Manufacturing method of hollow steel for rock drilling rod
Through the precise hollow steel manufacturing process, the strength and wear resistance requirements of rock drilling rods in complex environments are solved, the quality and safety of drilling rods are improved, maintenance costs and accident rates are reduced, and service life is extended.
Patent Information
- Application Number
- CN202411014006.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing hollow steel manufacturing technology is difficult to meet the high strength, wear resistance and safety requirements of rock drill rods in complex construction environments, and there are problems of unstable quality and high maintenance costs.
Adopting advanced materials and precision manufacturing processes, including material preparation, heating treatment, perforation and rolling, cooling and finishing, softening and annealing and cold rolling, etc., ensure the mechanical properties of hollow steel and Dimensional accuracy, combined with roughing, finishing and heat treatment, forms a high-quality rock drill rod.
The high strength, high toughness and wear resistance of hollow steel are achieved, the overall quality and performance of the drill rod are improved, the accident rate and maintenance cost are reduced, the service life is extended, and the operation efficiency is improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hollow steel manufacturing, in particular to a method for manufacturing hollow steel for rock drilling rods. Background Art
[0002] With the rapid development of modern mining, tunneling, railway and highway construction and other engineering fields, rock drilling equipment is a key tool in these projects, and its performance and quality directly affect the efficiency and safety of the projects. As an important part of rock drilling equipment, the quality of drill rods is particularly concerned, and hollow steel is the main material for producing drill rods. The quality of its manufacturing technology directly affects the performance and cost of the drill rod. Therefore, it is of great significance to study and improve the manufacturing method of hollow steel for rock drilling drill rods. The present application now proposes a manufacturing method of hollow steel for rock drilling drill rods. Summary of the invention
[0003] Technical Solution
[0004] To achieve the above object, the present invention provides the following technical solution: a method for manufacturing hollow steel for rock drilling rod, comprising the following steps:
[0005] S1. Material preparation: select the tube blank and process the surface of the tube blank;
[0006] S2, heating treatment: prepare heating equipment to heat the tube blank;
[0007] S3, piercing and rolling: piercing the tube blank, and then rolling the tube blank into hollow steel;
[0008] S4, cooling and finishing: the rolled hollow steel rough pipe is cooled and finished;
[0009] S5, Softening annealing: Softening annealing of the capillary tube with heat preservation;
[0010] S6, cold rolling: cold rolling the rough tube using a two-roller cold rolling unit;
[0011] S7, repeating steps S5 and S6 until a hollow steel seamless tube is formed, and the hollow steel seamless tube is used as a rock drilling rod.
[0012] Preferably, the material preparation includes tube blank selection and surface preparation, wherein:
[0013] Tube blank selection: Select tube blank materials suitable for producing hollow steel, which usually have good machinability and mechanical properties;
[0014] Surface preparation: Grind or peel the surface of the tube to ensure that the surface is smooth and free of impurities and oxide scale.
[0015] Preferably, the heating process comprises a heating device and temperature control, wherein:
[0016] Heating equipment: The tube blank is heated by a walking beam heating furnace. This method can realize the automatic control of the heating process, reduce energy consumption, and reduce environmental pollution;
[0017] Temperature control: Accurately control the heating temperature to ensure that the tube reaches the appropriate plastic deformation temperature range, while avoiding excessive temperature that causes material oxidation and decarburization.
[0018] Preferably, during the perforation and rolling:
[0019] Punching: Use a two-roller oblique piercing machine to perform the piercing operation and increase the piercing length to meet the requirements of hollow steel piercing specifications and length;
[0020] Preferably, the cooling and finishing:
[0021] Cooling: The rolled hollow steel is cooled on a cooling bed to ensure that the product reaches the appropriate hardness and mechanical properties;
[0022] Finishing: Cutting, grinding and other finishing processes are performed on the cooled hollow steel to meet the user's requirements for product size and appearance quality.
[0023] Preferably, the softening annealing comprises a heating stage, a heat preservation stage and a cooling stage.
[0024] Preferably, the cold rolling comprises the following steps:
[0025] S601, oblique rolling and piercing: a thick-walled rough tube is obtained by oblique rolling and piercing process;
[0026] S602, cold drawing or cold rolling: cold drawing or cold rolling the thick-walled rough tube obtained by oblique rolling and piercing to reduce its diameter and increase its length;
[0027] S603, Dimension control: During the cold rolling process, the gap between the rollers and the rolling force are precisely controlled to ensure the dimensional accuracy and surface quality of the hollow steel;
[0028] S604, quality inspection: perform quality inspection on the hollow steel after cold rolling.
[0029] Preferably, the preparation of the hollow steel into a rock drilling rod comprises rough processing, fine processing and heat treatment, wherein:
[0030] Rough processing: According to the design requirements, the raw materials are cut, polished and processed to make them have the initial shape and size of the drill rod;
[0031] Finishing: On the basis of rough machining, finishing processing is carried out, including turning, milling, drilling and other processes to ensure the dimensional accuracy and surface quality of the drill rod;
[0032] Heat treatment: The processed drill rod is heat treated, including quenching, tempering and other processes, to improve its hardness and wear resistance.
[0033] Compared with the prior art, the present invention provides a method for manufacturing hollow steel for rock drilling rods, which has the following beneficial effects:
[0034] 1. The manufacturing method of hollow steel for rock drilling rod adopts advanced materials and precise manufacturing process to ensure that the hollow steel has excellent mechanical properties, such as high strength, high toughness and wear resistance. These characteristics enable the rock drilling rod to better cope with various complex construction environments and engineering requirements. By strictly controlling key process steps such as heating, perforation and rolling, the geometric shape of the hollow steel is regular, the dimensional accuracy is high, and the core hole is round, which further improves the overall quality and performance of the drill rod.
[0035] 2. The manufacturing method of hollow steel for rock drilling rods and the strict quality inspection system ensure that the various performance indicators of the hollow steel meet the design requirements and relevant standards, thereby improving the reliability and safety of the product. The excellent corrosion resistance and wear resistance of the hollow steel enable the drill rod to operate stably for a long time in harsh construction environments, reducing the accident rate.
[0036] 3. The manufacturing method of the hollow steel for the rock drilling rod. The excellent mechanical properties and wear resistance of the hollow steel reduce the wear rate and failure rate of the drill rod, reduce the frequency of repair and replacement, and thus reduce the maintenance cost. At the same time, the design of the hollow steel reduces the weight of the drill rod while maintaining sufficient strength, which is convenient for operation and transportation, and further improves the use efficiency and life. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Embodiment 1:
[0039] A method for manufacturing hollow steel for rock drilling rods, characterized in that it comprises the following steps:
[0040] S1. Material preparation: select the tube blank and process the surface of the tube blank;
[0041] S2, heating treatment: prepare heating equipment to heat the tube blank;
[0042] S3, piercing and rolling: piercing the tube blank, and then rolling the tube blank into hollow steel;
[0043] S4, cooling and finishing: the hollow steel after rolling is cooled and finished;
[0044] S5. Quality control: Use measuring devices to inspect the dimensions of hollow steel;
[0045] S6. Process optimization and improvement: adjust various parameters in production according to actual needs;
[0046] S7. Preparing the hollow steel into a rock drilling rod: processing the hollow steel into a rock drilling rod.
[0047] Embodiment 2:
[0048] According to a method for manufacturing hollow steel for rock drilling rods proposed in Example 1, material preparation includes tube blank selection and surface preparation, wherein:
[0049] Tube blank selection: Select tube blank materials suitable for producing hollow steel, which usually have good machinability and mechanical properties;
[0050] Surface preparation: Grind or peel the surface of the tube to ensure that the surface is smooth and free of impurities and oxide scale.
[0051] Embodiment three:
[0052] According to a method for manufacturing hollow steel for rock drilling rods proposed in embodiment 1, the heating treatment includes heating equipment and temperature control, wherein:
[0053] Heating equipment: The tube blank is heated by a walking beam heating furnace. This method can realize the automatic control of the heating process, reduce energy consumption, and reduce environmental pollution;
[0054] Temperature control: Accurately control the heating temperature to ensure that the tube reaches the appropriate plastic deformation temperature range, while avoiding excessive temperature that causes material oxidation and decarburization.
[0055] Embodiment 4:
[0056] According to a method for manufacturing hollow steel for rock drilling rods proposed in Example 1, during the punching and rolling:
[0057] Punching: Use a two-roller oblique piercing machine to perform the piercing operation and increase the piercing length to meet the requirements of hollow steel piercing specifications and length;
[0058] Rolling: Multiple rolling is carried out on a six-roll hot rolling forming machine. Through the steps of rough rolling, intermediate rolling and finishing rolling, the perforated tube billet is gradually rolled into a hollow steel product.
[0059] Embodiment five:
[0060] A method for manufacturing hollow steel for rock drilling rods, including quality control including size detection and performance testing, wherein:
[0061] Dimension inspection: Use appropriate measuring tools and equipment to inspect the dimensions of hollow steel to ensure that the product meets relevant standards and specifications;
[0062] Performance testing: Conduct mechanical performance tests on hollow steel, including tensile strength, yield strength, and elongation, to ensure that the product has good mechanical properties and service life.
[0063] Embodiment six:
[0064] A method for manufacturing hollow steel for rock drilling rods, including process optimization and improvement, process parameter adjustment, equipment upgrade and transformation, wherein:
[0065] Process parameter adjustment: According to the actual production situation and product performance requirements, the heating temperature, piercing speed, rolling pressure and other process parameters are adjusted and optimized to improve production efficiency and product quality.
[0066] Equipment upgrade and transformation: With the continuous development of technology and changes in market demand, production equipment is upgraded and transformed to improve the degree of automation and production capacity of the equipment.
[0067] Embodiment seven:
[0068] According to a method for manufacturing hollow steel for a rock drilling rod proposed in Example 1, the preparation of the hollow steel into a rock drilling rod includes rough processing, fine processing and heat treatment, wherein:
[0069] Rough processing: According to the design requirements, the raw materials are cut, polished and processed to make them have the initial shape and size of the drill rod;
[0070] Finishing: On the basis of rough machining, finishing processing is carried out, including turning, milling, drilling and other processes to ensure the dimensional accuracy and surface quality of the drill rod;
[0071] Heat treatment: The processed drill rod is heat treated, including quenching, tempering and other processes, to improve its hardness and wear resistance.
[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for manufacturing hollow steel for rock drilling rods, characterized in that: The following steps are involved: S1. Material preparation: select the tube blank and process the surface of the tube blank; S2, heating treatment: prepare heating equipment to heat the tube blank; S3, piercing and rolling: piercing the tube blank, and then rolling the tube blank into hollow steel; S4, cooling and finishing: the rolled hollow steel rough pipe is cooled and finished; S5, Softening annealing: Softening annealing of the capillary tube with heat preservation; S6, cold rolling: cold rolling the rough tube using a two-roller cold rolling unit; S7, repeating steps S5 and S6 until a hollow steel seamless tube is formed, and the hollow steel seamless tube is used as a rock drilling rod.
2. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The material preparation includes tube blank selection and surface preparation, wherein: Tube blank selection: Select tube blank materials suitable for producing hollow steel, which usually have good machinability and mechanical properties; Surface preparation: Grind or peel the surface of the tube to ensure that the surface is smooth and free of impurities and oxide scale.
3. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The heating process includes heating equipment and temperature control, wherein: Heating equipment: The tube blank is heated by a walking beam heating furnace. This method can realize the automatic control of the heating process, reduce energy consumption, and reduce environmental pollution; Temperature control: Accurately control the heating temperature to ensure that the tube reaches the appropriate plastic deformation temperature range, while avoiding excessive temperature that causes material oxidation and decarburization.
4. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: In the perforation and rolling: Punching: Use a two-roller oblique piercing machine to perform the piercing operation and increase the piercing length to meet the requirements of hollow steel piercing specifications and length; Rolling: Multiple rolling is carried out on a six-roll hot rolling forming machine. Through the steps of rough rolling, intermediate rolling and finishing rolling, the perforated tube billet is gradually rolled into a hollow steel product.
5. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The cooling and finishing: Cooling: The rolled hollow steel is cooled on a cooling bed to ensure that the product reaches the appropriate hardness and mechanical properties; Finishing: Cutting, grinding and other finishing processes are performed on the cooled hollow steel to meet the user's requirements for product size and appearance quality.
6. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The soft annealing includes a heating stage, a heat preservation stage and a cooling stage.
7. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The cold rolling comprises the following steps: S601, oblique rolling and piercing: a thick-walled rough tube is obtained by oblique rolling and piercing process; S602, cold drawing or cold rolling: cold drawing or cold rolling the thick-walled rough tube obtained by oblique rolling and piercing to reduce its diameter and increase its length; S603, Dimension control: During the cold rolling process, the gap between the rollers and the rolling force are precisely controlled to ensure the dimensional accuracy and surface quality of the hollow steel; S604, quality inspection: perform quality inspection on the hollow steel after cold rolling.
8. The method for manufacturing a hollow steel for a rock drilling rod according to claim 1, characterized in that: The preparation of the hollow steel into a rock drilling rod includes rough processing, fine processing and heat treatment, wherein: Rough processing: According to the design requirements, the raw materials are cut, polished and processed to make them have the initial shape and size of the drill rod; Finishing: On the basis of rough machining, finishing processing is carried out, including turning, milling, drilling and other processes to ensure the dimensional accuracy and surface quality of the drill rod; Heat treatment: The processed drill rod is heat treated, including quenching, tempering and other processes, to improve its hardness and wear resistance.
Citation Information
Patent Citations
Method for manufacturing high-hardness cold-drawn steel tube
CN104338781A
Hot-piercing and hot rolling process for production of hollow steel
CN1097153A
Hot rolling method of hollow steel for drill rod, hollow steel and hot rolling mill
CN114558891A
Hot-rolling perforation-cold-rolling forming method for hollow rock-drill steel
CN1411921A
Production of seamless steel tube having low hardness and high toughness
JP1992021721A
Cited By