Bio-oil hydrodeoxygenation oxygen-enriched defect NiM / NC catalyst as well as preparation method and application thereof

CN118925775APending Publication Date: 2024-11-12ZHENGZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410989675.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

但是,该催化剂仅具有Ni活性位点,且只有基体RGO具有层状结构,活性位点与反应物的接触有限,因此其加氢脱氧反应仍需在高压H2下采用较高的催化剂用量实现

Benefits of technology

[0030] 1) The present invention prepares a NiM/NC catalyst with a flower-like layered structure with a high specific surface area through a simple hydrothermal method, and has hydrodeoxygenation performance similar to that of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925775A_ABST
    Figure CN118925775A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-oil hydrodeoxygenation oxygen-enriched defect NiM / NC catalyst as well as a preparation method and application thereof. The catalyst is of a flower-shaped layered structure formed by loading a NiM active center on an N-doped C carrier, and the NiM active center has a Ni active center and a MyOx oxygen vacancy active center at the same time. The Ni active center and the MyOx oxygen vacancy center of the catalyst promote hydrocracking of C-O bonds in bio-oil, and efficient hydrodeoxygenation performance is achieved. Under mild conditions, the conversion rate of guaiacol reaches up to 99%, and the selectivity of cyclohexanol is close to 90%. The invention provides a low-cost, efficient and stable non-noble metal catalyst for the traditional biomass hydrodeoxygenation reaction, and has a good large-scale application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst and a preparation method and application thereof, belonging to the technical field of catalytic hydrogenation and biomass energy utilization. Background Art

[0002] With the increasing shortage of petroleum resources and the increasing attention paid to energy and environmental issues. Biomass resources have gradually become an important way to solve the energy crisis and reduce environmental pressure due to their renewability and environmental friendliness. Green and renewable biomass oil can be obtained through biomass pyrolysis and catalytic processes. However, the oxygen content of bio-oil is too high, which makes it impossible to use it directly as fuel. Therefore, the catalytic process of bio-oil hydrodeoxygenation has emerged. However, the common bio-oil hydrodeoxygenation catalysts are precious metal catalysts, such as Ru, Pt and Pd, etc. These catalysts are not only expensive, but also have low deoxygenation efficiency. In addition, the hydrodeoxygenation of bio-oil is carried out under high pressure H2, which has great safety hazards.

[0003] Ni-based non-precious metal catalysts have catalytic hydrogenation performance similar to that of precious metals, but the cost is less than one-tenth of that of precious metals. Chinese patent CN108671947 B discloses a Ni2P / reduced graphene oxide catalyst for bio-oil hydrodeoxygenation reaction and its preparation method. The conversion rate of benzaldehyde by the catalyst is more than 96%, indicating that the Ni-based non-precious metal catalyst has good catalytic hydrodeoxygenation performance. However, the catalyst only has Ni active sites, and only the matrix RGO has a layered structure, and the contact between the active sites and the reactants is limited, so its hydrodeoxygenation reaction still needs to be achieved with a higher catalyst dosage under high pressure H2.

[0004] Therefore, developing a low-cost and efficient non-precious metal catalyst for in-situ hydrodeoxygenation of biomass resources, especially lignin, to produce high calorific value bio-oil fuel products under safe conditions is of far-reaching significance for promoting the development of green chemistry and achieving a sustainable society. Summary of the invention

[0005] In view of the defects existing in the prior art, the first object of the present invention is to provide a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst, which has a high specific surface area and a special flower-like layered structure. y O x The synergistic effect of oxygen vacancy centers leads to efficient hydrodeoxygenation performance.

[0006] The second object of the present invention is to provide a method for preparing a bio-oil hydrodeoxygenation oxygen-defective NiM / NC catalyst, which can obtain a flower-shaped NiM / NC catalyst with a high specific surface area by a simple hydrothermal method, and has the advantages of simple process flow, easy availability of raw materials and low cost.

[0007] The third object of the present invention is to provide an application of a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst, which is used as a catalyst for the in-situ hydrodeoxygenation reaction of bio-oil or bio-oil model compounds. The reaction is carried out under the condition of a hydrogen supply solvent, without using high-pressure H2, and is safe and efficient.

[0008] In order to achieve the above technical objectives, the present invention provides a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst, which is composed of a NiM active center supported on an N-doped C carrier to form a flower-like layered structure; the NiM active center has both a Ni active center and a M y O x Oxygen vacancy active center; wherein x is 1 to 3, such as 1, 2 or 3; y is 1 to 3, such as 1, 2 or 3; M is selected from any one of the lanthanide metals or manganese.

[0009] The NiM / NC catalyst of the technical solution of the present invention has a special flower-like layered structure, which not only significantly increases the specific surface area of ​​the catalyst and promotes the contact area between the catalyst and the substrate, but also can be well adsorbed with the substrate and the subsequent hydrodeoxygenation reaction. Compared with a simple layered structure, the flower-like layered structure of the present invention can more evenly disperse the catalytic active components, avoid excessive concentration of local active sites, and effectively reduce the risk of catalyst sintering and deactivation. In addition, the catalyst of the present invention has both Ni active centers and M y O x Oxygen vacancy active centers, among which Ni active centers are beneficial to promote the in-situ cracking of hydrogen donor solvents to release H + ions, active hydrogen overflows to M y O x Oxygen vacancies: The abundant oxygen vacancies in the catalyst have the function of enriching active hydrogen and promoting the adsorption and cracking of CO bonds. y O x The synergistic effect of the oxygen vacancy active center achieves in-situ cracking of CO in the bio-oil and reduces the oxygen content of the bio-oil. Therefore, the catalyst of the present invention can have high catalytic activity and selectivity by adding a hydrogen supply solvent without using high-pressure H2.

[0010] As a preferred solution, the loading amount of active metal Ni in the catalyst is 20 to 40 wt % of the total weight of the catalyst.

[0011] As a preferred solution, the metal M in the catalyst is Mn, Ce or La. The further preferred metal M species of the present invention have a better effect of catalyzing the hydrocracking of CO bonds in bio-oil.

[0012] As a preferred solution, the loading amount of M in the catalyst is 1 to 10 wt % of the total weight of the catalyst.

[0013] The Ni metal in the catalyst of the present invention can promote the in-situ cracking of the hydrogen supply solvent to release H + ions, but too high a Ni loading will not only lead to the agglomeration of the active metals of the catalyst and reduce the catalytic activity, but also lead to too high a catalyst cost. M metal introduces abundant oxygen vacancies, but too high a metal M loading will not further increase the oxygen vacancy concentration, so the catalyst performance obtained when the Ni loading and the M loading are within the selected range of the present invention is optimal.

[0014] The present invention also provides a method for preparing a bio-oil hydrodeoxygenation oxygen-deficient NiM / NC catalyst, which comprises subjecting a mixed solution containing a Ni salt, an M salt and a carrier source to a hydrothermal reaction to obtain a NiM / NC catalyst precursor; the NiM / NC catalyst precursor is calcined and reduced to obtain a catalyst; the carrier source is a compound containing both N and C; and the M salt is selected from any salt of a lanthanide metal or a manganese salt.

[0015] The technical solution of the present invention can obtain a flower-shaped NiM / NC catalyst with a high specific surface area through a simple hydrothermal method, and has the advantages of simple process flow, easy availability of raw materials and low cost.

[0016] As a preferred solution, the Ni salt is at least one of nickel nitrate, nickel chloride and nickel hydroxide.

[0017] As a preferred solution, the M salt is manganese nitrate, cerium nitrate or lanthanum nitrate.

[0018] As a preferred solution, the carrier source is at least one of imidazole, 2-methylimidazole and urea. The carrier source selected by the present invention contains both N source and C source, which is more conducive to in-situ synthesis of a structurally stable N-doped C carrier.

[0019] As a preferred solution, the mass ratio of the Ni salt to the carrier source is (0.8-3):1, and the mass ratio of the M salt to the carrier source is 1:(2-7).

[0020] As a preferred solution, the mixed solution further comprises at least one solvent selected from the group consisting of water, ethanol and methanol.

[0021] As a preferred solution, the conditions of the hydrothermal reaction are: temperature of 120-180° C. and time of 4-12 h.

[0022] As a preferred solution, the calcination conditions are: temperature of 400-800°C, time of 1-5h, and atmosphere of N2. The catalyst calcined below 600°C is very easy to be reduced, and the catalytic performance is stable. However, when the calcination temperature is too high, the flower-like layered structure of the catalyst collapses, and the active metals agglomerate, resulting in a decrease in catalytic performance. It is further preferred that the calcination temperature is 400-600°C.

[0023] As a preferred solution, the reduction conditions are: temperature of 500-600°C, time of 1-3h, and atmosphere of H2. The temperature of the reduction reaction of the present invention has a direct impact on the microstructure and catalytic performance of the NiM / NC catalyst. When the reduction temperature is too low, the active center of the catalyst cannot be fully exposed, thereby reducing the catalytic performance of the catalyst; and when the reduction temperature is too high, the flower-like structure of the catalyst collapses, and the catalyst agglomerates into a block structure.

[0024] The present invention also provides an application of a bio-oil hydrodeoxygenation oxygen-rich NiM / NC catalyst, which is used as a catalyst for in-situ hydrodeoxygenation of bio-oil or bio-oil model compounds. The NiM / NC catalyst selected by the present invention has a Ni active center that is beneficial to the production of hydrogen from the hydrogen supply solvent, and a M y O x The synergistic effect of oxygen vacancy centers promotes efficient hydrodeoxygenation performance and avoids the use of high-pressure H2.

[0025] As a preferred solution, the bio-oil is lignin oil and / or pyrolysis oil, and the bio-oil model compound is at least one of guaiacol, phenoxyethylbenzene and phenol.

[0026] As a preferred solution, the in-situ hydrodeoxygenation reaction conditions are: temperature of 130-220°C, time of 1-4h, and pressure of 1-4MPa. The temperature of the catalytic reaction has a direct impact on the conversion rate and product selectivity of the bio-oil. As the temperature increases and the time increases, the reaction conversion rate continues to rise until equilibrium is reached, and the product selectivity tends to be a product with a high degree of deoxygenation.

[0027] As a preferred solution, the mass ratio of the bio-oil or bio-oil model compound to the catalyst is (1-2): (1-3). As the amount of catalyst increases, the conversion of the reaction first increases and then stabilizes, so the appropriate amount of catalyst is beneficial to the control of production costs.

[0028] As a preferred solution, the hydrogen supply solvent for the in-situ hydrodeoxygenation reaction is at least one of isopropanol and formic acid. The preferred hydrogen supply solvent of the present invention is used as an in-situ hydrogen source, which avoids the use of hydrogen, reduces costs and improves the safety of the experiment.

[0029] Compared with the prior art, the technical solution of the present invention brings about innovative and beneficial technical effects:

[0030] 1) The present invention prepares a flower-like layered NiM / NC catalyst with a high specific surface area by a simple hydrothermal method, and the hydrodeoxygenation performance is similar to that of precious metals.

[0031] 2) Cheap non-precious metal NiM / NC catalyst has more advantages in cost and catalytic activity. The catalyst of the present invention has both Ni active center and M y O x Oxygen vacancy active center; Ni active center can promote the in-situ cracking of hydrogen donor solvent to release H + Ion and M y O x Oxygen vacancies can directly promote the cracking of CO in bio-oil in situ and reduce the oxygen content of bio-oil.

[0032] 3) The magnetic NiM / NC catalyst can be recycled and reused, which not only reduces the process production cost but also facilitates large-scale promotion and application.

[0033] 4) The hydrogen supply solvent used in the present invention is used as an in-situ hydrogen source, which is very safe in the reaction compared with high-pressure hydrogen, and there is no risk or safety hazard of hydrogen transportation and storage.

[0034] 5) The catalyst of the present invention has a conversion rate of up to 99% for guaiacol under mild conditions, and a selectivity for cyclohexanol close to 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the XRD pattern of the NiMn / NC catalyst in Example 2.

[0036] Figure 2 This is the SEM image of the NiMn / NC catalyst in Example 2.

[0037] Figure 3 The graph shows the conversion rate of guaiacol at different temperatures for the NiMn / NC catalyst in Example 2 and the Ni / NC catalyst in Comparative Example 3. DETAILED DESCRIPTION

[0038] The technical solution of the present invention will be further described below in conjunction with specific embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; these embodiments are only for a better understanding of the present invention, rather than limiting the scope of protection of the present invention.

[0039] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.

[0040] Example 1

[0041] In terms of catalyst, 4.35g nickel nitrate, 2.46g dimethylimidazole, 0.38g manganese nitrate, and 50ml methanol were added to a reactor and heated at 150°C for 9h to finally obtain a NiMn / NC catalyst precursor. Then, it was calcined at 600°C for 5 hours under a nitrogen atmosphere and reduced at 500°C for 1 hour under a hydrogen atmosphere to finally obtain a NiMn / NC catalyst. The catalyst has both Ni active centers and MnO2 oxygen vacancy active centers, with a Ni loading of 40wt% and a Mn loading of 3wt%.

[0042] Example 2

[0043] Compared with Example 1, the only difference is that the hydrogen reduction temperature is 600°C, and the other conditions and steps are the same, and finally a NiMn / NC catalyst is obtained. The catalyst has both Ni active centers and MnO oxygen vacancy active centers, and the Ni loading is 40wt% and the Mn loading is 3wt%.

[0044] Example 3

[0045] Compared with Example 2, the only difference is that the mass ratio of Ni salt to carrier source is reduced, the mass of nickel nitrate is replaced by 2.17g, and the other conditions and steps are the same, and finally a NiMn / NC catalyst is obtained. The catalyst has both Ni active centers and MnO oxygen vacancy active centers, and the Ni loading is 20wt% and the Mn loading is 3wt%.

[0046] Example 4

[0047] Compared with Example 2, the only difference is that the mass ratio of Mn salt to carrier source is increased, the mass of manganese nitrate is replaced by 1.14g, and the other conditions and steps are the same, and finally a NiMn / NC catalyst is obtained. The catalyst has both Ni active centers and MnO oxygen vacancy active centers, and the loading amount of Ni is 40wt% and the loading amount of Mn is 9wt%.

[0048] Example 5

[0049] Compared with Example 2, the only difference is that the type of M metal salt is changed, manganese nitrate is replaced by cerium nitrate, the mass is 0.49g, and the other conditions and steps are the same, and finally a NiCe / NC catalyst is obtained. The catalyst has both Ni active centers and CeO2 oxygen vacancy active centers, and the Ni loading is 40wt% and the Ce loading is 3wt%.

[0050] Example 6

[0051] Compared with Example 2, the only difference is that the type of M metal salt is changed, manganese nitrate is replaced by lanthanum nitrate, the mass is 0.49g, and the other conditions and steps are the same, and finally a NiLa / NC catalyst is obtained. The catalyst has both Ni active centers and La2O3 oxygen vacancy active centers, and the Ni loading is 40wt% and the La loading is 3wt%.

[0052] Comparative Example 1

[0053] Compared with Example 1, the only difference is that the hydrogen reduction temperature is 700°C, and the other conditions and steps are the same, and finally a NiMn / NC catalyst is obtained. The catalyst has both Ni active centers and MnO oxygen vacancy active centers, and the Ni loading is 40wt% and the Mn loading is 3wt%.

[0054] Comparative Example 2

[0055] Compared with Example 1, the only difference is that hydrogen reduction is not performed, and the other conditions and steps are the same, and finally a NiMn / NC catalyst precursor is obtained.

[0056] Comparative Example 3

[0057] Compared with Example 2, the only difference is that manganese nitrate is not added, and the other conditions and steps are the same, and finally a Ni / NC catalyst is obtained. The catalyst has only Ni active centers, and the Ni loading is 40wt%.

[0058] The specific surface area and pore volume parameter results of the catalysts prepared in Examples 1 to 6 and Comparative Examples 1 to 3 are shown in Table 1.

[0059] Table 1

[0060] serial number <![CDATA[Specific surface area / m 2 ·g -1 > <![CDATA[Pore volume / cm 3 ·g -1 > Example 1 238 0.19 Example 2 229 0.16 Example 3 232 0.21 Example 4 230 0.17 Example 5 196 0.19 Example 6 215 0.23 Comparative Example 1 125 0.29 Comparative Example 2 217 0.12 Comparative Example 3 235 0.17

[0061] As shown in Table 1, the catalysts of Examples 1 to 6 and Comparative Example 1, the catalyst precursor of Comparative Example 2, and the Ni / NC catalyst of Comparative Example 3 were subjected to nitrogen physical adsorption tests. The unreduced NiMn / NC catalyst precursor had a nitrogen adsorption capacity of 217 m 2 ·g -1 The specific surface area and pore volume of the catalysts in Examples 1 to 2 and Comparative Example 1 decrease with the increase of reduction temperature. This is because at a higher reduction temperature, the flower-like layer structure of the catalyst collapses, causing the catalyst to agglomerate into a block structure, thereby causing a decrease in specific surface area and pore volume. In Examples 3 to 4 and Comparative Example 3, changing the loading of Ni and Mn has little effect on the specific surface area and pore volume of the catalyst. Changing the type of M metal does not significantly change the specific surface area and pore volume of the catalysts in Examples 5 to 6.

[0062] Application Example 1

[0063] The NiMn / NC, NiCe / NC, NiLa / NC, Ni / NC catalysts and NiMn / NC catalyst precursors prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were used to perform hydrodeoxygenation reactions on bio-oil model compounds, respectively. Guaiacol, a typical bio-oil model compound, was selected as a substrate for study: 24.8 mg of guaiacol, 0.03 g of catalyst and 4 ml of isopropanol were added to a reactor and heated under 2 MPa nitrogen and 140° C. for 1 h. After the reaction, the samples obtained were analyzed by gas chromatography. The results are shown in Table 2.

[0064] Table 2

[0065] catalyst Guaiacol conversion rate / % Cyclohexanol selectivity / % Example 1 94.25 84.29 Example 2 99.51 89.68 Example 3 85.24 79.24 Example 4 99.46 90.12 Example 5 98.69 88.21 Example 6 99.03 93.22 Comparative Example 1 90.46 86.32 Comparative Example 2 0 0 Comparative Example 3 62.13 70.56

[0066] As shown in Table 2, the results of the hydrodeoxygenation reaction of guaiacol show that the NiMn / NC catalyst precursor without hydrogen reduction has no Ni 0 The presence of guaiacol results in the inability to produce hydrogen in situ, so no hydrogenation reaction occurs to guaiacol. As the reduction temperature increases, the catalysts in Examples 1 to 2 and Comparative Example 1 are beneficial to the conversion rate of guaiacol and the selectivity of the deoxygenated product cyclohexanol. However, at higher reduction temperatures, the flower-like layer structure of the catalyst collapses and the specific surface area and pore volume decrease, affecting the adsorption of the catalyst to guaiacol and the subsequent hydrogenation and deoxygenation reaction, resulting in a slight decrease in the conversion rate of guaiacol and the selectivity of the deoxygenated product cyclohexanol. In addition, under the reduction temperature conditions of Examples 1 to 2, MnO was detected. x Medium Mn 4+ To Mn 2+ The reduction in valence promotes the formation of oxygen vacancies and improves the catalytic performance of the catalyst in Example 2. With the further increase in reduction temperature, such as in Comparative Example 1, the valence of Mn in the catalyst tends to be stable, and the main reason for the decrease in catalytic performance is the agglomeration of active metals and the reduction in specific surface area at high temperature. The conversion rate of the catalyst to guaiacol in Example 3 decreases by reducing the loading of Ni metal, which may be caused by the fact that the active metal sites are not sufficient to meet the needs of in-situ hydrogen production and CO bond hydrogenation cracking. Increasing the loading of Mn metal, the conversion rate of the catalyst to guaiacol in Example 4 remains unchanged, which shows that excessive Mn loading will not further increase the oxygen vacancy concentration. The conversion rate of guaiacol by the Ni / NC catalyst in Comparative Example 3 is only 62.13%, which shows that the presence of only Ni hydrogenation without the synergistic effect of oxygen vacancies will greatly reduce the catalytic performance of the catalyst. Changing the type of M metal, the catalysts of Examples 5 to 6 still have Ni active centers and oxygen vacancy centers, so the conversion rate and selectivity of guaiacol are similar to those of the NiMn / NC catalyst.

[0067] Application Example 2

[0068] The NiMn / NC catalyst prepared in Example 2 and the Ni / NC catalyst prepared in Comparative Example 3 were applied to guaiacol as a substrate to study the effect of temperature (heating for 1 h at 120°C, 130°C, 140°C, 150°C, 160°C and 170°C, respectively). The other conditions and steps were the same as those in Application Example 1. After the reaction, the obtained samples were analyzed by gas chromatography. The results were as follows: Figure 3 .

[0069] Application Example 3

[0070] The NiMn / NC catalyst prepared in Example 2 was used for the in-situ hydrodeoxygenation reaction of lignin oil: 200 mg of lignin oil, 0.1 g of catalyst, and 6 ml of isopropanol were added to a reactor, and heated for 3 h under 2 MPa nitrogen and 220°C. After the reaction, the obtained sample was analyzed by gas chromatography. The results showed that the NiMn / NC catalyst had good hydrodeoxygenation performance and converted guaiacol and eugenol compounds in lignin oil into cyclohexanol products.

[0071] Results test:

[0072] like Figure 1 As shown, the NiMn / NC catalyst prepared in Example 2 was subjected to XRD analysis, and the results showed that the diffraction peaks at 44.3°, 51.7° and 76.3° were respectively attributed to the (111), (200) and (220) crystal planes of the metal Ni phase (JCPDS04-0850). In addition, due to the reoxidation of metal Ni during the storage, transfer and characterization of the sample in air, diffraction peaks at 37.3° and 63.0° were observed in the catalyst, corresponding to the (111) and (220) crystal planes of the NiO phase (JCPDS 73-1519).

[0073] like Figure 2 As shown, the NiMn / NC catalyst prepared in Example 2 exhibits a flower-like layered structure, which significantly increases the specific surface area of ​​the catalyst, promotes the contact area between the catalyst and the substrate, and can be well adsorbed with the substrate and undergo subsequent hydrodeoxygenation reactions.

[0074] like Figure 3 As shown, the NiMn / NC catalyst prepared in Example 2 and the Ni / NC catalyst prepared in Comparative Example 3 carried out in-situ hydrodeoxygenation reaction of guaiacol at different temperatures. As the reaction temperature increases, the conversion of guaiacol first increases and then tends to equilibrium. The conversion rate of guaiacol can reach up to 99%, and the conversion rate of NiMn / NC prepared in the present invention is significantly higher than the catalytic effect of the Ni / NC catalyst in Comparative Example 3.

[0075] The above embodiments are only for better explanation of the principles and practical applications of the present invention, so that those skilled in the relevant technical field can better understand and utilize the present invention, but they are not intended to limit the patent scope of the present invention. All equivalent changes made using the contents of the present invention are within the patent protection scope of the present invention.

Claims

1. A bio-oil hydrodeoxygenation oxygen-rich NiM / NC catalyst, Features: The catalyst is composed of a NiM active center supported on an N-doped C carrier to form a flower-like layered structure; the NiM active center has both a Ni active center and a M y O x Oxygen vacancy active center; Wherein, x is 1 to 3; y is 1 to 3; and M is selected from any one of the lanthanide metals or manganese.

2. The bio-oil hydrodeoxygenation oxygen-rich NiM / NC catalyst according to claim 1, Features: The loading amount of the active metal Ni in the catalyst is 20-40 wt % of the total weight of the catalyst.

3. A bio-oil hydrodeoxygenation NiM / NC catalyst according to claim 2, Features: The metal M in the catalyst is Mn, Ce or La, and the loading amount of M is 1 to 10 wt% of the total weight of the catalyst.

4. A method for preparing a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst according to any one of claims 1 to 3, Features: A mixed solution containing Ni salt, M salt and carrier source is subjected to hydrothermal reaction to obtain a NiM / NC catalyst precursor; The NiM / NC catalyst precursor is calcined and reduced to obtain; The carrier source is a compound containing both N and C; The M salt is selected from any salt of lanthanide metals or manganese salts.

5. The method for preparing a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst according to claim 4, Features: The Ni salt is at least one of nickel nitrate, nickel chloride and nickel hydroxide; The M salt is manganese nitrate, cerium nitrate or lanthanum nitrate; The carrier source is at least one of imidazole, 2-methylimidazole and urea.

6. The method for preparing a bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst according to claim 5, Features: The mixed solution also includes at least one solvent selected from the group consisting of water, ethanol and methanol.

7. A bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst and a preparation method thereof according to claim 6, Features: The conditions of the hydrothermal reaction are: temperature of 120-180° C. and time of 4-12 hours.

8. A bio-oil hydrodeoxygenation oxygen-rich defect NiM / NC catalyst and a preparation method thereof according to claim 4, Features: The calcination conditions are: temperature of 400-800°C, time of 1-5h, atmosphere of N 2 ; The reduction conditions are: temperature of 500-600°C, time of 1-3h, atmosphere of H 2 .

9. Use of the oxygen-deficient NiM / NC catalyst for bio-oil hydrodeoxygenation according to any one of claims 1 to 3, Features: It is used as a catalyst for the in situ hydrodeoxygenation reaction of bio-oil or bio-oil model compounds.

10. Use of a bio-oil hydrodeoxygenation oxygen-rich NiM / NC catalyst according to claim 9, Features: The in-situ hydrodeoxygenation reaction conditions are: temperature of 130-220° C., time of 1-4 h, nitrogen pressure of 1-4 MPa, and mass ratio of bio-oil or bio-oil model compound to catalyst of (1-2):(1-3).

Citation Information

Patent Citations

  • Ni2P / reduced graphene oxide catalyst for hydrodeoxygenation of bio-oil and its preparation method

    CN108671947B