Preparation method of carbon dot composite material taking waste plastic as raw material

By heating and processing waste plastic with reactants such as glycol and urea, carbon dot composite materials are prepared, which solves the problem of waste plastic treatment and carbon dot material luminescence in the water environment, and realizes the long afterglow luminescence performance and stability of the material Improved sex, suitable for a variety of application fields.

CN118929637APending Publication Date: 2024-11-12CHONGQING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160390.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively treat and reuse waste plastics, resulting in environmental pollution and waste of resources, and carbon dot materials cannot emit light in water environments, resulting in strong water absorption and unstable long afterglow luminescence performance.

Method used

By mixing waste plastic with reactants such as glycol and urea and heating it, ultrasonic, centrifugation, dialysis and freeze-drying treatment, carbon dot material is obtained and mixed with the matrix material in a hydrothermal reaction to prepare a water-resistant carbon dot composite material. , solves the problem of luminescence of materials in water environment.

Benefits of technology

It has achieved effective upgrade and recycling of waste plastics and long afterglow luminescence performance of carbon dot composite materials, improved the stability and application potential of the material, and is suitable for lighting, imaging and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929637A_ABST
    Figure CN118929637A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a carbon dot composite material with waste plastic as a raw material, and relates to the field of material preparation, and the preparation method comprises the following steps: S1, mixing the waste plastic, a reactant and an auxiliary reactant, heating to 200-300 DEG C, and reacting for 6-12 hours; the reactant is ethylene glycol; the auxiliary reactant is urea or a derivative thereof; s2, dissolving the reaction product in deionized water, and sequentially performing ultrasonic treatment, centrifugation, dialysis and freeze drying treatment to obtain a carbon dot material; and S3, mixing the carbon dot material and the matrix material, carrying out a hydrothermal reaction at 50-300 DEG C for 0.5-12 h, and washing and filtering the product after the reaction is completed to obtain the water-resistant carbon dot composite material. The waste plastic is used as the raw material, the carbon dot composite material is prepared by upgrading and recycling the waste plastic through the provided method, and the problems of plastic pollution and resource regeneration can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material preparation, and in particular to a method for preparing a carbon dot composite material using waste plastics as raw materials. Background Art

[0002] Polymer materials are widely used, bringing great convenience to daily life and industrial development. However, the generation of waste plastics is also a major problem that cannot be ignored at the social level. At present, the global methods for dealing with waste plastics include landfill, incineration, recycled granulation and pyrolysis. Among them, landfill and incineration will cause pollution to the environment. If plastic products remain in farmland for a long time, it will affect the absorption of water and nutrients by crops, inhibit the growth and development of crops, and cause a reduction in crop yields. If animals eat plastic products by mistake, they will suffer from indigestion or even death. This not only puts great pressure on the environment, but also fails to achieve effective reuse of resources. Upcycling of waste plastics is a very challenging problem. If the degradation and reprocessing of waste plastics can be achieved in one step, resources can be effectively reused. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a carbon dot composite material using waste plastics as raw materials.

[0004] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0005] Provided is a method for preparing a carbon dot composite material using waste plastics as raw materials, comprising the following steps:

[0006] S1: Mix waste plastics, a reactant and an auxiliary reactant, heat to 200-300°C and react for 6-12 hours; the reactant is ethylene glycol; the auxiliary reactant is urea or its derivatives;

[0007] S2: dissolving the reaction product in deionized water, and sequentially subjecting it to ultrasonic treatment, centrifugation, dialysis and freeze drying to obtain a carbon dot material;

[0008] S3: After mixing the carbon dot material and the matrix material, a hydrothermal reaction is carried out at 50-300° C. for 0.5-12 hours. After the reaction is completed, the product is washed and filtered to obtain a water-resistant carbon dot composite material.

[0009] Furthermore, the waste plastics are a combination of one or more of discarded polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon or unsaturated polyester.

[0010] Furthermore, the auxiliary reaction agent is urea, 1,1-dimethylurea, 1,3-dimethylurea, tetramethylurea, thiourea, 2-pyrrolidone, tetrahydro-2-pyrimidinone, ethyl carbamate, uric acid, urea phosphate or urea.

[0011] Furthermore, the mass ratio of waste plastics, reactants and auxiliary reactants is 1:5-50:0.2-10.

[0012] Furthermore, the matrix material is a combination of one or more of cyanuric acid, urea, uric acid, urea phosphate, urea thiocyanate, boric acid, boron trioxide, silicon dioxide, silica gel, orthosilicate, hydrotalcite, molecular sieve, ethyl carbamate, polyvinyl alcohol, polymethyl methacrylate, polyacrylonitrile or polyvinyl pyrrolidone.

[0013] Furthermore, the mass ratio of the matrix material to the carbon dot material is 0.5-100:1.

[0014] Furthermore, a step S110 is provided between steps S1 and S2: the reaction product of S1 is subjected to a reduced pressure distillation reaction at 125° C. for 1 hour, and the product obtained by the reduced pressure distillation reaction is used to execute S2.

[0015] The beneficial effects of the present invention are:

[0016] The present invention uses waste plastics as raw materials and uses the provided method to upgrade and recycle waste plastics to obtain carbon dot composite materials, which can effectively solve the problems of plastic pollution and resource regeneration. The carbon dot material made from waste plastics is embedded in a suitable matrix in an "encapsulation" manner, effectively avoiding the quenching effect of the external environment on the carbon long afterglow luminescence performance, overcoming the defects of carbon dot materials that are highly hygroscopic and cannot emit light in a water environment, and further improving the lifespan and stability of the long afterglow luminescence of the carbon dot composite material. The carbon dot composite material prepared using waste plastics as raw materials has excellent long afterglow luminescence performance and can be applied to many fields such as lighting, imaging, road signs and warnings, product anti-counterfeiting, information encryption, biological identification, and sensing. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the appearance of the carbon dot composite material prepared in Example 1;

[0018] Figure 2 This is the infrared spectrum of the afterglow carbon dot material prepared by the present invention;

[0019] Figure 3 is the phosphorescence spectrum of the carbon dot composite material prepared in Example 1;

[0020] Figure 4 is a phosphorescence spectrum of the carbon dot composite material prepared in Example 2;

[0021] Figure 5 is the phosphorescence spectrum of the carbon dot composite material prepared in Example 3;

[0022] Figure 6 is the phosphorescence spectrum of the carbon dot composite material prepared in Example 4; Figure 7 is the phosphorescence spectrum of the carbon dot composite material prepared in Example 5; Figure 8 This is the phosphorescence spectrum of the carbon dot composite material prepared in Example 6. DETAILED DESCRIPTION

[0023] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0024] The waste plastics used in the embodiments of the present invention are household waste plastics and experimental waste plastics collected within the scope of Chongqing University of Technology, including waste bottle pieces, packing tapes, food packaging, medicine packaging, sample bags, disposable plastic experimental consumables, etc. In specific implementation, waste polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon, unsaturated polyester or other plastic products can be used in combination of one or more.

[0025] Cut the waste plastic into pieces. The purpose of cutting into pieces is to control the weight component, facilitate laboratory experiments, and facilitate placement into the reactor. In specific implementation, in large-scale preparation, if the reactor feed port is larger than the waste plastic, no cutting is required.

[0026] Example 1

[0027] 2 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of urea were placed in a reactor, and the reactor was reacted at 275 °C for 6 h. After the reaction is completed, it is transferred to a vacuum distillation device and vacuum distilled at 125°C for 1h to obtain a crude product. 50mL of deionized water is used to dissolve the obtained crude product. A centrifuge is used to centrifuge at a speed of 4000r / min for 1h, and then the supernatant is removed. The residue is poured into a dialysis bag with a molecular weight cutoff of 200. In specific implementation, a dialysis bag with a molecular weight cutoff of 100, 300 or 500 can also be used; it is placed in a beaker filled with 300ml of deionized water for dialysis, and the dialysis time is 48h. After the dialysis is completed, the supernatant in the dialysis bag is taken and freeze-dried using a freeze dryer model FDS-2000. The internal pressure is 0pa, the temperature is -80°C, and the freeze drying time is 72h to obtain a carbon dot material. 0.3 carbon dot material is weighed and hydrothermally reacted with 3g of cyanuric acid at 200°C for 3h. After filtering the reaction product, it is washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot material. Figure 1 The carbon dot composite material shown is composed of Figure 1 It can be seen that the carbon dot composite material is quasi-spherical with a diameter of about 10 nm.

[0028] Example 2

[0029] 2g of waste plastic fragments, 20mL of ethylene glycol and 2g of urea were placed in a reactor, and the reactor was reacted at 275°C for 6h. After the reaction was completed, it was transferred to a vacuum distillation device and vacuum distilled at 125°C for 1h to obtain a crude product. 50mL of deionized water was used to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a carbon dot material. 0.3 of the carbon dot material was weighed and hydrothermally reacted with 3g of boric acid at 200°C for 3h. After filtering the reaction product, it was washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot composite material.

[0030] Example 3

[0031] 2g of waste plastic fragments, 20mL of ethylene glycol and 2g of urea were placed in a reactor, and the reactor was reacted at 275°C for 6h. After the reaction was completed, it was transferred to a vacuum distillation device and vacuum distilled at 125°C for 1h to obtain a crude product. 50mL of deionized water was used to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a carbon dot material. 0.3 carbon dot material was weighed and hydrothermally reacted with 3g of silica at 200°C for 3h. After filtering the reaction product, it was washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot composite material.

[0032] Example 4

[0033] 2g of waste plastic fragments, 20mL of ethylene glycol and 2g of urea were placed in a reactor, and the reactor was reacted at 275°C for 6h. After the reaction was completed, it was transferred to a vacuum distillation device and vacuum distilled at 125°C for 1h to obtain a crude product. 50mL of deionized water was used to dissolve the obtained crude product, and the same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a carbon dot material. 0.3 carbon dot material was weighed and hydrothermally reacted with 3g of hydrotalcite at 200°C for 3h. After filtering the reaction product, it was washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot composite material.

[0034] Example 5

[0035] 3 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of tetramethylurea were placed in a reactor, and the reactor was reacted at 275 ° C for 6 h. After the reaction was completed, it was transferred to a vacuum distillation device and vacuum distilled at 125 ° C for 1 h to obtain a crude product. 50 mL of deionized water was used to dissolve the obtained crude product. The same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a carbon dot material. 0.3 carbon dot material was weighed and hydrothermally reacted with 3 g of cyanuric acid at 200 ° C for 3 h. After filtering the reaction product, it was washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot composite material.

[0036] Example 6

[0037] 4 g of waste plastic fragments, 20 mL of ethylene glycol and 2 g of thiourea were placed in a reactor, and the reactor was reacted at 275 ° C for 6 h. After the reaction was completed, it was transferred to a vacuum distillation device and vacuum distilled at 125 ° C for 1 h to obtain a crude product. 50 mL of deionized water was used to dissolve the obtained crude product. The same ultrasonic, centrifugal, dialysis and freeze-drying treatment as in Example 1 was used to obtain a carbon dot material. 0.3 carbon dot material was weighed and hydrothermally reacted with 3 g of cyanuric acid at 200 ° C for 3 h. After filtering the reaction product, it was washed three times with deionized water and anhydrous ethanol respectively to obtain a carbon dot composite material.

[0038] In other embodiments of the present invention, the mass ratio of waste plastics, ethylene glycol and auxiliary reactant can also be 1:5:0.2, 1:30:5, 1:45:8 or 1:50:10; any ratio within the range of 1:5-50:0.2-10 can be selected.

[0039] In other embodiments of the present invention, the auxiliary reactant may also be any one of 1,1-dimethylurea, 1,3-dimethylurea, 2-pyrrolidone, tetrahydro-2-pyrimidone, ethyl carbamate, uric acid, urea phosphate or urea.

[0040] The matrix material can also be any one of urea, uric acid, urea phosphate, urea, boron trioxide, silica gel, orthosilicate, molecular sieve, ethyl carbamate, polyvinyl alcohol, polymethyl methacrylate, polyacrylonitrile or polyvinyl pyrrolidone.

[0041] Example 7

[0042] The carbon dot composite materials prepared in Examples 1-3 were subjected to infrared spectroscopy tests. The test results are as follows: Figure 2 As shown by Figure 2 It can be seen that the infrared spectra of the carbon dot composite materials prepared in Examples 1-3 are at 1750 cm -1 There is a characteristic peak of carbonyl (C=O) stretching vibration at 1150cm -1 There is a characteristic peak of CO stretching vibration at 3300cm -1 There is a characteristic peak caused by the stretching vibration of the NH group of the amino group, which proves that the structure of this material contains amino functional groups. -1 There are sp 2 The C=C stretching vibration of the structure is a characteristic peak of graphite, which proves that the material structure has a graphite core structure. That is, the method provided by the present invention can prepare a quasi-spherical carbon dot composite material.

[0043] The photophysical properties of the carbon dot composite materials prepared in Examples 1-6 were tested respectively, and the specific method was as follows: 2 g of the prepared carbon dot composite material was weighed and irradiated with ultraviolet light of wavelengths of 365 nm and 310 nm for 1 s at room temperature respectively; and the afterglow duration of the carbon dot composite material in air and water was tested in a dark room.

[0044] The test results are shown in Table 1;

[0045] Table 1

[0046]

[0047] It can be seen from Table 1 that the carbon dot composite materials prepared in Examples 1-6 can emit light in both air and water after being irradiated with ultraviolet light of different wavelengths, and the afterglow duration in water is shorter than that in air.

[0048] The results of photophysical properties test are as follows Figure 3-8 As shown, Figure 3-8 The photophysical properties of the carbon dot composite materials obtained in Examples 1-6 are shown in the figure below. Figure 3-8 (A) is the afterglow test result of the carbon dot composite material obtained in Examples 1-6 in air, Figure 3-8(B) is the afterglow test result of the carbon dot composite materials prepared in Examples 1-6 in water.

Claims

1. A method for preparing a carbon dot composite material using waste plastics as raw materials, characterized in that: The steps include: S1: Mix waste plastics, a reactant and an auxiliary reactant, heat to 200-300°C and react for 6-12 hours; the reactant is ethylene glycol; the auxiliary reactant is urea or its derivatives; S2: dissolving the reaction product in deionized water, and sequentially subjecting it to ultrasonic treatment, centrifugation, dialysis and freeze drying to obtain a carbon dot material; S3: After mixing the carbon dot material and the matrix material, a hydrothermal reaction is carried out at 50-300° C. for 0.5-12 hours. After the reaction is completed, the product is washed and filtered to obtain a water-resistant carbon dot composite material.

2. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 1, characterized in that: The waste plastics are a combination of one or more of discarded polyolefin materials, aliphatic polyester materials, aromatic polyester materials, polycarbonate, polyurethane, nylon or unsaturated polyester.

3. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 1, characterized in that: The auxiliary reaction agent is urea, 1,1-dimethylurea, 1,3-dimethylurea, tetramethylurea, thiourea, 2-pyrrolidone, tetrahydro-2-pyrimidone, ethyl carbamate, uric acid, urea phosphate or urea.

4. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 1, characterized in that: The mass ratio of the waste plastic, the reactant and the auxiliary reactant is 1:5-50:0.2-10.

5. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 1, characterized in that: The matrix material is a combination of one or more of cyanuric acid, urea, uric acid, urea phosphate, urea thiocyanate, boric acid, boron trioxide, silicon dioxide, silica gel, orthosilicate, hydrotalcite, molecular sieve, ethyl carbamate, polyvinyl alcohol, polymethyl methacrylate, polyacrylonitrile or polyvinyl pyrrolidone.

6. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 5, characterized in that: The mass ratio of the matrix material to the carbon dot material is 0.5-100:

1.

7. The method for preparing a carbon dot composite material using waste plastics as raw materials according to claim 1, characterized in that: A step S110 is further provided between the steps S1 and S2: subjecting the reaction product of S1 to a reduced pressure distillation reaction at 125° C. for 1 hour, and using the product obtained by the reduced pressure distillation reaction to perform S2.