single Bi4Ti3O 12 (63.45%), and the production of NO2 is low. Figure 3 , Figure 4 The scanning electron microscope image shows that Bi4Ti3O 12 -BiPO4 exhibits the same 12 Similar nanoflower-like morphology indicates that BiPO4 has achieved 12 In-situ growth on the surface. This unique in-situ preparation method enables the heterojunction to form a closer contact interface, which is very beneficial to the transfer and separation of photogenerated carriers, thereby greatly improving the efficiency of photocatalytic oxidation of NO and inhibiting the generation of NO2. The catalyst has stable properties, simple preparation process and low cost. It is expected to be widely used in the fields of photocatalytic degradation of pollutants in the atmosphere and water, and has practical application prospects and value.

[0063] The applicant declares that the above is only a practical implementation of the present invention, but the protection scope of the present invention is not limited thereto. It should be clear to those skilled in the art that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A Bi4Ti3O 12 -The in-situ preparation method of BiPO4 composite photocatalyst is characterized by: The Bi4Ti3O 12 The preparation method of the BiPO4 composite photocatalyst is as follows: (1) Preparation of Bi4Ti3O 12 : Dissolve bismuth nitrate pentahydrate, tetrabutyl titanate and sodium hydroxide in deionized water, stir for 15 to 30 minutes, ultrasonicate for 15 to 30 minutes, stir for 30 to 60 minutes, then perform hydrothermal treatment, wash and dry to obtain Bi4Ti3O 12 ; (2) preparing sodium dihydrogen phosphate solution; (3) Preparation of Bi4Ti3O 12 -BiPO4: Bi4Ti3O prepared in step (1) 12 After being mixed with deionized water, the mixture is ultrasonicated for 30 to 60 minutes, and then mixed with the sodium dihydrogen phosphate solution prepared in step (2) and stirred for 30 to 60 minutes, and then subjected to hydrothermal treatment, and then washed and dried to obtain Bi4Ti3O 12 -BiPO4.

2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of bismuth nitrate pentahydrate to tetrabutyl titanate is 4:3, the molar ratio of sodium hydroxide to bismuth nitrate is 45:1, and the molar ratio of deionized water to sodium hydroxide is 11:

1.

3. The preparation method according to claim 1, characterized in that: In step (1), the hydrothermal treatment uses a hydrothermal kettle with a capacity of 50 ml, the reaction temperature is 150 to 200 degrees Celsius, and the reaction time is 10 to 24 hours.

4. The preparation method according to claim 1, characterized in that: In step (1), the washing method is to use deionized water and anhydrous ethanol for cleaning.

5. The preparation method according to claim 1, characterized in that: In step (1), the drying temperature is 60 to 80 degrees Celsius.

6. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the sodium dihydrogen phosphate solution is 0.25 to 1.0 mol / L.

7. The preparation method according to claim 1, characterized in that: In step (3), the Bi4Ti3O 12 The molar ratio of sodium dihydrogen phosphate to sodium dihydrogen phosphate is 0.2 to 0.

5.

8. The preparation method according to claim 1, characterized in that: In step (3), the hydrothermal treatment uses a hydrothermal kettle with a capacity of 50 ml, the reaction temperature is 150-200 degrees Celsius, and the reaction time is 12-24 hours.

9. The preparation method according to claim 1, characterized in that: In step (3), the washing method is to use deionized water and anhydrous ethanol for cleaning.

10. The preparation method according to claim 1, characterized in that: In step (3), the drying temperature is 60 to 80 degrees Celsius.