Roll-type preparation method of pure titanium polar plate
Through slab preparation and coil hot rolling process, combined with EB smelting or VAR smelting + forging, the problem of low efficiency of single-piece hot rolling process is solved, and high-efficiency production of high-quality pure titanium electrode plates is achieved to meet the metallurgy and chemical industries' titanium Strict requirements of the board.
Patent Information
- Application Number
- CN202410974969.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing single-piece hot rolling process is low efficiency, long cycle and high cost, and cannot meet the demand for high-quality pure titanium electrode plates in the metallurgy and chemical industries. Especially in the processing of titanium plates with a thickness of ≥5mm, there is tissue uniformity and grains. Poor degree and poor surface quality.
The process routes of slab preparation, coil hot rolling, tissue control, pattern size control, and surface treatment include EB smelting or VAR smelting + forging to prepare flat ingots, and through peeling treatment, coil hot rolling, continuous annealing, annealing pressure Correction, cutting, grinding and cold straightening treatments ensure the satisfaction of grain size and geometric accuracy.
Mass production of high-quality pure titanium electrode plates with thickness of 5mm to 8mm and width of 800mm to 1500mm is achieved, which improves production efficiency, reduces costs, and ensures good performance of tissue uniformity, grain size ≥6 levels and surface quality.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metal processing, and in particular to a rolling preparation method of a pure titanium pole plate. Background Art
[0002] Pure titanium and titanium alloys are widely used in aerospace, marine, metallurgy, chemical industry and other fields because of their low density, good comprehensive performance and corrosion resistance. In recent years, with the continuous advancement of industrial technology, the quality requirements of raw materials and products in various industries have been continuously improved. Taking the metallurgical and chemical industries as an example, pure titanium plates are often used as the substrate for metallurgical plates, and precious metal coatings need to be applied on the surface of the titanium plates. The comprehensive performance, grain size and uniformity of titanium plates directly affect their service life and the quality of downstream products. In the high-end fields of metallurgy and chemical industry, the requirements for pure titanium plates are extremely strict. For example, the grain size grade of titanium plates is crucial to the quality of metallurgical products and the service life of titanium plates. Therefore, the grain size of titanium plates needs to be ≥6. The overall uniformity of the titanium plates has a great impact on metallurgical efficiency and product quality, so the grain size difference of the whole plate is ≤0.5; the unevenness of titanium plates is also a key factor, so the unevenness of titanium plates should reach ≤3mm / m; it can be seen that the quality requirements of pure titanium plates in titanium products are extremely high.
[0003] At present, the processing method of pure titanium plate products with a thickness of ≥5mm is mainly single-piece hot rolling. The process route is slab smelting, small ingot cutting, single-piece hot rolling, reversing rolling, organization control, oxide layer removal, sizing, straightening, and surface treatment. The single-piece hot rolling production method has low efficiency, long cycle, and high cost. On the one hand, with the increasing demand of the industry, on the other hand, industrial development has higher and higher requirements for the quality of raw materials and products, and the existing single-piece hot rolling process can no longer meet the needs of the industry.
[0004] The present invention provides a new process route suitable for batch production of pure titanium plates for chemical and metallurgical industries. Through slab preparation, coil hot rolling, structure control, plate size control, and surface treatment, high-quality pure titanium plates with good surface quality, comprehensive performance, and good structure uniformity can be stably obtained. Summary of the invention
[0005] In view of this, the present invention aims to propose a method for preparing a pure titanium pole plate in a rolled form, so as to achieve the purpose of producing a pure titanium pole plate in a rolled form with a thickness of 5 mm to 8 mm and a width of 800 mm to 1500 mm.
[0006] In the prior art, in order to realize the production of pure titanium plates, the titanium ingot is melted and cast, and then hot-rolled and cold-rolled for processing, and finally ground to produce 1-4mm pure titanium plates with high surface accuracy. In the traditional coil hot rolling process, due to the narrow thermoplastic processing temperature range of titanium, the flat ingot is often prone to rolling tearing due to product deformation during the rolling and thinning process, and has quality problems such as uniform organization, poor grain size, internal stress accumulation, and low surface quality, which are difficult to meet the requirements. In actual processing, the hot-rolled pure titanium plate is annealed to obtain a 4-10mm thick pure titanium plate. At this time, the pure titanium plate has quality problems such as uniform organization, poor grain size, many cracks, internal stress accumulation, and low surface quality. It is necessary to use cold rolling and mechanical processing to remove the thicker surface layer of the pure titanium plate to obtain a 1-4mm thick plate with more uniform grains and more stable performance. The whole process is long, time-consuming, material waste, and low production efficiency.
[0007] In order to solve various problems arising from the size change of pure titanium pole plates during hot rolling and shorten the long processing time and low production efficiency of the annealing process after hot rolling, the inventors obtained pure titanium pole plates whose grain size and geometric accuracy met the product process requirements through measures such as slab preparation, slab size control, slab post-coil hot rolling annealing process adjustment and mechanical processing, thereby improving production efficiency.
[0008] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0009] A method for preparing a pure titanium pole plate in a rolled form comprises the following steps:
[0010] S1: TA1 grade titanium is used as raw material, and EB smelting or VAR smelting + forging is used to prepare flat ingots, and the flat ingots are peeled after preparation;
[0011] S2: coil hot rolling; determine the hot rolling target thickness according to the annealing process, and roll the prepared flat ingot slab to the target thickness through rough rolling and finish rolling;
[0012] S3: Annealing treatment; when the coil is subjected to continuous annealing after hot rolling, the annealing temperature T1 is 765℃~870℃, the continuous annealing coil speed is V, and the oxide layer is removed by shot blasting + pickling process; when the coil is subjected to annealing press straightening after hot rolling, the annealing temperature T2 is 540℃~680℃, the holding time is t, and the oxide layer is removed after annealing;
[0013] S4: Cutting: cutting the annealed and press-corrected titanium plate or hot-rolled white titanium coil to the finished product size;
[0014] S5: Surface treatment: Grind the local defects on the plate surface, and then sandblast the plate after grinding;
[0015] S6: Cold straightening treatment is performed on the plates with large unevenness;
[0016] S7: pickling treatment.
[0017] Furthermore, in step S1, the chemical composition of titanium meets the requirements of GBT 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions" TA1 standard, and the impurity element content is: C≤0.03%, 0.02%≤O≤0.06%, N≤0.03%, H≤0.015%, Fe≤0.05%.
[0018] Furthermore, in step S1, the thickness of the prepared slabs ranges from 160 to 260 mm, and the thickness of the slabs to be peeled on one side after preparation ranges from 3 to 10 mm.
[0019] Furthermore, in step S1, when EB smelting is adopted, no more than 50% of recycled materials can be added, and the recycled materials are fully mixed with the titanium sponge particles before smelting and smelted once.
[0020] Further, in step S1, when VAR smelting is adopted, smelting is performed twice, and the ingot size is: H×W×L2,
[0021] Where: H = X × k1
[0022] W=X×k2
[0023] L2=L1×k3
[0024] Wherein X is the diameter of the VAR smelting ingot, L1 is the length of the VAR smelting ingot; H is the thickness of the flat ingot after forging; W is the width of the flat ingot after forging; L2 is the length of the flat ingot after forging; k1 is a coefficient of 0.15 to 0.25; k2 is a coefficient of 1.0 to 1.7; k3 is a coefficient of 2.6 to 3.2.
[0025] Furthermore, in step S2, the target thickness of the plate is h 总 , the finished product thickness is h, and the reserved thickness is h 工 ,h 总 =h+h 工 ;
[0026] During continuous annealing after hot rolling, h 工 Range: 0.05~0.2mm;
[0027] After hot rolling without continuous annealing, h 工 Range: 0.1~0.3mm.
[0028] Furthermore, in step S3, during continuous annealing, the annealing temperature T1 is 780°C to 850°C, the coiling speed V is in the range of 0.5m / min to 20m / min, and after annealing, a shot blasting + pickling process is used to remove the oxide layer.
[0029] Furthermore, in step S3, during annealing and press-straightening, the coil is first unrolled and cut into titanium plates of length L before annealing, where L is an integer multiple of the length of the final product; then the annealing operation is performed, and the annealing temperature T2 is 560°C to 660°C. After heating to a predetermined temperature, the temperature is kept constant for a holding time t=C×k4, where C is the total thickness of the plate and the press-straightened plate during annealing and press-straightening, in mm, and k4 is the insulation coefficient, with a value range of 0.8 to 40 min / mm; the oxide layer is removed after annealing.
[0030] Furthermore, in step S5, the thickness of the grinding area is not less than the thickness of the finished product.
[0031] Compared with the prior art, the pure titanium plate roll preparation method of the present invention has the following advantages:
[0032] 1. Through slab preparation, coil hot rolling, organization control, plate size control, and surface treatment, high-quality pure titanium plates with good surface quality, comprehensive performance, and good organization uniformity can be stably obtained, and the coil production of pure titanium plates with a thickness of 5mm to 8mm and a width of 800mm to 1500mm can be achieved. The performance meets the relevant technical requirements of GB / T 3620 and GB / T 3621, with uniform organization, grain size ≥6, and good surface quality.
[0033] 2. The process design is carried out by two smelting methods: EB smelting to prepare flat ingots or VAR smelting + forging to prepare flat ingots. It is convenient to select the processing route according to product needs and the capacity of titanium processing equipment. EB smelting to prepare flat ingots has low energy consumption, short production process and saves 3 to 5 days of processing time. VAR smelting equipment has low investment and large number of equipment, making the preparation method more widely applicable.
[0034] 3. By setting TA1 grade titanium raw material, limiting the impurity content, and adjusting the annealing temperature, the purpose of shortening the processing time of the annealing process and improving the processing efficiency is achieved. Compared with the traditional single-sheet hot rolling process, the present invention improves production efficiency and product quality, and reduces production costs by about 10 yuan / kg, which is of great significance to the field of pure titanium plate production.
[0035] 4. Through the process design of the size of titanium ingot forging titanium ingot, the total deformation of the ingot during the forging process is avoided to be too large, more heat is generated during the forging process, and small cracks are generated inside the ingot, which affects the mechanical properties and product quality of the titanium ingot. DETAILED DESCRIPTION
[0038] In order to make the technical means, objectives and effects of the present invention easy to understand, the embodiments of the present invention are described in detail below.
[0039] It should be noted that all the terms used in the present invention to indicate directionality and position, such as "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "inside", "outside", "top", "lower", "lateral", "longitudinal", "center", etc., are only used to explain the relative positional relationship and connection status between the components in a certain state, and are only for the convenience of describing the present invention, rather than requiring the present invention to be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features.
[0040] In the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0041] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0042] The invention discloses a method for preparing a pure titanium pole plate in a rolled form, comprising the following steps:
[0043] S1: TA1 grade titanium is used as raw material, and EB smelting or VAR smelting + forging is used to prepare flat ingots, and the flat ingots are peeled after preparation;
[0044] S2: coil hot rolling; determine the hot rolling target thickness according to the annealing process, and roll the prepared flat ingot slab to the target thickness through rough rolling and finish rolling;
[0045] S3: Annealing treatment; when the coil is subjected to continuous annealing after hot rolling, the annealing temperature T1 is 765℃~870℃, the continuous annealing coil speed is V, and the oxide layer is removed by shot blasting + pickling process; when the coil is subjected to annealing press straightening after hot rolling, the annealing temperature T2 is 540℃~680℃, the holding time is t, and the oxide layer is removed after annealing;
[0046] S4: Cutting: cutting the annealed and press-corrected titanium plate or hot-rolled white titanium coil to the finished product size;
[0047] S5: Surface treatment: Grind the local defects on the plate surface, and then sandblast the ground plate;
[0048] S6: Cold straightening treatment is performed on the plates with large unevenness;
[0049] S7: pickling treatment.
[0050] The method for preparing a pure titanium pole plate in a coiled form is designed for two smelting methods, namely, preparing a flat ingot by EB smelting or preparing a flat ingot by VAR smelting + forging, so that the processing route can be selected according to product requirements and the capacity of titanium material processing equipment. The flat ingot prepared by EB smelting has low energy consumption, short production process and saves 3 to 5 days of processing time. The VAR smelting equipment has low investment and a large number of equipment. High-quality pure titanium pole plates with good surface quality, comprehensive performance and good uniformity of organization can be stably obtained through slab preparation, coiled hot rolling, organization control, plate size control and surface treatment, so that the coiled production of pure titanium pole plates with a thickness of 5 mm to 8 mm and a width of 800 mm to 1500 mm can be realized. The performance meets the relevant technical requirements of GB / T 3620 and GB / T 3621, the organization is uniform, the grain size is ≥6 levels and the surface quality is good. By setting a TA1 grade titanium raw material, limiting the impurity content and adjusting the annealing temperature, the processing time of the annealing process is shortened and the processing efficiency is improved.
[0051] Specifically, the final geometric accuracy of the pure titanium plate is: 5mm~8mm thickness, surface roughness Ra≥1.5μm, grain size difference in the same batch ≤0.5 level, and plate unevenness ≤3mm / m.
[0052] Specifically, in step S1, the chemical composition of titanium meets the requirements of GBT 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions" TA1 standard, and the impurity element content is: C≤0.03%, 0.02%≤O≤0.06%, N≤0.03%, H≤0.015%, Fe≤0.05%. The setting of the impurity element content range of titanium raw materials reduces the deviation of the impurity elements on the titanium phase transition temperature and the change of the phase transition dynamics, and at the same time avoids the impurity elements from hindering or promoting the growth of grains during annealing, resulting in uneven grain size distribution or abnormal grain boundary structure, thereby affecting the mechanical properties and processing properties of titanium plates; within this range, the annealing processing time of titanium plates is shorter than that of general raw materials, the annealing temperature is high, and the grain size can reach 6 to 9 levels, and the same roll difference is about 0.5 levels, which effectively improves production efficiency and product quality and meets the needs of mass production of titanium plates.
[0053] Specifically, in step S1, the thickness range of the prepared slab is 160-260 mm, and the thickness range of the single-sided peeling treatment after the slab is prepared is 3-10 mm. The setting of the slab range makes the titanium slab ingot have greater flexibility in subsequent processing, can be cut, forged or rolled, and meet various process requirements, so that the producer can flexibly adjust the product specifications according to market demand. The appropriate thickness helps to control its internal grain structure and phase composition, maintain good thermal conductivity and uniform temperature distribution during hot rolling or forging, and help to obtain titanium materials with excellent strength, ductility and corrosion resistance, reduce energy consumption in the production process, and improve production efficiency; at the same time, due to the large volume of titanium slabs, the influence of external factors during the production process is relatively small, which is conducive to maintaining the consistency and stability of product quality; through peeling treatment, the oxide layer on the surface of the titanium slab can be removed, which significantly improves the surface quality of the titanium slab, and also makes the surface of the titanium slab smoother, which is conducive to subsequent rolling and cutting operations, reduces production difficulty, and improves production efficiency.
[0054] Preferably, the thickness of the prepared slab ranges from 180 to 240 mm.
[0055] Specifically, in step S1, when EB smelting is used, no more than 50% of recycled materials can be added, and the recycled materials are fully mixed with sponge titanium particles before smelting and smelted once. This setting uses EB smelting to save 3 to 5 days of electrode pressing, secondary smelting and other processes, and improves the manufacturing efficiency of titanium ingots. At the same time, EB smelting can use recycled materials for smelting processing. Since the price of recycled materials is about 30% to 50% of the price of sponge titanium, based on this calculation, EB smelting can save 15% to 25% of the cost, significantly reducing the processing and production cost of titanium plates.
[0056] Specifically, in step S1, when VAR smelting is adopted, smelting is performed twice, and the ingot size is: H×W×L2,
[0057] Where: H = X × k1
[0058] W=X×k2
[0059] L2=L1×k3
[0060] Where X is the diameter of the VAR smelting ingot, L1 is the length of the VAR smelting ingot; H is the thickness of the flat ingot after forging; W is the width of the flat ingot after forging; L2 is the length of the flat ingot after forging; k1 is a coefficient of 0.15 to 0.25; k2 is a coefficient of 1.0 to 1.7; k3 is a coefficient of 2.6 to 3.2. This setting is used to design the size of the titanium ingot forging titanium flat ingot, to avoid excessive total deformation of the ingot during forging, to generate more heat during forging, to generate fine cracks inside the flat ingot, and to affect the mechanical properties and product quality of the titanium flat ingot.
[0061] Specifically, in step S2, the target thickness of the titanium electrode plate is htotal, the finished product thickness is h, the reserved thickness is hwork, and htotal=h+hwork;
[0062] During continuous annealing after hot rolling, h range: 0.05~0.2mm;
[0063] When hot rolling is not subjected to continuous annealing, the h process range is 0.1 to 0.3 mm. This setting designs different process margins according to different process flows, so that the preparation method of titanium plates can adapt to the actual equipment processing capacity, which helps to improve the processing quality of products, reduce the scrap rate, control the production process size, and improve the consistency of batch products.
[0064] Specifically, in step S3, during continuous annealing, the annealing temperature T1 is 780℃~850℃, the coiling speed V is in the range of 0.5m / min~20m / min, and the oxide layer is removed by shot blasting + pickling process after annealing. The coiling speed V setting greatly improves the processing speed of the equipment annealing titanium plate, shortens the annealing time, ensures that the product quality meets the process requirements, improves the production rate, and helps to further reduce the production cost.
[0065] Preferably, during continuous annealing, the annealing temperature T1 is 820° C. or 840° C.
[0066] Preferably, the range of the winding speed V is 8 m / min to 15 m / min. This configuration further increases the winding speed V, which helps to further increase the production rate and reduce the production cost.
[0067] Specifically, the continuous processing system of pure titanium strip includes an uncoiler, a clamping straightener, a plasma welder, an inlet looper, an annealing furnace, a drying device, a shot blasting machine, a pickling device, an outlet looper and a coiler which are arranged in sequence.
[0068] Specifically, in step S3, during annealing and press-straightening, the coil is first unrolled and slit before annealing, and the coil is cut into titanium plates of length L according to the equipment capacity, where L is an integer multiple of the length of the final product; then the annealing operation is performed, and the annealing temperature T2 is 560°C to 660°C. After heating to a predetermined temperature, the temperature is kept constant for a holding time of t=C×k4, where C is the total thickness of the plate and the press-straightened plate during annealing and press-straightening, in mm, and k4 is the insulation coefficient, ranging from 0.8 to 40 min / mm; the oxide layer is removed after annealing. This setting unwinds and cuts the hot-rolled coil, which is convenient for subsequent processing and production. The integer multiple cutting reduces the generation of scraps, helps to reduce production costs and improve production efficiency; the holding time t is determined according to the thickness of the annealing and press-straightening plate, which improves the adaptability of the process and avoids the influence of annealing quality due to the difference in plate thickness; the unevenness of the finished plate using the annealing and press-straightening process is better than that of continuous annealing. In mass production, the proportion of plates that need cold straightening treatment is 30%-50% less than that of plates using the continuous annealing process.
[0069] Preferably, the value range of k4 is 1.1 to 1.8 min / mm. This setting greatly shortens the holding time during annealing and press straightening, improves the processing efficiency of the annealing process, and better meets the needs of actual production.
[0070] Preferably, during annealing and press straightening, the oxide layer is removed by shot blasting / sand blasting + pickling process. This setting can effectively remove rust, oxide scale and oil stains on the surface of the titanium plate, improve the surface finish and appearance quality, make the plate surface have better adhesion, and facilitate subsequent processing.
[0071] Specifically, in step S5, the thickness of the grinding part is not less than the thickness of the finished product. This setting limits the grinding range of the titanium plate, avoids the grinding size being too large, which makes the local size of the titanium plate too small, and the local strength of the plate decreases, affecting its overall structural stability, and avoids the reduction of conductivity and corrosion resistance due to too thin thickness, which helps to improve the quality of the titanium plate and meet the use requirements.
[0072] Example 1
[0073] VAR smelting + forging to prepare flat ingots by annealing and pressing
[0074] S1: The chemical composition must meet the requirements of GBT 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions" TA1 standard, and the impurity elements must further meet the composition range in Table 2;
[0075] Table 2
[0076] C O N H Fe 0.01-0.02 0.03-0.06 0.08-0.1 <0.005 0.02-0.04
[0077] After the VAR double smelting round ingot is peeled, the diameter is 1100mm and the length is 2400mm. The round ingot is forged to obtain a flat ingot slab with a size of 210×1573×6930mm H×W×L2. The single side is peeled 3mm to obtain a hot-rolled slab;
[0078] S2: hot rolled to 6.2 mm thick, unannealed black skin hot rolled coil;
[0079] S3: The hot-rolled black coil is unrolled and cut into 10 times the length of the finished product; the cut titanium plate is subjected to atmospheric annealing and press-correction, the annealing temperature T2 is 600-650°C, and the holding time t=11min; the titanium plate after atmospheric annealing and press-correction is subjected to shot blasting / sand blasting + pickling to remove the surface oxide scale;
[0080] S4: Slitting to finished product size;
[0081] S5: Grind the local defects on the plate surface and perform sandblasting after grinding;
[0082] S6: Cold straightening treatment is performed on the plates with large unevenness;
[0083] S7: The plate is pickled to obtain a pure titanium plate with a thickness of 6.0-6.1 mm, a surface roughness of Ra ≥ 1.8 μm, a grain size difference of ≤ 0.5 in the same batch, and a plate unevenness of ≤ 2.8 mm / m. The finished product performance is shown in Table 3.
[0084] Table 3
[0085]
[0086] Example 2
[0087] EB smelting is prepared by continuous annealing
[0088] S1: The chemical composition must meet the requirements of GBT 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions" TA1 standard, and the impurity elements must further meet the composition range in Table 4;
[0089] Table 4
[0090] C O N H Fe 0.01-0.02 0.03-0.06 0.08-0.1 <0.005 0.02-0.04
[0091] EB smelting, peeling 10mm, to produce 220mm thick slab;
[0092] S2: hot rolled to 6.1 mm thick;
[0093] S3: After hot rolling, the coil is subjected to continuous annealing, the annealing temperature T1 is 780℃~850℃, the continuous annealing coil speed is 15m / min, the annealing time is about 15min, and the oxide layer is removed by online shot blasting + pickling process;
[0094] S4: unwinding and slitting into finished product size;
[0095] S5: Grind the local defects on the plate surface and perform sandblasting after grinding;
[0096] S6: Cold straightening treatment is performed on the plates with large unevenness;
[0097] S7: The plate is pickled to obtain a pure titanium plate with a thickness of 5.9-6.0 mm, a surface roughness of Ra ≥ 1.5 μm, a grain size difference of ≤ 0.5 levels in the same batch, and a plate unevenness of ≤ 3 mm / m. The finished product performance is shown in Table 5.
[0098] Table 5
[0099]
[0100] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a pure titanium plate in a rolled form, It is characterized in that The following steps are involved: S1: TA1 grade titanium is used as raw material, and EB smelting or VAR smelting + forging is used to prepare flat ingots, and the flat ingots are peeled after preparation; S2: coil hot rolling; determine the hot rolling target thickness according to the annealing process, and roll the prepared flat ingot slab to the target thickness through rough rolling and finish rolling; S3: Annealing treatment; when the coil is subjected to continuous annealing after hot rolling, the annealing temperature T1 is 765℃~870℃, the continuous annealing coil speed is V, and the oxide layer is removed by shot blasting + pickling process; when the coil is subjected to annealing press straightening after hot rolling, the annealing temperature T2 is 540℃~680℃, the holding time is t, and the oxide layer is removed after annealing; S4: Cutting: cutting the annealed and press-corrected titanium plate or hot-rolled white titanium coil to the finished product size; S5: Surface treatment: Grind the local defects on the plate surface, and then sandblast the ground plate; S6: Cold straightening treatment is performed on the plates with large unevenness; S7: pickling treatment.
2. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S1, the chemical composition of titanium meets the requirements of GBT 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions" TA1 standard, and the impurity element content is: C≤0.03%, 0.02%≤O≤0.06%, N≤0.03%, H≤0.015%, Fe≤0.05%.
3. The method for preparing a pure titanium pole plate in a rolled form according to claim 2, It is characterized in that In step S1, the thickness of the prepared slabs ranges from 160 to 260 mm, and the thickness of the slabs to be peeled on one side ranges from 3 to 10 mm.
4. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S1, when EB smelting is adopted, no more than 50% of recycled materials can be added, and the recycled materials are fully mixed with the titanium sponge particles before smelting and smelted once.
5. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S1, when VAR smelting is used, smelting is performed twice, and the ingot size is: H×W×L 2 , Where: H = X × k 1 W=X×k 2 L 2 =L1×k 3 Where X is the diameter of the VAR smelting ingot, L 1 is the length of the VAR smelting round ingot; H is the thickness of the flat ingot after forging; W is the width of the flat ingot after forging; L 2 k is the length of the flat ingot after forging; 1 The coefficient is 0.15~0.25; k 2 The coefficient is 1.0~1.7; k 3 The coefficient is 2.6 to 3.
2.
6. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S2, the target plate thickness is h 总 , the finished product thickness is h, and the reserved thickness is h 工 ,h 总 =h+h 工 ; During continuous annealing after hot rolling, h 工 Range: 0.05~0.2mm; After hot rolling without continuous annealing, h 工 Range: 0.1~0.3mm.
7. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S3, during continuous annealing, the annealing temperature T1 is 780°C to 850°C, the coiling speed V is in the range of 0.5m / min to 20m / min, and the oxide layer is removed by shot blasting + pickling process after annealing.
8. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S3, during annealing and press-straightening, the coil is first unrolled and cut into titanium plates of length L before annealing, where L is an integer multiple of the length of the final product; then the annealing operation is performed, and the annealing temperature T2 is 560°C to 660°C. After heating to a predetermined temperature, the temperature is kept constant for a time t=C×k4, where C is the total thickness of the plate and the press-straightened plate during annealing and press-straightening, in mm, and k4 is the insulation coefficient, with a value range of 0.8 to 40 min / mm; the oxide layer is removed after annealing.
9. The method for preparing a pure titanium pole plate in a rolled form according to claim 1, It is characterized in that In step S5, the thickness of the grinding area is not less than the thickness of the finished product.
Citation Information
Patent Citations
Method for producing titanium slabs efficiently
CN102776390A
Continuous annealing method of pure titanium roll
CN104060205A
Preparation method of titanium plate for deep drawing
CN107723638A
Production machining method for pure titanium large-specification plate
CN108356088A
Forging method for improving yield of large-specification titanium slabs
CN113751637A