Method for preparing iron phosphate from phosphorus-containing wastewater precipitation slag and iron phosphate
By utilizing phosphorus-containing wastewater precipitate and ferrous sulfate heptahydrate, a byproduct of titanium dioxide production, to prepare lithium iron phosphate, the high cost of the traditional ammonium method has been solved, achieving low-cost and high-quality preparation of lithium iron phosphate and promoting the development of lithium iron phosphate cathode materials and lithium batteries.
Patent Information
- Application Number
- CN202411158569.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
In existing technologies, the traditional ammonium method for preparing ferric phosphate is costly, resulting in excessively high production costs for ferric phosphate.
Using phosphorus-containing wastewater sediment as the phosphorus source and ferrous sulfate heptahydrate, a byproduct of titanium dioxide production, as the iron source, ferric phosphate is prepared through a series of steps, including acid solution leaching, pH adjustment, filtration, hydrogen peroxide precipitation, and drying, thereby reducing production costs.
It effectively reduced the production cost of lithium iron phosphate while ensuring the quality indicators of battery-grade lithium iron phosphate, with an iron-to-phosphorus ratio of over 0.97. Other impurities and morphology indicators also met the requirements, thus promoting the development of lithium iron phosphate cathode materials and lithium batteries.
Smart Images

Figure BDA0005005781180000061 
Figure BDA0005005781180000071 
Figure BDA0005005781180000072
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ferric phosphate, and in particular to a method for preparing ferric phosphate by utilizing precipitated residue from phosphorus-containing wastewater and the ferric phosphate. Background Art
[0002] As new energy chemical materials enter a new round of economic cycle, the downstream supply and demand are expanding rapidly, and the demand for chemical materials related to various links in the upstream of the lithium battery industry chain is also increasing rapidly.
[0003] The current mainstream is to prepare lithium iron phosphate with iron phosphate, in which iron phosphate can provide both iron source and phosphorus source during the synthesis of lithium iron phosphate, and the unit cell volume changes slightly, only about 6.81%, which is beneficial to improving the stability of the material. Therefore, iron phosphate has become the core precursor for preparing lithium iron phosphate positive electrode materials.
[0004] However, the cost of iron phosphate prepared by the mainstream ammonium method is relatively high. The preparation of industrial ammonium phosphate requires the selection of suitable mineral sources, and the phosphoric acid is prepared and then neutralized to obtain industrial ammonium phosphate. It has high requirements for phosphorus sources and the cost is relatively high, resulting in a high cost of iron phosphate. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue and ferric phosphate, which can effectively reduce the production cost of ferric phosphate.
[0006] The embodiment of the present invention is achieved by the following technical solution: The method of preparing ferric phosphate using phosphorus-containing wastewater precipitate residue of the present invention comprises the following steps:
[0007] (1) using an acid solution to leach the phosphorus-containing wastewater to obtain an acidic leaching solution having a P content of 2.4-2.6 wt %, a Ca content of 0.9-1.2 wt %, and an Fe content of 0.03-0.05 wt %;
[0008] (2) adjusting the pH of the Fe(II) solution to 0.6-1.4 to obtain an iron source solution having an Fe content of 7.5-8.5 wt %; wherein ferrous sulfate heptahydrate produced as a byproduct of titanium dioxide can be used as the iron source.
[0009] (3) adding the acidic leaching solution obtained in step (1) dropwise to the iron source solution obtained in step (2), and obtaining a solid-liquid mixture after reaction; wherein the molar ratio of P in the acidic leaching solution to Fe in the iron source is 1-1.4:1.
[0010] (4) After filtering the solid-liquid mixture obtained in step (3), H2O2 is added to the filtrate, and the pH of the filtrate is adjusted to 0.8-1.5, and the reaction is maintained for 1-3 hours to obtain crude iron phosphate;
[0011] (5) adding phosphoric acid having a concentration of 85% to the crude iron phosphate in step (4), and aging for 2-5 hours to obtain iron phosphate dihydrate;
[0012] (6) filtering the ferric phosphate dihydrate obtained in step (5) and washing until the pH of the washing water reaches 2.6-3.5; and drying at 80-90° C. until the free water content is ≤1.0%.
[0013] The present invention also provides iron phosphate prepared based on the above method for preparing iron phosphate using phosphorus-containing wastewater precipitate residue.
[0014] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects: the method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue and the ferric phosphate of the present invention use low-cost phosphorus-containing wastewater precipitate residue as a phosphorus source to replace industrial ammonium phosphate in the traditional ammonium method, effectively solving the problem of high cost of raw materials for producing battery-grade ferric orthophosphate by the current traditional process;
[0015] The present invention has broad application prospects, and expands the road for the high-value phosphating slag and the high-value phosphate co-production. It uses ferrous sulfate heptahydrate, a byproduct of titanium dioxide, as an iron source to reduce production costs. The cost of battery-grade iron orthophosphate is greatly reduced, which will help promote the rapid development of lithium iron phosphate positive electrode materials and lithium batteries. Under the premise of ensuring that the prepared battery-grade iron phosphate meets the above indicators, the iron-phosphorus ratio reaches more than 0.97, and other impurities, morphology, crystallinity, etc. also meet the indicator requirements. DETAILED DESCRIPTION
[0016] Example 1
[0017] This embodiment provides a method for preparing iron phosphate using phosphorus-containing wastewater precipitate residue, comprising the following steps:
[0018] (1) using sulfuric acid to leach the phosphorus-containing wastewater to obtain an acidic leaching solution having a P content of 2.4 wt%, a Ca content of 0.9 wt%, and an Fe content of 0.03 wt%;
[0019] (2) using an acidic pH regulator to adjust the pH of the ferrous sulfate solution to 0.6-0.8 to obtain an iron source solution with an Fe content of 7.5%;
[0020] (3) adding the acidic leaching solution obtained in step (1) dropwise to the iron source solution obtained in step (2) at a molar ratio of P:Fe=1:1, and reacting for 1 hour to obtain a solid-liquid mixture;
[0021] (4) After filtering the solid-liquid mixture obtained in step (3), H2O2 was added to the filtrate and the pH was adjusted to 0.8 until complete precipitation to obtain crude iron phosphate;
[0022] (5) adding 85% phosphoric acid to the crude iron phosphate in step (4), and aging for 2 hours to obtain iron phosphate dihydrate;
[0023] (6) filtering the dihydrate ferric phosphate obtained in step (5), washing until the pH of the washing water reaches 2.6, drying at 80° C. until the free water content is ≤1.0%, and then crushing and sieving to control the particle size D50 to be ≥90% in the range of 2 to 5 μm, thereby obtaining battery-grade dihydrate or anhydrous ferric phosphate.
[0024] Example 2
[0025] This embodiment provides a method for preparing iron phosphate using phosphorus-containing wastewater precipitate residue, comprising the following steps:
[0026] (1) using sulfuric acid to leach the phosphorus-containing wastewater to obtain an acidic leaching solution having a P content of 2.6 wt%, a Ca content of 1.2 wt%, and an Fe content of 0.05 wt%;
[0027] (2) using an acidic pH regulator to adjust the pH of the ferrous sulfate solution to 0.8-1.4 to obtain an iron source solution with an Fe content of 8.5%;
[0028] (3) adding the acidic leaching solution obtained in step (1) dropwise to the iron source solution obtained in step (2) at a molar ratio of P:Fe=1.4:1, and reacting for 3 hours to obtain a solid-liquid mixture;
[0029] (4) After filtering the solid-liquid mixture obtained in step (3), H2O2 was added to the filtrate and the pH was adjusted to 1.5 until complete precipitation to obtain crude iron phosphate;
[0030] (5) adding 85% phosphoric acid to the crude iron phosphate in step (4), and aging for 5 hours to obtain iron phosphate dihydrate;
[0031] (6) filtering the dihydrate ferric phosphate obtained in step (5), washing until the pH of the washing water reaches 3.5, drying at 90° C. until the free water content is ≤1.0%, and then crushing and sieving to control the particle size D50 to be ≥90% in the range of 2 to 5 μm, thereby obtaining battery-grade dihydrate or anhydrous ferric phosphate.
[0032] Example 3
[0033] This embodiment provides a method for preparing iron phosphate using phosphorus-containing wastewater precipitate residue, comprising the following steps:
[0034] (1) using sulfuric acid to leach the phosphorus-containing wastewater to obtain an acidic leaching solution having a P content of 2.5 wt%, a Ca content of 1.1 wt%, and an Fe content of 0.04 wt%;
[0035] (2) using an acidic pH regulator to adjust the pH of the ferrous sulfate solution to 1-1.2 to obtain an iron source solution with an Fe content of 8.0%;
[0036] (3) adding the acidic leaching solution obtained in step (1) dropwise to the iron source solution obtained in step (2) at a molar ratio of P:Fe=1.2:1, and reacting for 2 hours to obtain a solid-liquid mixture;
[0037] (4) After filtering the solid-liquid mixture obtained in step (3), H2O2 was added to the filtrate and the pH was adjusted to 1.2 until complete precipitation to obtain crude iron phosphate;
[0038] (5) adding 85% phosphoric acid to the crude iron phosphate in step (4), and aging for 35 minutes to obtain iron phosphate dihydrate;
[0039] (6) filtering the dihydrate ferric phosphate obtained in step (5), washing until the pH of the washing water reaches 3.0, drying at 80-90° C. until the free water content is ≤1.0%, and then crushing and sieving to control the particle size D50 to be ≥90% in the range of 2-5 μm, thereby obtaining battery-grade dihydrate or anhydrous ferric phosphate.
[0040] Experimental Example 1
[0041] The components of the iron phosphate prepared in Examples 1-3 were tested and compared with the industry standards for iron phosphate, and the results are shown in Table 1. From the data in Table 1, it can be seen that the iron phosphate prepared by the method of the present application meets the standards in all aspects.
[0042] Table 1 Composition of the iron phosphate obtained in Examples 1-3
[0043]
[0044]
[0045] Experimental Example 2
[0046] Ferric phosphate was prepared according to the method of Example 3, and the cost was compared with that of the traditional ammonia process, and the results are shown in Table 2. From the data in Table 2, it can be seen that the method of the present application can effectively reduce the production cost by preparing ferric phosphate.
[0047] Table 2 Cost difference between Example 3 and traditional process for producing iron phosphate
[0048]
[0049] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue, characterized in that: The steps include: (1) using an acid solution to leach the phosphorus-containing wastewater to obtain an acidic leaching solution; (2) adjusting the pH of the Fe(II) solution to 0.6-1.4 to obtain an iron source solution; (3) adding the acidic leaching solution obtained in step (1) dropwise to the iron source solution obtained in step (2) to obtain a solid-liquid mixture after reaction; (4) filtering the solid-liquid mixture obtained in step (3), adding an oxidant to the filtrate and adjusting the pH to obtain crude ferric phosphate; (5) adding phosphoric acid to the crude iron phosphate in step (4), and obtaining iron phosphate dihydrate after aging; (6) filtering, washing and drying the ferric phosphate dihydrate obtained in step (5).
2. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: In the acidic leaching solution, the P content is 2.4-2.6wt%, the Ca content is 0.9-1.2wt%, and the Fe content is 0.03-0.05wt%.
3. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: The content of Fe in the iron source solution in step (2) is 7.5-8.5wt%.
4. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: In step (3), the molar ratio of P in the acidic leaching solution to Fe in the iron source is 1-1.4:
1.
5. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: In step (4), the oxidant added to the filtrate is H2O2, the pH of the filtrate is adjusted to 0.8-1.5, and the reaction is maintained for 1-3 hours.
6. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: In step (5), the concentration of phosphoric acid is 85% and the aging time is 2-5 hours.
7. The method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to claim 1, characterized in that: In step (6), washing is performed until the pH of the washing water reaches 2.6-3.5; and drying is performed at 80-90° C. until the free water content is ≤1.0%.
8. Ferric phosphate prepared by the method for preparing ferric phosphate using phosphorus-containing wastewater precipitate residue according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing anhydrous iron phosphate from titanium-containing lithium iron phosphate waste
CN114180546A
Method for preparing high-purity iron phosphate dihydrate and removing impurities
CN117105194A