Molding process of multicolor vamps

By filling and baking multi-color materials in the mold and hot-pressing with hot-melt adhesive connecting layer, the existing multi-color upper production process is solved, and the process is simplified, reducing costs and improving Productivity effect.

CN118927491APending Publication Date: 2024-11-12FUJIAN QINMINFENG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207658.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are many production processes for existing multi-color uppers, requiring multiple molds and equipment, resulting in long forming time, waste of raw materials, and high production costs, resulting in high shoe prices.

Method used

A multi-color upper molding process is adopted, by filling the mold with decorative materials and base materials of different colors, baking and hot-pressing molding, using hot melt adhesive connection layers, simplifying the process and reducing the demand for mold and equipment. Improve production efficiency.

Benefits of technology

The production process of multi-color uppers has been greatly simplified, cost is reduced, forming time is shortened, the quality and aesthetics of the upper are improved, raw materials are saved, and production efficiency and product output is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a forming process of a multicolor vamp, which comprises the following steps: step 1, respectively pouring a vamp decorative material with at least one color into at least one decorative pattern layer area of a mold, and then baking and curing for the first time to obtain a decorative pattern layer; step 2, pouring a vamp bottom color material into the mold, covering each decorative pattern layer area in the step 1, and then baking and curing for the second time to obtain a decorative pattern composite layer; 3, covering the surface of the decorative pattern composite layer prepared in the step 2 with a layer of hot melt adhesive, and then baking for the third time to obtain a decorative pattern composite layer with the hot melt adhesive; 4, the surface of the decorative pattern composite layer obtained in the step 3 is coated with a vamp substrate, then hot press molding, cooling and demolding are conducted, and the multicolor vamp is obtained.The decorative pattern layers of different colors are poured into one mold and integrally formed with the vamp bottom color layer, the finished multicolor vamp product is formed, the production process of the finished multicolor vamp product is greatly simplified, and the production efficiency is improved. The manufacturing cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shoe upper processing, and in particular to a molding process for a multi-color shoe upper. Background Art

[0002] At present, most of the uppers have a single-color or multi-color upper decorative layer, which can improve the overall appearance of the shoes and enhance the recognition of the products. However, the existing process for making such multi-color uppers requires six processes, such as processing the mold, pouring the decorative material into the mold, scraping the mold, cleaning the mold, and placing the mesh on the mold, to produce a single-color upper. If you want to add more colors on the basis of the first color of the upper, you need to repeat the first five of the six processes for each additional color of the upper. Therefore, the multi-color uppers in the prior art have many production processes, which are very troublesome to produce, require many molds, and require high equipment investment. The uppers need to be molded multiple times, which takes a long time to mold, and there is a lot of waste of raw materials. The production cost of the uppers is high, resulting in a high price of the shoes. Therefore, people are eager to have a multi-color upper molding process with short molding time, less waste of raw materials, and low production cost of the uppers. Summary of the invention

[0003] The purpose of the present invention is to solve the above technical problems and provide a multi-color upper forming process, which has fewer production processes, fewer molds, low equipment investment, short shoe material forming time, less waste of raw materials, lower shoe material production cost and strong three-dimensional sense of the upper.

[0004] To achieve the above object, the technical solution adopted by the present invention is as follows: A molding process of a multi-color upper comprises the following steps: Step 1: pouring at least one color of upper decorative material into at least one decorative layer area of ​​the mold, and then sending the mold into an oven for a first baking and curing to obtain a decorative layer; Step 2: pouring the upper base color material into the mold and covering each decorative layer area in step 1, and then sending the mold into an oven for a second baking and curing to obtain a decorative pattern composite layer; Step 3: Cover the surface of the decorative pattern composite layer obtained in step 2 with a layer of hot melt adhesive, and then press the upper base color edge material with a hot and cold press, clean the upper base color edge material, and then tear off the release paper on the hot melt adhesive, and continue to send the mold into the oven for a third baking, until the hot melt adhesive is melted and completely integrated with the upper base color material, to obtain a decorative pattern composite layer with hot melt adhesive; Step 4: Lay the surface of the decorative pattern composite layer obtained in step 3 on the upper base material, then send the upper base material and the mold to a hot press, perform hot pressing molding on the decorative pattern composite layer and the upper base material, cool and demold, and obtain a multi-color upper.

[0005] Preferably, the step one also includes cleaning the mold.

[0006] Preferably, in step one, the baking temperature of the first baking and curing is 300-330° C., and the baking time is 70-80 seconds; this can fully activate the upper decorative materials of different colors for curing, so that the decorative layer is partially solidified and formed, with low energy consumption and low cost.

[0007] Preferably, in the step 2, the baking temperature of the second baking and maturation is 300-330° C., and the baking time is 70-80 seconds; the material of the upper base color can be fully activated for maturation, so that the upper base color material is solidified and formed, and the energy consumption and cost are low.

[0008] Preferably, in the step three, the baking temperature of the third baking and maturation is 300-330°C, and the baking time is 70-80 seconds; the hot melt adhesive can be fully melted and completely integrated with the upper base material, so that the connection between the upper base material and the decorative pattern composite layer is more firmly connected and interlayer separation is less likely to occur.

[0009] Preferably, in step three, the hot pressing temperature of the hot pressing molding is 150-180°C, and the hot pressing time is 60-70s; the upper base material and the upper base color layer can be stably bonded, and interlayer separation is not likely to occur, and the energy consumption and cost are low.

[0010] Preferably, the upper decoration material in step one and the upper base material in step two are both polyurethane materials.

[0011] Preferably, in step one and step two, the mold is provided with a first groove for forming the decorative layer and a second groove for forming the upper base color layer, and the depth of the second groove is greater than the depth of the first groove.

[0012] Preferably, in step 4, cooling is performed by natural cooling or mold supercooling water cooling.

[0013] Preferably, in step 4, the upper bottom material is a cloth sheet.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The shoe upper forming process of the present invention is easy to operate. Decorative layers of different colors are poured into one mold and formed integrally with the shoe upper base color layer to form a multi-color shoe upper finished product, which greatly simplifies the production process of the multi-color shoe material finished product, reduces the manufacturing cost of the multi-color shoe material finished product, saves a large amount of raw materials, and saves the production cost of the multi-color shoe material.

[0015] 2. The shoe upper forming process of the present invention reduces the forming time of the shoe upper finished product, saves time, improves production efficiency, and increases the output of multi-color shoe upper finished products.

[0016] 3. A hot melt adhesive layer is added to the upper forming process of the present invention to make the decorative pattern composite layer and the upper base material more firmly connected and less likely to separate between layers, thereby improving the quality of the multi-color upper product.

[0017] 4. The finished shoes made of multi-color shoe fabrics of the present invention have improved grades in appearance, making them more eye-catching and beautiful. The decorative layer has a strong three-dimensional sense and rich colors, achieving a better decorative effect, having a sense of fashion and trend, and can be favored and recognized by consumers, thereby achieving the purpose of expanding the sales of finished shoes. DETAILED DESCRIPTION

[0018] The present invention is further described below in conjunction with embodiments, and the embodiments of the present invention include but are not limited to the following embodiments.

[0019] Example 1 A molding process for a multi-color shoe upper comprises the following steps: Step 1: pouring a shoe upper decoration material of one color into a decoration layer area of ​​the mold, and then sending the mold into an oven for the first baking and curing to obtain a decoration layer of one color; Step 2: pouring the upper base color material into the mold and covering each decorative layer area in step 1, and then sending the mold into an oven for a second baking and curing to obtain a decorative pattern composite layer; Step 3: Cover the surface of the decorative pattern composite layer obtained in step 2 with a layer of hot melt adhesive, and then press the upper base color edge material with a hot and cold press, clean the upper base color edge material, and then tear off the release paper on the hot melt adhesive, and continue to send the mold into the oven for a third baking, until the hot melt adhesive is melted and completely integrated with the upper base color material, to obtain a decorative pattern composite layer with hot melt adhesive; Step 4: Lay the surface of the decorative pattern composite layer obtained in step 3 on the upper base material, then send the upper base material and the mold to a hot press, perform hot pressing molding on the decorative pattern composite layer and the upper base material, cool and demold, and obtain a three-color upper.

[0020] The above step 1 also includes cleaning the mold before pouring the upper decorative material into the mold. By cleaning the mold, impurities in the mold are prevented from affecting product quality.

[0021] In the above step 1, the baking temperature of the first baking and curing is 300° C., and the baking time is 70 seconds; this can fully activate the upper decorative materials of different colors for curing, so that the decorative layer is partially solidified, with low energy consumption and low cost.

[0022] In the above step 2, the baking temperature of the second baking and maturation is 310° C., and the baking time is 72 seconds; this can fully activate the material of the upper base color for maturation, so that the upper base color material is solidified and formed, with low energy consumption and low cost.

[0023] In the above step three, the baking temperature of the third baking is 300°C and the baking time is 75 seconds; the hot melt adhesive can be fully melted and completely integrated with the upper base material, making the connection between the upper base material and the decorative pattern composite layer more firmly and less prone to interlayer separation.

[0024] In the above step three, the hot pressing temperature of the hot pressing molding is 160° C., and the hot pressing time is 60 seconds; the upper base material and the upper base color layer can be stably bonded, and the phenomenon of interlayer separation is not easy to occur, and the energy consumption and cost are low.

[0025] The upper decorative material in the above step 1 and the upper base material in the above step 2 are both polyurethane materials.

[0026] In the above steps 1 and 2, the above mold is provided with a first groove for forming the decorative layer and a second groove for forming the upper base layer, and the depth of the second groove is greater than the depth of the first groove.

[0027] In the above step 4, cooling is performed by using supercooled water to cool the mold, thereby improving production efficiency.

[0028] In the above step 4, the upper bottom material is a cloth sheet.

[0029] Example 2 A molding process for a multi-color shoe upper comprises the following steps: Step 1: Pour two colors of upper decorative materials into different decorative layer areas of the mold respectively, and then send the mold into an oven for the first baking and maturation, so that the two colors of upper decorative materials are cured at the same time to obtain two colors of decorative layers; of course, the present invention can also use three or more colors of upper decorative materials for simultaneous baking and maturation.

[0030] Step 2: pouring the upper base color material into the mold and covering each decorative layer area in step 1, and then sending the mold into an oven for a second baking and curing to obtain a decorative pattern composite layer; Step 3: Cover the surface of the decorative pattern composite layer obtained in step 2 with a layer of hot melt adhesive, and then press the upper base color edge material with a hot and cold press, clean the upper base color edge material, and then tear off the release paper on the hot melt adhesive, and continue to send the mold into the oven for a third baking, until the hot melt adhesive is melted and completely integrated with the upper base color material, to obtain a decorative pattern composite layer with hot melt adhesive; Step 4: Lay the surface of the decorative pattern composite layer obtained in step 3 on the upper base material, then send the upper base material and the mold to a hot press, perform hot pressing molding on the decorative pattern composite layer and the upper base material, cool and demold, and obtain a four-color upper.

[0031] The above step 1 also includes cleaning the mold before pouring the upper decorative material into the mold. By cleaning the mold, impurities in the mold are prevented from affecting product quality.

[0032] In the above step 1, the baking temperature of the first baking and curing is 330° C., and the baking time is 75 seconds; this can fully activate the upper decorative materials of different colors for curing, so that the decorative layer is partially solidified, and has low energy consumption and low cost.

[0033] In the above step 2, the baking temperature of the second baking and maturation is 300° C., and the baking time is 73 seconds; this can fully activate the material of the upper base color for maturation, so that the upper base color material is solidified and formed, with low energy consumption and low cost.

[0034] In the above step three, the baking temperature of the third baking is 300°C and the baking time is 75 seconds; the hot melt adhesive can be fully melted and completely integrated with the upper base material, making the connection between the upper base material and the decorative pattern composite layer more firmly and less prone to interlayer separation.

[0035] In the above step three, the hot pressing temperature of the hot pressing molding is 170° C., and the hot pressing time is 70 seconds; the upper base material and the upper base color layer can be stably bonded, and the phenomenon of interlayer separation is not easy to occur, and the energy consumption and cost are low.

[0036] The upper decorative material in the above step 1 and the upper base material in the above step 2 are both polyurethane materials.

[0037] In the above steps 1 and 2, the above mold is provided with a first groove for forming the decorative layer and a second groove for forming the upper base layer, and the depth of the second groove is greater than the depth of the first groove.

[0038] In the above step 4, cooling is performed by natural cooling or mold supercooling water cooling.

[0039] In the above step 4, the upper bottom material is a cloth sheet. The above embodiments are only preferred implementations of the present invention and should not be used to limit the protection scope of the present invention. Any changes or modifications that are made to the main design concept and spirit of the present invention without any substantial significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention.

Claims

1. A molding process for a multi-color upper. It is characterized in that The steps include: Step 1: pouring at least one color of upper decorative material into at least one decorative layer area of ​​the mold, and then sending the mold into an oven for a first baking and curing to obtain a decorative layer; Step 2: pouring the upper base color material into the mold and covering each decorative layer area in step 1, and then sending the mold into an oven for a second baking and curing to obtain a decorative pattern composite layer; Step 3: Cover the surface of the decorative pattern composite layer obtained in step 2 with a layer of hot melt adhesive, and then press the upper base color edge material with a hot and cold press, clean the upper base color edge material, and then tear off the release paper on the hot melt adhesive, and continue to send the mold into the oven for a third baking, until the hot melt adhesive is melted and completely integrated with the upper base color material, to obtain a decorative pattern composite layer with hot melt adhesive; Step 4: Lay the surface of the decorative pattern composite layer obtained in step 3 on the upper base material, then send the upper base material and the mold to a hot press, perform hot pressing molding on the decorative pattern composite layer and the upper base material, cool and demold, and obtain a multi-color upper.

2. A molding process for a multi-color upper according to claim 1, Features: The step one also includes cleaning the mold.

3. A molding process for a multi-color upper according to claim 1, Features: In the step 1, the baking temperature for the first baking and curing is 300-330° C., and the baking time is 70-80 seconds.

4. A molding process for a multi-color shoe upper according to claim 1, Features: In the step 2, the baking temperature for the second baking and curing is 300-330° C., and the baking time is 70-80 seconds.

5. A molding process for a multi-color shoe upper according to claim 1, Features: In the step 3, the baking temperature of the third baking and curing is 300-330° C., and the baking time is 70-80 seconds.

6. A molding process for a multi-color upper according to claim 1, Features: In the step 3, the hot pressing temperature of the hot pressing molding is 150-180° C., and the hot pressing time is 60-70 seconds.

7. A molding process for a multi-color shoe upper according to claim 1, Features: The upper decorative material in step one and the upper base material in step two are both polyurethane materials.

8. The forming process of a multi-color shoe upper according to claim 1, Features: In the step 1 and the step 2, the mold is provided with a first groove for forming the decorative layer and a second groove for forming the upper base layer, and the depth of the second groove is greater than the depth of the first groove.

9. The forming process of a multi-color shoe upper according to claim 1, Features: In the step 4, cooling is performed by natural cooling or mold supercooling water cooling.