Micro part manufacturing method based on additive and subtractive materials and micro part
In the manufacturing of fine parts, the continuous melting duct base is printed with high-energy-density laser, and the continuous melting duct is printed with low-energy-density laser, and combined with online detection and heat treatment, the melting pool discontinuity and difficulty in using support are solved. Problem, high-precision and low-cost micro-part manufacturing is achieved.
Patent Information
- Application Number
- CN202410839368.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-26
AI Technical Summary
In the prior art, when manufacturing fine parts, low energy density lasers lead to small and discontinuous melt pool width, resulting in poor surface quality and low dimensional accuracy of parts, and the large amount of support parts use increases operational difficulties and high costs, and the cost of existing improved devices. High, low efficiency.
The continuous melting duct base is printed with a high energy density first molding laser, and the continuous melting duct on the base is printed with a low energy density second molding laser, and the stability of the melt pool is adjusted using arc, and combined with a high-speed camera and infrared thermal imaging camera. Carry out online inspection and control, reduce or eliminate support, use continuous and pulsed lasers for heat treatment and surface trimming.
High-precision molding of fine parts is achieved, the minimum limit size of the parts is reduced, the cost is reduced, the production efficiency and the continuity and stability of the parts are improved, and the difficulty in using the support is avoided.
Smart Images

Figure CN118926542A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive and subtractive materials, and in particular to a micro-part manufacturing method based on additive and subtractive materials and a micro-part. Background Art
[0002] Multi-laser hybrid manufacturing based on laser powder bed fusion (LPBF) technology is an intelligent manufacturing method that combines laser additive manufacturing and pulsed laser processing. Compared with LPBF technology, multi-laser hybrid manufacturing can process the internal structure and surface of unclosed parts, form more complex internal structures, and obtain better surface quality and organizational properties.
[0003] "Micro-parts" refer to parts whose corresponding structures have a thickness extension of as low as 10μm to 500μm in at least one spatial direction. At present, the process of additive manufacturing of "micro-parts", such as "thin-wall" structures, is to stack single melt channels at the forming position of the parts. To obtain a single melt channel with a smaller molten pool width, the energy density of the melting forming laser must be reduced to obtain finer and finer parts. However, the laser with lower energy density will cause the powder to not melt, resulting in a large amount of powder sticking to the surface of the melt channel. The molten pool will spheroidize under the action of the surface tension of the metal solution, making the surface of the single channel discontinuous or even intermittent (such as Figure 1 As shown in the figure, continuous thermal stress cycles will cause excessive thermal stress in the melt channel and cause cracks.
[0004] The first layer of single melt channel is formed on the flat substrate plate, and the forming quality of the first single melt channel is poor. The single melt channel will affect the wettability of the molten pool of the next layer of stacked melt channels and thus affect its forming quality, ultimately affecting the surface and side quality, density, and dimensional accuracy of the manufactured "thin-walled" structure, causing deformation and cracking of parts, or even failure to form. In the prior art, a large number of supports are still used in the manufacture of thin-walled structures, but the removal of supports and the main body will increase the difficulty of operation. Therefore, it is necessary to combine the molten pool of laser-melted metal with in-situ online detection technology, subtractive laser processing, and laser heat treatment to improve the quality of additive manufacturing fine parts, reduce or even eliminate the use of a large number of supports, reduce the minimum limit size of formed parts, and manufacture more fine and delicate parts.
[0005] In this regard, a Chinese patent (CN107685149B) discloses a method and device for improving the forming quality of thin-walled parts manufactured by laser additive manufacturing. Although the device can make the laser deposition molten pool always solidify and form in a double-piece ceramic block, it can break through the accuracy limit of the molten pool limit size on the size of the formed thin-walled parts and improve the surface quality of the thin-walled parts. However, the device changes the forming shape of the metal molten pool through mechanical structure restrictions, and does not actually change the fluidity and stability of the solution in a single molten pool. Severe adhesion may occur between the ceramic sheet and the metal molten pool, and the accuracy of the double-piece ceramic sheet of the auxiliary forming system is difficult to meet the requirements of fine processing of thin-walled parts. The cost of constructing new equipment is high, and the strategy of adjusting the mechanical gripper and ceramic sheet at each layer greatly affects the printing efficiency, making it difficult to apply in actual engineering.
[0006] A Chinese patent (CN114799229A) discloses a powder-spreading multi-laser additive and subtractive composite precision manufacturing device and its processing method. The device uses multiple continuous lasers for laser subtraction and uses visual inspection of industrial cameras to detect defects and roughness, thereby reducing the possibility of internal defects in parts. However, the patent does not provide more detailed forming strategies and methods for the manufacturing process.
[0007] The Chinese patent (CN116745050A) discloses that a discontinuous support or support structure for supporting a thin-walled structure is established on a build plate or platform in an additive manner, and a discontinuous molten pool is generated in the powder bed to promote the additive construction of thin-walled structures in particular. However, the patent has a large number of support members, which will inevitably reduce production efficiency, and it is also difficult to remove the support members. Furthermore, this method does not reduce the limit forming size of thin-walled parts from the perspective of thin-wall forming, reduce defects, and improve the forming quality of thin-walled parts. Summary of the invention
[0008] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a method for manufacturing micro-parts based on additive and subtractive materials. The method can form a continuous melt path with a low energy density laser, which is conducive to forming micro-parts with high molding precision and has the advantages of easy operation and low cost.
[0009] The object of the present invention is to provide a method for using a method for manufacturing micro-parts based on additive and subtractive materials.
[0010] To achieve the above object, the present invention provides the following technical solutions:
[0011] A method for manufacturing micro-parts based on additive and subtractive materials is provided, comprising the following steps:
[0012] A first forming laser is used to print and form a first single melt path on the current layer to obtain a base with a curved surface;
[0013] A second single melt track is printed and formed on the base by using a second forming laser, so that the second single melt track is continuously formed on the base, and the structure formed by the second single melt track is the current layer of the part structure. The second forming laser is continuously used to form another single melt track on the second single melt track until the target fine part is obtained.
[0014] The linear energy density of the second shaping laser is lower than the linear energy density of the first shaping laser.
[0015] The linear energy density calculation formula is as follows:
[0016] El=p / v
[0017] E l —Linear energy density
[0018] p—laser power
[0019] v—Scanning speed.
[0020] In some embodiments, before forming the second single melt track, a recessed microstructure is first provided on the surface of the base, so that the second single melt track is formed on the recessed microstructure.
[0021] In some embodiments, the first shaping laser is a continuous laser, the linear energy density of the first shaping laser is greater than 0.2, and the second shaping laser is a continuous laser or a pulsed laser.
[0022] In some embodiments, when the linear energy density of the first forming laser is in the range of [0.2-0.5), the cross section of the base is spherical;
[0023] When the linear energy density of the first forming laser is [0.5-1.2), the cross section of the base is flat and sloped.
[0024] In some embodiments, the continuous laser power is 10 to 1000 W, the scanning speed is 50 to 7000 mm / s, and the spot diameter is 10 to 300 microns;
[0025] The pulse laser power ranges from 5 to 200 W, the scanning speed is from 50 to 5000 mm / s, the spot diameter is from 5 to 200 microns, and the frequency is from 20 to 5000 KHz.
[0026] In some embodiments, a high-speed camera and / or an infrared thermal imaging camera are used. The high-speed camera and / or the infrared imaging camera are connected to an online monitoring processor and a control module to form an in-situ detection device. The in-situ detection device detects the printing process and controls the laser parameters online.
[0027] In some embodiments, during the printing process, a continuous laser is used to perform laser remelting and / or laser heat treatment on the current layer, wherein the laser heat treatment eliminates thermal stress generated by additive manufacturing.
[0028] In some embodiments, during the printing process, a pulsed laser is used to perform laser processing, surface pulsed laser shock peening, or side laser cutting on the corresponding melt surface to trim the single-pass melt morphology and remove drill powder.
[0029] In some embodiments, before printing, the micro-part model file is first imported into the multi-laser additive and subtractive composite manufacturing equipment, and the required printing strategy is selected from the database according to the thickness of the micro-part.
[0030] In some embodiments, the database is established by:
[0031] High-speed cameras and infrared thermal imaging cameras are used to observe the state of the molten pool during printing. After printing, an electron microscope is used to observe the cross-sectional state of the melt path parts and record the corresponding laser parameters. The printing results and the corresponding laser parameters are stored in the database.
[0032] A micro-part is also provided, wherein the micro-part is manufactured by the above-mentioned micro-part manufacturing method based on additive and subtractive materials.
[0033] Beneficial effects of the micro-parts manufacturing method based on additive and subtractive materials of the present invention:
[0034] The method for manufacturing micro-parts based on additive and subtractive materials of the present invention first uses a high-energy-density first forming laser to form a first single melt on the current layer. Since the energy density of the first forming laser is high, the first single melt obtained is a continuous base with an arc surface. Based on this, a low-energy-density second forming laser is used to form a second single melt on the base for forming a thin-walled structure of micro-parts. Since the surface of the base formed by the first single melt has a certain curvature, the curvature can adjust the contact angle between the metal solution manufactured by the second forming laser and the base, so that the metal solution in the molten pool with a small width formed by the low-density energy second forming laser can also be continuously and evenly distributed on the base, overcoming the problem that the small width of the molten pool formed by the traditional low-density laser leads to poor continuity of the melt, thereby affecting the poor precision of the thin-walled structure of the formed parts. Subsequently, the single melts superimposed on the base all have an arc surface, and a continuous thin-walled structure can be formed directly using a low-energy-density laser. In addition, the present invention can form a thin-walled structure of micro-parts without a support, and has the advantages of easy operation and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic diagram of a small-sized molten pool width and a discontinuous single melt path obtained by a traditional linear energy density laser.
[0036] Figure 2 It is a first laser-printed base according to an embodiment of the present invention.
[0037] Figure 3 This is a diagram showing the effect of the second forming laser forming a second single melt path on a base according to an embodiment of the present invention.
[0038] Figure 4 It is a schematic diagram of machining a groove microstructure on a first single melt path according to an embodiment of the present invention.
[0039] Figure 5 It is a schematic diagram of processing a second single melt path on a groove microstructure according to an embodiment of the present invention.
[0040] Figure 6 It is a schematic diagram of processing a pit microstructure on a first single melting path according to an embodiment of the present invention.
[0041] Figure 7 It is a schematic diagram of processing a second single melt path on a pit microstructure according to an embodiment of the present invention.
[0042] Figure 8 It is a schematic diagram of a first laser-printed spherical base and printing a single channel of dot-shaped microcolumns on the spherical base according to an embodiment of the present invention.
[0043] Fig. 9 The cross-section of the corresponding spherical base is when the linear energy density of the first forming laser is in the range of [0.2 to 0.5);
[0044] Fig.10 The cross-section of the corresponding sloped base is when the linear energy density of the first forming laser is in the range of [0.5 to 1.2);
[0045] Fig.11 It is a schematic flow chart of a method for manufacturing micro-parts based on additive and subtractive materials according to an embodiment of the present invention.
[0046] Fig.12 It is an experimental diagram of a microcolumn embodiment of an embodiment of the present invention.
[0047] Reference numerals:
[0048] 1. First forming laser; 2. First single melting track; 3. Base; 4. Second forming laser; 5. Second single melting track; 6. Concave microstructure; 7. Spherical shape; 8. Flat slope shape; 9. Current layer. DETAILED DESCRIPTION
[0049] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0050] Example
[0051] The method for manufacturing micro-parts based on additive and subtractive materials disclosed in this embodiment is as follows: Fig.11 As shown, the following steps are included:
[0052] A first forming laser 1 is used to print and form a first single melt path 2 on the current layer 9 to obtain a base 3 with a curved surface;
[0053] Specifically, since the laser energy of the high linear energy density laser is large, the laser energy of the first molding laser 1 can ensure the continuity of the first single melt track 2 and enable the first single melt track 2 to form a curved structure on the current layer 9, which serves as a base 3 for printing and molding fine parts.
[0054] The second single melt path 5 is printed and formed on the base 3 by using the second forming laser 4, so that the second single melt path 5 is continuously formed on the base 3, and the structure formed by the second single melt path 5 is the current layer 9 of the part structure, wherein the linear energy density of the second forming laser 4 is lower than the linear energy density of the first forming laser 1, and the linear energy density calculation formula is as follows:
[0055] El=p / v
[0056] E l —Linear energy density
[0057] p—laser power
[0058] v—Scanning speed.
[0059] Specifically, since fine and delicate parts need to be formed by a single melt path with a smaller molten pool width, a low energy density laser is required. Based on this, a second forming laser 4 with a low linear energy density is used to form a single melt path with a smaller molten pool width on the base 3. At this time, although the linear energy density of the second forming laser 4 is low, the curvature of the surface of the base 3 can change the solid-liquid contact angle between the metal solution in the molten pool and the base 3, thereby improving the stability of the molten pool and avoiding problems such as disconnection in the molten pool, which is beneficial to improving the precision of the product.
[0060] After the current layer 9 (first layer) is prepared, the second forming laser 4 is used to form another single melting path (such as Fig.11The third single melt track shown is also made using low linear energy density) until the corresponding fine parts are obtained.
[0061] For example, Figure 2 As shown, the first forming laser 1 prints the base 3 formed into a strip, and the base 3 has a curvature. Figure 3 As shown, the second shaping laser 4 shapes a second single melt path 5 on the base 3 .
[0062] Furthermore, if Figure 8 As shown, the first forming laser 1 prints and forms the spherical 7 base 3 and prints a single track of dot-shaped micro-columns on the spherical 7 base 3.
[0063] The present embodiment does not limit the shape of the base 3 , as long as the base 3 having a curvature is produced by the first forming laser 1 .
[0064] In this embodiment, before forming the second single melt path 5 , a recessed microstructure 6 is firstly provided on the surface of the base 3 , so that the second single melt path 5 is formed on the recessed microstructure 6 .
[0065] Specifically, the concave microstructure 6 is formed on the surface of the base 3, which can help the molten metal in the molten pool to hang on the surface of the base 3 better. The specific shape of the concave microstructure 6 is not limited. For example, Figure 4 As shown, a groove microstructure is processed on the second single melting channel 5, such as Figure 6 As shown, it is a schematic diagram of processing a pit microstructure on the first single melting channel 2. The microstructure can also be a rectangular groove, a square groove, a circular groove, a curved groove, a straight groove, a cross-mixed groove; pit type: circular pit, square pit, rectangular pit, four-pointed star pit, octagonal pit; other types: micro-column type, micro-cone type, crescent concave texture, crescent convex texture, multi-wedge channel structure, sine structure, etc.
[0066] For example, Figure 5 As shown, a second single melt path 5 is processed on the groove microstructure; Figure 7 As shown, a second single melt path 5 is machined on the pit microstructure.
[0067] In this embodiment, the first shaping laser 1 is a continuous laser, the linear energy density of the first shaping laser 1 is greater than 0.2, and the second shaping laser 4 is a continuous laser or a pulsed laser.
[0068] Specifically, a continuous laser is selected as the first forming laser 1, which has high energy and can continuously form a single melt path, and a continuous laser or a pulsed laser is used as the second forming laser 4, as long as the linear energy density can be controlled. In order to ensure the quality of the base 3 made by the first forming laser 1, the linear energy density of the first forming laser 1 is determined to be greater than 0.2.
[0069] In this embodiment, when the linear energy density of the first forming laser 1 is in the range of [0.2-0.5), the cross section of the base 3 is spherical 7;
[0070] Specifically, Fig. 9 As shown, when the linear energy density of the first forming laser 1 is in the range of [0.2-0.5), the corresponding cross-section of the base 3 is spherical 7 .
[0071] When the linear energy density of the first forming laser 1 is [0.5-1.2), the cross section of the base 3 is in a flat slope shape 8.
[0072] Specifically, specifically, such as Fig.10 As shown, when the linear energy density of the first forming laser 1 is in the range of [0.5-1.2), the corresponding cross-section of the base 3 is sloped.
[0073] Therefore, the cross-sectional curvature of the base 3 can be adjusted by adjusting the linear energy density of the first shaping laser 1, thereby adjusting the degree of wetting between the molten metal obtained by the second shaping laser 4 and the base 3, thereby achieving controllability of the printing process.
[0074] In this embodiment, the continuous laser power is 10 to 1000 W, the scanning speed is 50 to 7000 mm / s, and the spot diameter is 10 to 300 microns;
[0075] The pulse laser power ranges from 5 to 200 W, the scanning speed is from 50 to 5000 mm / s, the spot diameter is from 5 to 200 microns, and the frequency is from 20 to 5000 KHz.
[0076] Specific continuous laser parameters and pulse laser parameters can be adjusted according to actual conditions.
[0077] In this embodiment, a high-speed camera and / or an infrared thermal imaging camera are used. The high-speed camera and / or the infrared imaging camera are connected to an online monitoring processor and a control module to form an in-situ detection device. The in-situ detection device detects the printing process and controls the laser parameters online.
[0078] Specifically, the present invention can perform heat treatment to relieve stress on the workpiece before or after manufacturing a specific number of layers while performing laser additive and subtractive composite manufacturing, and can combine an infrared thermal imaging camera with an online monitoring processor and control module to accurately control the heat treatment temperature and the subsequent annealing temperature.
[0079] The manufacturing of micro-parts is not limited by the above-mentioned conventional steps. In the manufacture of extremely fine micro-parts, a pulsed laser with a small spot size can be used for additive manufacturing. For micro-parts with slightly larger size and thickness, a heat treatment laser with a large spot size can be used for additive manufacturing.
[0080] In this embodiment, during the printing process, a continuous laser is used to perform laser remelting and / or laser heat treatment on the current layer 9, and the laser heat treatment eliminates the thermal stress generated by additive manufacturing.
[0081] Specifically, during the printing process, an industrial camera is used to monitor the quality of the metal molten pool of a specific layer. According to the actual monitoring situation, a continuous laser or heat treatment laser melt path remelting treatment can be used to achieve the purpose of surface structure improvement. After printing a specific number of layers, a continuous laser is used to perform laser heat treatment on fine parts to eliminate the thermal stress generated in additive manufacturing and improve their surface hardness, wear resistance, corrosion resistance, strength and high temperature performance.
[0082] In this embodiment, during the printing process, a pulsed laser is used to perform laser processing, surface pulsed laser shock strengthening or side laser cutting on the corresponding melt surface to trim the single-channel melt morphology and remove drill powder.
[0083] Specifically, during the printing process, an industrial camera is used to monitor the quality of the metal molten pool of a specific layer. According to the actual monitoring situation, a continuous laser or heat treatment laser melt path remelting treatment can be used to achieve the purpose of surface organization improvement. A pulsed laser is used to perform laser processing, surface pulsed laser shock strengthening, and side laser cutting on the surface of the corresponding melt path to achieve single-channel molten pool morphology correction, remove sticky powder on the surface side, reduce defects, refine the organization, increase the dislocation density, and thus improve the performance of additive manufacturing parts.
[0084] In this embodiment, before printing and molding, the fine part model file is first imported into the multi-laser additive and subtractive composite manufacturing equipment, and the required printing strategy is selected from the database according to the thickness of the fine part.
[0085] Specifically, in practical applications, a micro-part model is first established and imported into the additive and subtractive composite manufacturing equipment for printing. According to the width of the micro-part to be manufactured, a suitable manufacturing and processing combination strategy is selected from the additive and subtractive composite manufacturing database, the parameters of the corresponding strategy are selected, and printing begins.
[0086] In this embodiment, the database is established in the following manner:
[0087] High-speed cameras and infrared thermal imaging cameras are used to observe the state of the molten pool during printing. After printing, an electron microscope is used to observe the cross-sectional state of the melt path parts and record the corresponding laser parameters. The printing results and the corresponding laser parameters are stored in the database.
[0088] Specifically, the base 3 database is made: during the printing process, a high-speed camera and an infrared thermal imaging camera are used to observe the state of the molten pool during printing. The single-channel formed parts are observed using an electron scanning microscope SEM to observe the surface morphology and forming quality of the single-channel parts and measure the molten pool width of the single channel under various parameters. The cross-section of the formed single-channel parts is observed with an optical microscope, and the cross-sectional shape, curvature, molten pool height, cross-sectional quality, molten pool depth and the wetting angle between the molten pool and the substrate under various laser parameters are recorded. An additive and subtractive composite manufacturing database is established to record the single-channel quality data and the corresponding forming laser type, and the forming parameters are stored in the additive and subtractive composite manufacturing database-single-channel parts library.
[0089] Making the database of the second melt channel on the base 3: During the printing process, a high-speed camera and an infrared thermal imaging camera are used to monitor the state of the melt pool during printing. The surface morphology and forming quality of the formed double-melt channel parts are observed using a scanning electron microscope SEM, and the molten pool width of the second single melt channel 5 under each different base 3-second layer combination is measured. Use an optical microscope to observe the cross-section of the double-melt channel parts, record the molten pool shape, molten pool depth, molten pool height, molten pool curvature of the second single melt channel 5 under each different combination, and the wetting angle between the two molten pools of the base 3 and the second melt channel, and analyze the changes in the molten pool stability between the single melt channel parts and the base 3-second layer combination parts under the same parameters. Record the data under each base 3-second layer combination and store it in the additive and subtractive composite manufacturing database-double melt channel parts database.
[0090] Preparation of microstructure database: Use three model formulas for solid surface wettability evaluation: Young state model, Wenzel state model, Cassie-Baxter state model to analyze the metal pool wetting angle and its changes of the second single melt channel 5 after microstructure processing, and the stability of the metal melt pool; observe the continuity of the second layer melt pool surface, melt pool width, powder sticking, defect type and quantity, cross-sectional melt pool height, depth, curvature, shape, and defect occurrence. The micro-parts processing strategy of the organic combination of base 3-microtexture-second layer, the parts manufactured by the base 3-second layer processing strategy in the above "Preparation of the second melt channel database on base 3" are compared, and the parts with excellent quality of the second layer melt pool are selected, and their quality shape data, laser type, and parameters are recorded and stored in the additive and subtractive composite manufacturing database.
[0091] In this cycle, through continuous verification and collection, the corresponding database is obtained.
[0092] Test example
[0093] In order to further illustrate the performance of the micro-parts obtained by the manufacturing method of the present invention, the following test examples are conducted:
[0094] Step 1: Prepare the model file of the micro-parts, and prepare for printing by multi-laser additive and subtractive composite manufacturing equipment. Select the forming laser type and laser parameters of each layer of the melt channel according to the thickness of the micro-parts to be manufactured, and the subtractive pulse laser type and laser parameters. In the first layer of melt channel molding, continuous laser molding is selected, and continuous laser parameters are selected according to the fine thickness of the thin-walled parts to be manufactured: spot diameter: 10-300 microns, continuous laser power of 10-1000W, scanning speed of 50-7000mm / s. Use laser line energy density E=P / V to calculate the energy density, where E is the laser line energy density, P is the laser power, and V is the scanning speed. Select a combination of laser power and scanning speed with high line energy density (greater than 0.2) to form a stable and continuous bottom single melt channel base 3. There are two types of cross-sections of the molded base 3: flat slope 8 (linear energy density 0.55-1.5) and hemispherical 7 (linear energy density 0.2-0.55). When the size of the manufactured fine parts is 10-80 microns, the hemispherical 7 single-melt base 3 is used, and when the size is 80-300 microns, the flat slope 8 single-melt base 3 is used.
[0095] Step 2: Use pulsed laser to process microstructures such as grooves and pits in a single melt, and select the parameters of the pulsed laser according to the type, size, and processing depth of the microstructure. Pulse laser parameter selection range: pulse laser power range is 5-200W, the fastest scanning speed is 50-5000mm / s, the spot diameter is 5-200 microns, frequency: 20-5000KHz, and the number of scans is selected according to the depth.
[0096] Step 3: On the single-melt channel base 3 after processing the micro-structure, a second single-melt channel 5 is formed by continuous laser or pulsed laser. The laser type and corresponding laser parameters of the second single-melt channel 5 are selected according to the micro-parts to be manufactured, and the size of the second single-melt channel 5 is ensured to be consistent with the size of the micro-parts to be formed. When the size of the formed micro-parts is 5-50 microns, pulsed laser is used for additive manufacturing (the spot diameter of the pulsed laser is smaller, and the printing can obtain a smaller molten pool size). When manufacturing micro-parts of 50-150 microns, low energy density (linear energy density 0.1-0.2) continuous laser is used to form the second single-melt channel 5. When manufacturing micro-parts of 150-300, continuous laser forming with a linear energy density of 0.2-0.5 is selected, and the appropriate spot diameter is selected according to the size of the micro-parts to be formed, and the spot diameter should be close to the size of the micro-parts to be formed. (Since the second single melt path 5 is stacked on the base 3, compared with the melt path of directly molding fine parts on a flat substrate, the solid-liquid contact angle (wetting angle) of the single melt path stacked on the base 3 is smaller (less than 90 degrees), the stability of the second single melt path 5 is improved, the melt path is more continuous, and the quality is higher.)
[0097] Step 4: Use pulsed laser to remove powder adhered to the surface of the second single melt 5 and correct the melt edge. Use pulsed laser to process microstructures on the second single melt 5 as needed (reasonable arrangement of microstructures can further change the solid-liquid contact angle when two melt layers are stacked, and improve the stability of the metal molten pool of the upper melt).
[0098] Step 5: Repeat steps 3 and 4, and the fine parts are formed. Fig.12 The micro parts shown are Fig.12 It can be seen that the micro-part can have a micro-column with a length of 534.806 μm, and the micro-column is a continuous structure. It can be seen that the manufacturing method of the present invention can produce a continuous thin-walled structure.
[0099] It is best to use a pulsed laser to laser polish the upper surface of the part.
[0100] The present invention generally uses a manufacturing process method of directly forming laser melting powder to form a single melt channel and then stacking single melt channels on top for the manufacture of extremely fine micro-parts. In order to make the thickness of thin-walled parts finer, the energy density of the forming laser must be reduced, so that the molten pool width of the single melt channel is smaller. However, reducing the energy density of the forming laser will cause insufficient melting of the powder, increase the amount of unmelted powder, and adhere to the surface of the melt channel. Secondly, under the action of surface tension and viscosity of the metal liquid, the unstable melt pool will have spheroidization defects, making the melt channel intermittent. In view of the above situation, before printing and forming micro-parts of extremely fine size, a high-energy-density forming laser is first used to form a single melt channel with a large, stable and continuous molten pool width as a base 3 for micro-manufacturing. Then, on the basis of the stable molten pool base 3, a low-energy-density laser is used to form a single melt channel with a small molten pool width. Due to the change in the solid-liquid contact angle, the stability of the original molten pool is improved, and a single-channel molten pool with a small, stable and continuous molten pool width can be obtained. High-speed cameras and industrial cameras are used to monitor the printing process online, and pulsed lasers can be used to remove powder from the edge of the melt path at a specific layer to correct the melt path.
[0101] For parts that require two parts with different fine sizes, after the forming laser processes a single-melt base 3, a pulsed laser is used to process a micro-texture on the surface of the base 3 that is beneficial to reducing the molten pool wetting angle and improving the stability of the molten pool. A single melt with a finer size is superimposed on the micro-textured base 3. During the printing process, a continuous laser with a large spot can be used to heat treat the surface of the part to remove thermal stress.
[0102] For parts with columnar microstructures, a forming laser with a relatively high energy density is used to form a hemispherical 7 molten pool base 3 with a single-pass scanning strategy of closed-loop scanning. A pulsed laser is used to process the micro-texture on the spherical 7 base 3 that is beneficial to the stability of the metal molten pool. A single pass of a small-sized molten pool is stacked on the stable spherical 7 base 3 with the same closed-loop scanning strategy. During the printing process, high-speed cameras and industrial cameras are used for online monitoring, and pulsed lasers are used to remove the powder on the side of the layer. In each layer, pulsed laser processing of micro-textures can also be used for the layer according to actual needs to improve the stability of the lower molten pool and obtain parts with better quality and finer size.
[0103] The present invention starts from the perspective of the molten pool, changes the curvature of the bottom base 3 through additive and subtractive laser composite manufacturing, thereby changing the solid-liquid contact angle of the metal solution and the solid, and improving the stability of the metal molten pool. By superimposing a single melt channel on the stable base 3, the quality of the single melt channel parts that were originally poor in quality and difficult to form under low laser energy density can be significantly improved, a single melt channel with a smaller molten pool width is obtained, the limit size of part forming is reduced, and more sophisticated parts are manufactured.
[0104] The present invention combines continuous laser, pulsed laser, high-speed camera and infrared thermal imaging camera in-situ online detection technology, uses continuous laser to manufacture single-channel molten pool bases 3 of different shapes and curvatures, and then uses pulsed laser to finely process the structural morphology of the base 3, and establishes a database to record the single-channel molten pool morphology under each additive and subtractive laser parameter. A single molten track is superimposed again on the single-channel molten pool base 3 with different surface morphologies, surface microstructures, and cross-sectional curvatures, and online detection is performed using a high-speed camera and an infrared thermal imaging camera. In this way, the most excellent combination of base 3 morphology and surface microstructure, and the combination of base 3 parameters and micro-part parameters for manufacturing micro-parts of a specific thickness can be obtained.
[0105] Continuous laser and pulsed laser composite manufacturing can use pulsed laser to cut inside unsealed parts to achieve molten pool morphology correction. After a specific number of layers of additive manufacturing, pulsed laser is used to remove the adhered powder parts on the side, which can greatly improve the side quality and density of fine parts. The surface of the part can also be laser polished and laser shock strengthened with pulsed laser.
[0106] The present invention can perform heat treatment to relieve stress on the workpiece before or after manufacturing a specific number of layers while performing laser material addition and subtraction composite manufacturing, and can combine an infrared thermal imaging camera with an online monitoring processor and a control module to accurately control the heat treatment temperature and the subsequent annealing temperature.
[0107] The present invention is not limited to the above-mentioned conventional steps in the manufacture of micro-parts. In the manufacture of extremely fine micro-parts, a pulsed laser with a small spot size can be used for additive manufacturing. For micro-parts with slightly larger size and thickness, a heat treatment laser with a large spot size can be used for additive manufacturing.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing micro-parts based on additive and subtractive materials, characterized in that: The following steps are involved: A first forming laser is used to print and form a first single melt path on the current layer to obtain a base with a curved surface; A second single melt track is printed and formed on the base by using a second forming laser, so that the second single melt track is continuously formed on the base, and the structure formed by the second single melt track is the current layer of the part structure. The second forming laser is continuously used to form another single melt track on the second single melt track until the target fine part is obtained. The linear energy density of the second shaping laser is lower than the linear energy density of the first shaping laser. The linear energy density calculation formula is as follows: El=p / v E l —Linear energy density p—laser power v—Scanning speed.
2. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 1, characterized in that: Before forming the second single melt track, a recessed microstructure is firstly provided on the surface of the base so that the second single melt track is formed on the recessed microstructure.
3. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 1, characterized in that: The first shaping laser is a continuous laser, the linear energy density of the first shaping laser is greater than 0.2, and the second shaping laser is a continuous laser or a pulsed laser.
4. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 1, characterized in that: When the linear energy density of the first forming laser is in the range of [0.2-0.5), the cross section of the base is spherical; When the linear energy density of the first forming laser is [0.5-1.2), the cross section of the base is flat and sloped.
5. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 3, characterized in that: The continuous laser power is 10-1000W, the scanning speed is 50-7000mm / s, and the spot diameter is 10-300 microns; The pulse laser power ranges from 5 to 200 W, the scanning speed is from 50 to 5000 mm / s, the spot diameter is from 5 to 200 microns, and the frequency is from 20 to 5000 KHz.
6. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 1, characterized in that: A high-speed camera and / or an infrared thermal imaging camera are used. The high-speed camera and / or the infrared imaging camera are connected to an online monitoring processor and a control module to form an in-situ detection device. The in-situ detection device detects the printing process and controls the laser parameters online.
7. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 6, characterized in that: During the printing process, a continuous laser is used to perform laser remelting and / or laser heat treatment on the current layer, wherein the laser heat treatment eliminates the thermal stress generated by additive manufacturing.
8. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 6, characterized in that: During the printing process, a pulsed laser is used to perform laser processing on the corresponding melt surface, surface pulsed laser shock strengthening or side laser cutting to trim the single-channel melt morphology and remove drill powder.
9. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 6, characterized in that: Before printing, the micro-part model file is first imported into the multi-laser additive and subtractive composite manufacturing equipment, and the required printing strategy is selected from the database according to the thickness of the micro-part.
10. The method for manufacturing micro-parts based on additive and subtractive materials according to claim 9, characterized in that: The database is established in the following manner: High-speed cameras and infrared thermal imaging cameras are used to observe the state of the molten pool during printing. After printing, an electron microscope is used to observe the cross-sectional state of the melt path parts and record the corresponding laser parameters. The printing results and the corresponding laser parameters are stored in the database.
11. A micro-part, characterized in that: The micro-part is manufactured by the micro-part manufacturing method based on additive and subtractive materials as described in any one of claims 1 to 10.
Citation Information
Patent Citations
Method for improving precision of stepped components in laser spot-changing direct formation mode
CN104923784A
Electric arc wire filling additive manufacturing method for inclined thin-walled structural part
CN105921852A
Laser additive manufacturing method for multi-support surface structure of cavity thin-wall structural part
CN107321979A
System and method for additively manufacturing by laser melting of powder bed
CN108136669A
Laser connection method for metal / carbon fiber reinforced thermoplastic composite material
CN112123789A