Blue-green algae-based photocatalyst as well as preparation method and application thereof

The preparation of Fe single-atom doped g-C3N4 photocatalyst by co-pyrolyzing cyanobacterium carbide and g-C3N4 precursors was solved, and the problem of low efficiency of existing g-C3N4 photocatalysts was achieved, and high activity and high selectivity CO2 reduction was achieved , and reduces costs and is suitable for industrial applications.

CN118925773APending Publication Date: 2024-11-12NANJING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980519.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing graphite carbon nitride (g-C3N4) photocatalysts have low efficiency during CO2 reduction, low active position, high charge recombination, narrow light absorption, poor product selectivity, and the high cost of precious metal modification limits its practical application.

Method used

Using a photocatalyst composited by carbon nitride g-C3N4 nanosheets and Fe matrix, the g-C3N4 photocatalyst with uniformly supported Fe single atoms was prepared by co-pyrolysis of cyanobacteria as Fe single atom precursor. , the elements and biological macromolecules in cyanobacteria are used to form synergistic effects, nitrogen doping sites and protective layers during the calcination process, and improve the activity and stability of the catalyst.

Benefits of technology

The catalytic activity and selectivity of the photocatalyst are significantly improved, the yields of CO and CH4 are significantly improved, the specific surface area of ​​the catalyst increases, the reaction efficiency and product selectivity are improved, and the preparation method is simple and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925773A_ABST
    Figure CN118925773A_ABST
Patent Text Reader

Abstract

The invention discloses a photocatalyst based on blue-green algae and a preparation method and application thereof, the catalyst is formed by compounding a carbon nitride g-C3N4 nanosheet and a Fe matrix, g-C3N4 is a carrier, Fe monatomic is uniformly loaded on the surface of g-C3N4, and the monatomic Fe and four N atoms are combined and limited in a g-C3N4 layer; the Fe monatomic precursor is carbonized blue-green algae; the photocatalyst is obtained by calcining carbonized blue-green algae and a g-C3N4 precursor; the g-C3N4 is modified through the carbonized blue-green algae, so that the catalytic activity and selectivity of the catalyst are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photocatalysis technology, and in particular to a photocatalyst based on cyanobacteria and a preparation method and application thereof. Background Art

[0002] Solar energy is an inexhaustible and sustainable energy source. Therefore, the use of photocatalytic technology to reduce carbon dioxide has great development prospects.

[0003] Photocatalytic conversion of CO 2 The conversion of TiO into chemical fuels provides a new alternative to reduce anthropogenic emissions and realize carbon cycle. The design and synthesis of efficient photocatalysts are crucial for their practical application. 2 , C 3 N 4 Abundant semiconductor materials such as 2 Among various semiconductors, graphitic carbon nitride (gC 3 N 4 ) has attracted much attention due to its large specific surface area, adjustable band gap and low cost. However, the original gC 3 N 4 CO 2 The conversion efficiency is far lower than expected, which is mainly limited by factors such as its low active site, high charge recombination, narrow light absorption, and poor product selectivity.

[0004] To address these limitations, people have been working on exploring various strategies to improve catalytic activity and selectivity, including noble metal modification, element doping, heterostructure construction, and photosensitizer modification. 2 The reduction efficiency is still relatively low, and the high cost of noble metals inevitably limits their practical applications. 3 N 4 Based photocatalysts are urgently needed. Summary of the invention

[0005] Purpose of the invention: The first purpose of the present invention is to provide a method for improving gC 3 N 4 The catalytic activity of the cyanobacteria-based photocatalyst is improved; the second object of the present invention is to provide a method for preparing the cyanobacteria-based photocatalyst; the third object of the present invention is to provide the cyanobacteria-based photocatalyst in the photocatalytic reduction of CO 2 Produces CO and CH 4 Application in.

[0006] Technical solution: The carbon nitride gC 3 N 4Nanosheets and Fe matrix composite, gC 3 N 4 As the carrier, Fe single atoms are uniformly loaded on gC 3 N 4 On the surface, a single Fe atom is bound to four N atoms and is confined to the gC 3 N 4 layer; the Fe single atom precursor is carbonized cyanobacteria; the photocatalyst is carbonized cyanobacteria and gC 3 N 4 The precursor is obtained by calcining.

[0007] Preferably, the mass of the Fe single atom accounts for 0.001 to 0.015 wt % of the mass of the single atom photocatalyst.

[0008] Preferably, the gC 3 N 4 The mass ratio to carbonized cyanobacteria is: 1:0.6~1.4.

[0009] The method for preparing the cyanobacteria-based photocatalyst of the present invention comprises the following steps:

[0010] (1) carbonizing the cyanobacteria to obtain carbonized cyanobacteria;

[0011] (2) gC 3 N 4 The precursor is added to the solvent, followed by the carbonized cyanobacteria, mixed evenly and heated until the solvent is completely evaporated, the obtained material is ground and calcined to obtain Fe-SA / gC 3 N 4 Photocatalyst.

[0012] Preferably, in step (1), the carbonization treatment is: drying and grinding the cyanobacteria, and then calcining them under a nitrogen atmosphere.

[0013] Preferably, the cyanobacteria are ground in a ball mill.

[0014] Preferably, in step (1), the carbonization treatment is carried out in a tubular furnace, the calcination temperature is 700-900°C, the calcination time is 1-3h, the calcination atmosphere is nitrogen, and the heating rate is 4-6°C / min.

[0015] In step (2), gC 3 N 4 The precursor and carbonized cyanobacteria are added to the solvent, mixed evenly, and heated until the solvent is completely evaporated to make gC 3 N 4 The precursor and the carbonized cyanobacteria are fully mixed.

[0016] Preferably, in step (2), the heating temperature is 60-100°C.

[0017] Preferably, the gC 3 N 4 The precursor of cyanamide is urea, thiourea, melamine or dicyandiamide.

[0018] Preferably, the solvent is deionized water.

[0019] Preferably, the gC 3 N 4 The precursor is urea, the mass of cyanobacteria is 0-2g, the mass of urea is 8-12g, and the solvent is 20-40mL deionized water.

[0020] Preferably, in step (2), the calcination is carried out in a tubular furnace, the calcination temperature is 400-600° C., the calcination time is 3-5 hours, the calcination atmosphere is nitrogen, and the heating rate is 2-3° C. / min.

[0021] The cyanobacteria-based photocatalyst of the present invention is used for photocatalytic reduction of CO 2 Produces CO and CH 4 Application in.

[0022] The CO 2 The reduction products are CO and CH 4 The yield ratio is 1:0.01~0.13.

[0023] Invention mechanism: The present invention proposes a spirulina-doped carbon nitride (g-C3N4) photocatalyst based on blue algae, which significantly improves the photocatalytic activity and stability of the photocatalyst.

[0024] C 3 N 4 The presence of abundant tri-s-triazine motifs and electron-rich N atoms can promote the coordination and anchoring of single metal atoms. 3 N 4 Small nitrogen-containing molecules in the precursor solution, such as urea solution, are beneficial for anchoring more iron elements during high-temperature pyrolysis.

[0025] Cyanobacteria have the following effects: (1) The elements in cyanobacterial biomass produce synergistic effects: trace metal elements may produce synergistic effects with iron atoms, optimize the electronic structure and surface properties of the catalyst, and enhance the efficiency of the photocatalytic reaction; (2) Suitable nitrogen doping sites are formed: the nitrogen generated by the decomposition of proteins in cyanobacteria during the calcination process can form a large number of nitrogen doping sites, which can enhance the separation efficiency of photogenerated electrons and holes and improve the photocatalytic activity; (3) Distribution of active sites: The decomposition products of biomacromolecules can help evenly disperse iron atoms, prevent the agglomeration of iron atoms, ensure the uniform distribution of single-atom catalytic sites, and improve the photocatalytic performance; (4) Protection of active centers: The vitamins and antioxidants in cyanobacteria can form a protective layer during the calcination process to prevent iron atoms from agglomerating or deactivating at high temperatures and maintain the high activity of single-atom catalytic centers; (5) Formation of pore structure: The polysaccharides and lipids of cyanobacterial species volatilize and decompose during the calcination process to form a porous structure, which is beneficial to increase the specific surface area of ​​the catalyst, enhance the contact area between the catalyst and the reactants, and promote the reaction.

[0026] By introducing iron-rich Spirulina, on the one hand, the specific surface area and light absorption capacity of g-C3N4 were improved, while the electron-hole recombination was reduced. The interfacial interaction between Spirulina and g-C3N4 improved the separation and migration efficiency of photogenerated carriers and enhanced the activity of the photocatalyst. On the other hand, the Fe element, as an active site, further promoted the adsorption and reduction of CO2.

[0027] Using the uniform distribution of iron precursors and gC in biomass cyanobacteria 3 N 4 Precursor co-pyrolysis strategy and in-situ conversion to achieve green preparation of Fe single atom-doped gC 3 N 4 (Fe-SA / gC 3 N 4 ) catalyst, pristine carbon nitride gC 3 N 4 The single Fe atom is bound to four N atoms and is confined to gC 3 N 4 layer, serving as active sites to promote CO 2 molecules, thereby regulating and improving the photocatalytic CO 2 Activity and selectivity for CO reduction.

[0028] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) by modifying the carbonized cyanobacteria into gC 3 N 4 , which improved the catalytic activity and selectivity of the catalyst; (2) The maximum reduction product yield of the best catalyst in four hours was 116.56 μmol g-1 The yield of CO was 102.96 μmol g -1 , CH 4 The yield was 13.6 μmol g -1 ; (3) The preparation method is simple and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 X-ray diffraction (XRD) patterns of carbon dioxide reduction photocatalysts prepared in Examples 1 to 3 and Comparative Example 1;

[0030] Figure 2 This is a transmission electron microscope (TEM) image of the carbon dioxide reduction photocatalyst prepared in Example 2;

[0031] Figure 3 This is a high-angle annular dark field scanning transmission (HAADF-STEM) image of the carbon dioxide reduction photocatalyst prepared in Example 2.

[0032] Figure 4 The STEM-EDX elemental mapping diagram of the carbon dioxide reduction photocatalyst prepared in Example 2 is a spherical aberration electron microscope scanning transmission element mapping energy spectrum (STEM-EDX elemental mapping);

[0033] Figure 5 The photocatalytic carbon dioxide reduction rate diagram of carbon monoxide and methane production of carbon dioxide reduction photocatalysts of Examples 1 to 3 and Comparative Examples 1 to 2;

[0034] Figure 6 is a UV-visible diffuse reflectance spectrum (DRS) of the carbon dioxide reduction photocatalyst of Example 2;

[0035] Figure 7 This is a stability test diagram of the carbon dioxide reduction photocatalyst prepared in Example 2. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below in conjunction with embodiments.

[0037] Example 1

[0038] The preparation method of the cyanobacteria-based photocatalyst of the present invention comprises the following steps:

[0039] (1) Preparation of Carbonized Spirulina

[0040] 1.0 g of Spirulina was ground into powder in a ball mill, and all the dried powder was calcined in a tube furnace under nitrogen atmosphere at a calcination temperature of 800°C, a heating rate of 5°C / min, and a calcination time of 2 h to obtain 0.3685 g of carbonized Spirulina;

[0041] (2) Preparation of Fe-SA / gC 3 N 4 Photocatalyst

[0042] 10g urea (theoretically, 0.457g gC can be obtained after calcination) 3 N 4 ) was dissolved in 30 ml of deionized water, and then all the carbonized spirulina obtained in step (1) was added, and the mixture was stirred continuously for 12 h to be evenly mixed, and the resulting solution was heated at 80° C. until the water was completely evaporated; the dried mixture was ground and calcined in a tube furnace under a nitrogen atmosphere at a calcination temperature of 550° C., a heating rate of 2.3° C. / min, and a calcination time of 4 h to obtain Fe-SA / gC 3 N 4 Photocatalyst.

[0043] According to ICP test, the catalyst contains 0.007wt% Fe.

[0044] Example 2

[0045] The preparation method of the cyanobacteria-based photocatalyst of the present invention comprises the following steps:

[0046] (1) Preparation of Carbonized Spirulina

[0047] 1.5 g of Spirulina was ground into powder in a ball mill, and all the dried powder was calcined in a tube furnace under nitrogen atmosphere at a temperature of 800 °C, a heating rate of 5 °C / min, and a calcination time of 2 h to obtain 0.5480 g of carbonized Spirulina;

[0048] (2) Preparation of Fe-SA / gC 3 N 4 Photocatalyst

[0049] 10 g of urea was dissolved in 30 ml of deionized water, and then all the carbonized spirulina obtained in step (1) was added, and the mixture was stirred continuously for 12 h to be evenly mixed, and then the resulting solution was heated at 80° C. until the water was completely evaporated; the dried mixture was ground and calcined in a tube furnace under a nitrogen atmosphere at a calcination temperature of 550° C., a heating rate of 2.3° C. / min, and a calcination time of 4 h to obtain Fe-SA / gC 3 N 4 Photocatalyst.

[0050] According to ICP test, the catalyst contains 0.01wt% Fe.

[0051] Example 3

[0052] The preparation method of the cyanobacteria-based photocatalyst of the present invention comprises the following steps:

[0053] (1) Preparation of Carbonized Spirulina

[0054] 2.0 g of Spirulina was ground into powder in a ball mill, and all the dried powder was calcined in a tube furnace under nitrogen atmosphere at a calcination temperature of 800 °C, a heating rate of 5 °C / min, and a calcination time of 2 h to obtain 0.7314 g of carbonized Spirulina;

[0055] (2) Preparation of Fe-SA / gC 3 N 4 Photocatalyst

[0056] 10 g of urea was dissolved in 30 ml of deionized water, and then all the carbonized spirulina obtained in step (1) was added, and the mixture was stirred continuously for 12 h to be evenly mixed, and then the resulting solution was heated at 80° C. until the water was completely evaporated; the dried mixture was ground and calcined in a tube furnace under a nitrogen atmosphere at a calcination temperature of 550° C., a heating rate of 2.3° C. / min, and a calcination time of 4 h to obtain Fe-SA / gC 3 N 4 Photocatalyst.

[0057] According to ICP test, the catalyst contains 0.015wt% Fe.

[0058] Comparative Example 1

[0059] Comparative Example Carbon Nitride gC 3 N 4 The preparation method is as follows:

[0060] 10g urea was placed in a muffle furnace and calcined at 550℃, a heating rate of 2.3℃ / min, and a calcination time of 4h to obtain gC 3 N 4 .

[0061] Comparative Example 2

[0062] Based on Example 2, 0.000224 g FeCl 3 6H 2 O g replaced carbonized spirulina, and the other conditions remained unchanged.

[0063] Structural characterization

[0064] The carbon dioxide reduction photocatalysts of Examples 1 to 3 and Comparative Example 1 were characterized by X-ray diffraction (XRD). Figure 1 As shown. Figure 1 It can be seen that all samples show the characteristic peaks of carbon nitride, indicating that graphite phase carbon nitride was successfully synthesized.

[0065] The catalyst prepared in Example 2 was characterized by transmission electron microscopy (TEM), spherical aberration electron microscopy, HAADF-STEM and STEM–EDXelemental mapping. Figures 2 to 4 shown.

[0066] Depend on Figures 2-3 It can be seen that Fe-SA / gC 3 N 4 It is composed of ultra-thin gC 3 N 4 It is composed of nanosheets and Fe matrix.

[0067] from Figure 3 Some evenly dispersed bright spots can be observed in the spherical aberration electron microscope image. These bright spots with different brightness further confirm the Fe-SA / gC 3 N 4 The metal sites where Fe atoms are dispersed are highlighted in bright red circles.

[0068] Figure 4 Provides Fe-SA / gC 3 N 4 The high-angle annular dark field scanning transmission electron microscopy (HAADF-SEM) and element mapping images show that the existing samples contain uniformly distributed C, N, and Fe elements. The Fe element in the composite material is uniformly dispersed on the carbon nitride matrix, and no obvious Fe nanoparticles are observed. Combined with the above-mentioned XRD analysis, it is effectively proved that Fe exists in the carbon nitride matrix in the form of atomic dispersion.

[0069] Performance Characterization

[0070] The reduction performance of the carbon dioxide reduction photocatalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was tested, and the testing method included the following steps:

[0071] (1) Add 10 mg of catalyst, 9 mL of acetonitrile, 1 mL of ultrapure water, and 2 mL of triethanolamine (TEOA) into a 100 mL beaker and sonicate for 30 min.

[0072] (2) transferring the ultrasonic reaction solution into a reactor;

[0073] (3) Install the reactor on the photocatalytic device and start the vacuum pump to evacuate for 20 minutes;

[0074] (4) Then use CO 2 The whole reaction device was cleaned 3 times with gas to remove the air in the device and avoid interference;

[0075] (5) Turn on the magnetic stirrer, xenon lamp, and gas chromatograph;

[0076] (6) Photocatalytic reaction for 4 hours.

[0077] The results are as follows Figure 5 shown.

[0078] Depend on Figure 5 It can be seen that as the Fe content increases in Examples 1 to 3, the yields first increase and then decrease. The carbon dioxide reduction rate of the catalyst prepared in Example 2 to produce carbon monoxide is as high as 25.74 μmol g -1 h -1 The carbon dioxide reduction effect of the catalyst in Comparative Example 1 is significantly reduced relative to that in Example 2, which proves that the introduction of Fe single atoms improves the gC 3 N 4 The structure of gC 3 N 4 Comparative Example 2 relative to the implementation of the catalyst in Example 2 significantly reduced the carbon dioxide reduction effect, this is because the inorganic iron salt only provides a single atom of Fe to enter the gC 3 N 4 There is no 3 N 4 The structure of the spirulina is modified, and spirulina not only provides Fe single atoms, but also uses the iron precursors evenly distributed in the biomass cyanobacteria to react with gC 3 N 4 Precursor co-pyrolysis strategy and in-situ conversion to achieve green preparation of Fe single atom-doped gC 3 N 4 (Fe-SA / g-C3N4) catalyst, pristine carbon nitride gC 3 N 4 The single Fe atom is bound to four N atoms and is confined to gC 3 N 4 layer, serving as active sites to promote CO 2 molecules, thereby regulating and improving the photocatalytic CO 2 Activity and selectivity for CO reduction.

[0079] The carbon dioxide reduction photocatalysts prepared in Examples 1 to 3 and Comparative Example 1 were characterized by UV-visible diffuse reflectance spectroscopy (DRS). Figure 6 shown.

[0080] By UV-vis DRS Figure 6 It can be seen that all photocatalysts have strong absorption in the visible light region, and the absorption edge is in the visible light region. The absorption of visible light by Examples 1 to 3 is better than that of Comparative Example 1. The reason is that Fe is loaded onto gC 3 N 4 The substrate produces a synergistic effect, acting as an active site to promote CO2 molecules, thereby regulating and improving the photocatalytic CO 2 Activity and selectivity for CO reduction.

[0081] The stability test of the carbon dioxide reduction photocatalyst of Example 2 was carried out, and the results were as follows: Figure 7 shown.

[0082] Depend on Figure 7 It can be found that the material maintained good stability after 12 hours of carbon dioxide reduction test. The production of carbon monoxide and methane decreased slightly in the third cycle, while the production was stable in the first two cycles, proving that the material maintained good stability.

Claims

1. A photocatalyst based on cyanobacteria, characterized in that: The invention is composed of a composite of carbon nitride g-C3N4 nanosheets and an Fe matrix, wherein g-C3N4 is used as a carrier, single Fe atoms are uniformly loaded on the surface of g-C3N4, and single Fe atoms are combined with four N atoms and confined in the g-C3N4 layer; the single Fe atom precursor is carbonized cyanobacteria; and the photocatalyst is obtained by calcining the carbonized cyanobacteria and the g-C3N4 precursor.

2. The cyanobacteria-based photocatalyst according to claim 1, characterized in that The mass of the Fe single atom accounts for 0.001 to 0.015 wt % of the mass of the single atom photocatalyst.

3. The cyanobacteria-based photocatalyst according to claim 1, characterized in that The mass ratio of the g-C3N4 to the carbonized cyanobacteria is 1:0.6-1.

4.

4. A method for preparing a cyanobacteria-based photocatalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) carbonizing the cyanobacteria to obtain carbonized cyanobacteria; (2) Add the g-C3N4 precursor to the solvent, then add the carbonized cyanobacteria, mix well, heat until the solvent is completely evaporated, grind the obtained material and calcine it to obtain the Fe-SA / g-C3N4 photocatalyst.

5. The method for preparing a photocatalyst based on cyanobacteria according to claim 4, characterized in that: The heating temperature is 60-100°C.

6. The method for preparing a photocatalyst based on cyanobacteria according to claim 4, characterized in that: The precursor of the g-C3N4 is urea, thiourea, melamine or dicyandiamide.

7. The method for preparing a photocatalyst based on cyanobacteria according to claim 4, characterized in that: In step (1), the calcination temperature of the carbonization treatment is 700-900° C., the calcination time is 1-3 hours, and the calcination atmosphere is nitrogen.

8. The method for preparing a photocatalyst based on cyanobacteria according to claim 4, characterized in that: In step (2), the calcination temperature is 400-600° C., the calcination time is 3-5 hours, and the calcination atmosphere is nitrogen.

9. Use of the cyanobacteria-based photocatalyst according to any one of claims 1 to 3 in photocatalytic reduction of CO2 to produce CO and CH4.

10. The use according to claim 9, characterized in that: The yield ratio of the CO2 reduction products CO and CH4 is 1:0.01-0.13.