Local ordering method of graphite carbon material, prepared graphite carbon material and application of graphite carbon material in dual-ion battery

By regulating the structure of activated carbon materials at the microscopic level and transforming them into a locally ordered graphite structure, the problem of lower anion storage capacity of traditional graphite positive electrode materials is solved, and the high energy density and power density of graphite positive electrode materials are improved. Improved cycle stability.

CN118929649AActive Publication Date: 2024-11-12SUN YAT SEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410962048.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Traditional graphite positive electrode materials have a low specific capacity to store anions in the high voltage range, which cannot effectively improve the energy density and power density of dual-ion batteries. The existing surface modification methods are complex and costly, and cannot effectively improve the performance of carbon positive electrode materials.

Method used

By regulating the disordered regional structure of activated carbon materials at the microscopic level and transforming them into locally ordered graphite structures, a graphite carbon material with controllable proportions is prepared, increasing the storage site of ions and high-pressure stability. , improves the ion storage capacity and cycle stability of the carbon positive electrode.

Benefits of technology

The specific capacity and energy density of graphite positive electrode material have been significantly improved. The specific capacity of the battery has been increased from 150mAh/g to 240mAh/g, and the energy density has been increased from 350Wh/kg to 630Wh/kg, and the cycle stability has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929649A_ABST
    Figure CN118929649A_ABST
Patent Text Reader

Abstract

The invention discloses a local ordering method of a graphite carbon material, the prepared graphite carbon material and application of the material in a dual-ion battery. The method comprises the following steps: 1) dispersing activated carbon and an eighth group metal salt in water, stirring for 2-24 hours, and uniformly mixing; 2) drying and fully grinding the mixed solution obtained in the step 1) to obtain a precursor, and then roasting and carbonizing in an inert atmosphere; and 3) cooling the product obtained in the step 2), washing with acid and water to remove residual metal particles, and drying to obtain the graphitized carbon positive electrode material. According to the preparation method disclosed by the invention, the internal part of the active carbon is converted into an ordered-disordered structure from a completely disordered structure by regulating and controlling the local micro-area structure of the active carbon, so that the designability of the graphite positive electrode material is improved. According to the preparation method, the ion adsorption mechanism of pore channels in the activated carbon is fully utilized, meanwhile, the anion intercalation capacity of the dual-ion battery in a high-voltage region is increased, and the energy density is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of battery materials, and in particular, relates to a method for locally ordering disordered carbon positive electrode materials, as well as a graphite carbon material prepared thereby and use of the material as a positive electrode material for a dual-ion battery. Background Art

[0002] In order to meet the needs of the national energy strategy, it is necessary to vigorously develop new energy storage devices with high specific energy and fast charging advantages. Thanks to the anion-cation synergistic redox energy storage mechanism, dual-ion batteries using graphite as the positive electrode have the advantages of high operating voltage, excellent power characteristics, and low cost, and have attracted much attention in recent years. However, traditional graphite positive electrode materials have a high voltage range (4.5-5.4V vs.Li + / Li) relies on the intercalation / deintercalation mechanism to store anions, showing a lower specific capacity (~100mAh / g). As a result, compared with traditional lithium-ion batteries, the energy density of dual-ion batteries has no competitive advantage. Therefore, stimulating other energy storage mechanisms in carbon positive electrode materials is the key to improving specific capacity. Lithium-ion capacitors using activated carbon positive electrode materials store charge energy through physical adsorption. Combining the energy storage mechanisms of the two is expected to improve the energy density and power density of dual-ion batteries.

[0003] The prior art focuses on modifying traditional graphite materials at the submicron scale, such as modifying the surface of graphite materials through inert materials such as Al2O3 and TiO2, or using strong oxidants to expand the interlayer spacing of graphite. These technologies have improved the cycle life and rate performance of dual-ion batteries to a certain extent. However, the physical and chemical properties of existing commercially available graphite are stable, its surface is dense, and it is difficult for modified molecules / ions to enter its bulk phase, that is, the structural adjustability of highly graphitized carbon materials is weak, and only surface modification can be performed, so it is impossible to increase the storage sites of ions and improve the specific capacity of the carbon positive electrode. This surface modification method of the prior art does not effectively improve the performance of graphite carbon materials from a microscopic structure, and the above-mentioned prior art preparation process is complicated and the production cost is higher, so it is necessary to develop a carbon positive electrode material with higher capacity and high stability. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to transform the disordered regional structure of the activated carbon material into a locally ordered graphite structure by regulating the disordered regional structure of the activated carbon material at a more microscopic level, thereby obtaining a graphite carbon material with a controllable ratio of the ordered structure part and the disordered structure part, aiming to stimulate the multiple energy storage mechanisms of ions in the positive electrode of the graphite carbon material by increasing the active sites. The ordered graphite structure provides additional anion embedding capacity and high-voltage stability. In addition, the retained disordered structure has good ion adsorption capacity, thereby improving the ion storage capacity of the carbon positive electrode. At the same time, the process of converting the irreversible site into a more stable ion storage site significantly improves the cycle stability of the battery.

[0005] According to one aspect of the present invention, an object of the present invention is to provide a method for preparing a graphite positive electrode material, the method comprising the following steps:

[0006] 1) Disperse the activated carbon and the Group VIII metal salt in water and stir for 2-24 hours to mix evenly;

[0007] 2) drying and fully grinding the mixed solution obtained in step 1) to obtain a precursor, and then calcining and carbonizing it under an inert atmosphere;

[0008] 3) Cooling the product obtained in step 2) and washing it with acid and water to remove residual metal particles, and drying it to obtain a graphitized carbon positive electrode material.

[0009] Preferably, the Group VIII metal salt in step 1) is selected from one or more of potassium ferrocyanide, potassium ferrate, potassium ferric trioxalate, ferric chloride, nickel acetate, and cobalt acetate, preferably potassium ferrocyanide.

[0010] Preferably, in step 1), the weight ratio of the activated carbon to the Group VIII metal salt is 1:0.2 to 1:5, preferably 1:0.5 to 1:3, and more preferably 1:1 to 1:2.

[0011] Preferably, the activated carbon concentration in step 1) is 5 g / L to 70 g / L, preferably 10 g / L to 40 g / L.

[0012] Preferably, the concentration of the Group VIII metal salt in step 1) is 5 g / L to 80 g / L, preferably 10 g / L to 60 g / L.

[0013] Preferably, the drying temperature in step 2) is 70-160°C, preferably 70-100°C.

[0014] Preferably, the drying time in step 2) is 6-24 hours, preferably 10-14 hours.

[0015] Preferably, the calcination carbonization temperature in step 2) is 600-1000°C, preferably 600-800°C, more preferably 750°C.

[0016] Preferably, the heating rate of the calcination carbonization in step 2) is 1-10°C / min, preferably 1-8°C / min, preferably 5°C / min.

[0017] Preferably, the inert atmosphere in step 2) is selected from nitrogen atmosphere or argon atmosphere.

[0018] Preferably, the acid used for washing in step 3) is dilute hydrochloric acid or dilute nitric acid.

[0019] Preferably, the drying temperature in step 3) is 80°C.

[0020] Preferably, the preparation method is carried out as follows: 1.5 g of potassium ferrocyanide is dissolved in 50 ml of deionized water, and then 1 g of activated carbon is added to the solution and dispersed by magnetic stirring for 12 hours. After being placed in an oven at 100 degrees Celsius for 20 hours, the precursor is fully ground to obtain the precursor; the precursor is placed in a tubular furnace and heated to 750°C at 5°C / min, kept warm for 2 hours, and after natural cooling, the residual metal substances are repeatedly washed with dilute hydrochloric acid and deionized water, and the graphitized activated carbon material is obtained after drying in an oven at 80°C.

[0021] According to another aspect of the present invention, another object of the present invention is to provide a graphite positive electrode material prepared by the preparation method of the present invention, wherein the graphite positive electrode material includes an ordered structure and a disordered structure portion, wherein the ordered structure portion accounts for approximately 0-60% of the graphite positive electrode material, and the disordered structure portion accounts for approximately 40-100% of the graphite positive electrode material.

[0022] Preferably, the ordered structure portion in the graphite positive electrode material accounts for about 5-40% of the graphite positive electrode material, and the disordered structure portion accounts for about 50-90% of the graphite positive electrode material.

[0023] More preferably, the ordered structure portion in the graphite positive electrode material accounts for about 10-30% of the graphite positive electrode material, and the disordered structure portion accounts for about 65-85% of the graphite positive electrode material.

[0024] According to another aspect of the present invention, another object of the present invention is to provide use of the graphite positive electrode material as a positive electrode material for a dual ion battery.

[0025] According to another aspect of the present invention, another object of the present invention is to provide a dual-ion battery, wherein the dual-ion battery uses the graphite positive electrode material prepared by the preparation method of the present invention as a positive electrode material.

[0026] Beneficial Effects

[0027] The technical solution according to the present invention has the following advantages:

[0028] 1. The preparation method according to the present invention regulates the local microstructure of activated carbon so that its internal structure is transformed from a completely disordered structure to an ordered-disordered structure, thereby increasing the designability of the graphite positive electrode material.

[0029] 2. The preparation method according to the present invention makes full use of the ion adsorption mechanism of the pores in the activated carbon, and at the same time increases the anion intercalation capacity of the dual-ion battery in the high-voltage region. Therefore, compared with both traditional lithium-ion capacitors and dual-ion batteries, the energy density has been significantly improved. The battery capacity increased from 150 to 240 mAh / g, and the corresponding energy density increased from 350 to 630 Wh / kg. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0031] Figure 1 X-ray diffraction spectra of the graphitized activated carbon material, commercial activated carbon and commercial graphite carbon prepared in Example 1.

[0032] Figure 2 This is the Raman spectrum of commercial activated carbon.

[0033] Figure 3 This is the Raman spectrum of the graphitized activated carbon material prepared in Example 1.

[0034] Figure 4 The Raman spectrum of the graphitized activated carbon material prepared for comparison in Example 2.

[0035] Figure 5 This is the Raman spectrum of the graphitized activated carbon material prepared in Example 2.

[0036] Figure 6 This is the Raman spectrum of commercial graphite material.

[0037] Figure 7 Transmission electron microscope image of commercial activated carbon at low magnification.

[0038] Figure 8 Transmission electron microscope image of commercial activated carbon at high magnification.

[0039] Fig. 9 This is a transmission electron microscope image of the graphitized activated carbon material prepared in Example 1 at low magnification.

[0040] Fig.10 This is a transmission electron microscope image of the graphitized activated carbon material prepared in Example 1 at high magnification.

[0041] Fig.11 The cyclic voltammetry curves of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 1 and the commercial activated carbon positive electrode.

[0042] Fig.12 The charge and discharge curve of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 1.

[0043] Fig.13 This is a comparison chart of the rate performance of dual-ion batteries containing the graphitized activated carbon positive electrode prepared in Example 1.

[0044] Fig.14 This is a test diagram of the cycle stability of a dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 1.

[0045] Fig.15 The figure is a relationship diagram between energy density and power density of a dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 1 and a commercial activated carbon positive electrode.

[0046] Fig.16 The charge and discharge curve diagram of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 2.

[0047] Fig.17 This is a comparison chart of the rate performance of dual-ion batteries containing the graphitized activated carbon positive electrode prepared in Example 2.

[0048] Fig.18 This is a test diagram of the cycle stability of a dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 2.

[0049] Fig.19 The charge and discharge curves of a dual-ion battery containing a commercial activated carbon positive electrode.

[0050] Fig. 20 This is a comparison chart of the rate performance of dual-ion batteries containing commercial activated carbon positive electrodes.

[0051] Fig.21 This is a graph showing the cycling stability test of a dual-ion battery containing a commercial activated carbon positive electrode.

[0052] Fig. 22 The charge and discharge curve diagram of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Comparative Example 2.

[0053] Fig.23 This is a comparison chart of the rate performance of a dual-ion battery containing a graphitized activated carbon positive electrode prepared in Comparative Example 2.

[0054] Fig.24 This is a test diagram of the cycle stability of a dual-ion battery containing the graphitized activated carbon positive electrode prepared in Comparative Example 2.

[0055] Fig.25 The charge and discharge curves of a dual-ion battery containing a commercial graphite carbon positive electrode.

[0056] Fig.26 This is a comparison chart of the rate performance of dual-ion batteries containing commercial graphite carbon positive electrodes.

[0057] Fig. 27 This is a graph showing the cycling stability test of a dual-ion battery containing a commercial graphite carbon positive electrode. DETAILED DESCRIPTION

[0058] Hereinafter, the present invention will be described in detail. Before describing, it should be understood that the terms used in this specification and the appended claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the present invention on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the descriptions presented here are only preferred examples for illustrative purposes and are not intended to limit the scope of the present invention, so that it should be understood that other equivalents or improvements can be obtained therefrom without departing from the spirit and scope of the present invention.

[0059] In this document, the terms "include", "including", "have", "contain" or any other similar terms are open conjunctions, which are intended to cover non-exclusive inclusions. For example, a composition or product containing multiple elements is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or product. In addition, unless otherwise explicitly stated, the term "or" refers to an inclusive "or" rather than an exclusive "or". For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and A and B are both true (or exist). In addition, in this document, the interpretation of the terms "include", "including", "have", and "contain" should be considered to have been specifically disclosed and simultaneously cover closed or semi-closed conjunctions such as "consisting of" and "consisting essentially of".

[0060] In this article, all features or conditions defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible secondary ranges and individual values ​​within the range, especially integer values. For example, the range description of "1 to 8" should be deemed to have specifically disclosed all secondary ranges such as 1 to 7, 2 to 8, 2 to 6, 3 to 6, 4 to 8, 3 to 8, etc., especially secondary ranges defined by all integer values, and should be deemed to have specifically disclosed individual values ​​such as 1, 2, 3, 4, 5, 6, 7, 8, etc. within the range. Unless otherwise specified, the above interpretation method applies to all contents of the entire present invention, regardless of whether the range is broad or not.

[0061] If the quantity or other numerical value or parameter is expressed as a range, a preferred range or a series of upper and lower limits, it should be understood that all ranges consisting of any upper limit or preferred value of the range and the lower limit or preferred value of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.

[0062] In this document, under the premise of achieving the purpose of the invention, numerical values ​​should be understood to have the accuracy of the number of significant digits of the numerical value. For example, the number 40.0 should be understood to cover the range from 39.50 to 40.49.

[0063] In addition, unless otherwise stated, the reagents and solvents disclosed below are purchased from Dongguan Kelude Experimental Equipment Technology Co., Ltd. X-ray diffraction (XRD) was tested using an X-ray diffractometer of model D-MAX 2200VPC; and Raman spectroscopy was tested using a Raman spectrometer of model inVia; TEM was tested using a transmission electron microscope of model F30. The constant current charge-discharge battery test of the dual-ion battery was carried out on a Blue Electric Battery Test System (CT002A); the cyclic voltammetry curve was collected by a CHI760E electrochemical workstation. The ratio of ordered and disordered structures in carbon materials is obtained by fitting the D band (representing disordered structure) and G band (representing ordered structure) peak areas of the carbon material in the Raman spectrum, and performing normalized calculations.

[0064] The following examples are only listed as examples of embodiments of the present invention and do not constitute any limitation to the present invention. It can be understood by those skilled in the art that modifications within the scope of the essence and concept of the present invention fall within the scope of protection of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples are all commercially available products.

[0065] Example 1

[0066] 1.5 g of potassium ferrocyanide (purchased from Shanghai McLean Co., Ltd.) was dissolved in 50 ml of deionized water, and then 1 g of activated carbon was added to the solution and dispersed by magnetic stirring for 12 hours. After being placed in an oven at 100°C for 20 hours, the precursor was fully ground. The precursor was placed in a tubular furnace and heated to 750°C at 5°C / min, kept warm for 2 hours, and after naturally cooling, it was repeatedly washed with dilute hydrochloric acid and deionized water to remove residual metal substances, and then dried in an oven at 80°C to obtain a graphitized activated carbon material.

[0067] Figure 1 The XRD spectra of the graphite positive electrode material prepared in this embodiment, the existing commercial activated carbon (XFP01, purchased from Nanjing Pioneer Nanomaterial Technology Co., Ltd.) and the commercial graphite carbon (KS-6, purchased from Dongguan Kelude Experimental Equipment Technology Co., Ltd.) show that the carbon material prepared in this embodiment has good crystallinity, indicating that the prepared carbon material contains an ordered structure. However, compared with commercial graphite, its intensity is weaker and the half-width peak is wider, indicating that the carbon material also has a disordered structure (i.e., defects in the carbon material).

[0068] Example 2

[0069] Compared with Example 1, the carbonization temperature was changed to 850°C, and other conditions remained unchanged. Figure 5 It was calculated from the Raman spectrum that the ordered structure of the carbon material prepared in this embodiment accounted for 18%, while the corresponding disordered structure accounted for 82%.

[0070] Comparative Example 1

[0071] Commercial activated carbon was used as a comparison. Figure 1 In the XRD spectrum of commercial activated carbon, it can be seen that the diffraction peaks are broad and weak, indicating that the crystallinity is low and the carbon atoms are arranged in a disordered manner. Figure 2 In the Raman spectrum of activated carbon, the ordered structure accounts for 13.3%, while the disordered structure accounts for as high as 86.7% (obtained by calculating their peak areas), which is the most disordered among several carbon materials. Figure 7 and Figure 8 These are transmission electron microscope images of commercial activated carbon at different magnifications. It can also be observed that the carbon atoms in commercial activated carbon are arranged in a disordered manner.

[0072] Comparative Example 2

[0073] Compared with Example 1, the carbonization temperature was changed to 650°C, and other conditions remained unchanged. Figure 3 It was calculated from the Raman spectrum that the ordered structure of the carbon material prepared in Comparative Example 2 accounted for 14.6%, while the corresponding disordered structure accounted for 85.4%.

[0074] Comparative Example 3

[0075] This comparative example 3 directly uses commercial graphite material (KS-6) as a comparison. Figure 1 From the XRD spectrum of commercial graphite material, it can be seen that the commercial graphite material has a strong diffraction peak and a narrow half-width peak, indicating that it has a higher degree of crystallinity. Figure 6 This is the Raman spectrum of commercial graphite material. From the figure, we can observe that there is a strong G peak in the Raman spectrum of commercial graphite material, indicating that there are more ordered carbon atom structures inside the material. By calculating the peak area, it can be obtained that the disordered structure accounts for 58% and the corresponding ordered structure accounts for 42%. It is the most ordered one among the above-mentioned carbon materials.

[0076] Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 They are Raman spectra of commercial activated carbon, graphitized activated carbon material prepared in Example 1, graphitized activated carbon material prepared in Comparative Example 2, graphitized activated carbon material prepared in Example 2, and commercial graphite carbon material. Figure 4 From the areas of the D and G bands in the Raman spectrum, it can be calculated that the ordered structure of the graphitized activated carbon material prepared in this embodiment accounts for 16%, and the corresponding disordered structure accounts for 84%. Figure 7 and Figure 8 Transmission electron microscope images of commercial activated carbon at different magnifications. Fig. 9 and Fig.10 This is a high-resolution transmission electron microscope image of the graphitized activated carbon positive electrode material prepared in Example 1. Figure 7 , Figure 8 and Fig. 9 , Fig.10 From the comparison, it can be seen that after regulation, the carbon atoms inside the activated carbon are transformed from a completely disordered structure to an ordered-disordered mixed structure.

[0077] Test Example 1

[0078] Preparation of dual-ion battery positive electrode:

[0079] According to the conventional electrode preparation method in the art, the positive electrode materials in Examples 1 and 2 and Comparative Examples 1 to 3 were mixed with the conductive agent super P and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 in N-methylpyrrolidone (NMP) solvent, and then evenly coated on aluminum foil by blade coating. After being fully dried in a vacuum oven at 80°C for 12 hours, it was cut directly into 10 mm discs to obtain positive electrode sheets. The loading amount of active material was 1.5±0.3 mg / cm2 .

[0080] Assembly of dual-ion battery:

[0081] In the R2032 button cell, the dual-ion battery positive electrode prepared above, the Li single negative electrode with a diameter of 14mm, and the separator are glass fiber (GF / D), and 150μL of electrolyte (4M LiPF6 / EMC) are added and the battery is encapsulated with a pressure of 50kPa. All dual-ion batteries need to be left to stand for 12h before electrochemical testing, and the voltage window is 1.5-5.1V. Charge / discharge tests were performed at current densities of 200, 400, 600, 800 and 1000mA / g to evaluate the rate performance of the dual-ion battery, and long-cycle stability tests were performed at a current density of 1A / g.

[0082] Fig.11 The cyclic voltammetry curve of the dual-ion battery containing commercial activated carbon and the graphitized activated carbon positive electrode in Example 1 is shown in FIG. Fig.11 From the comparison in , it can be seen that the graphitized activated carbon positive electrode prepared in Example 1 exhibits a pair of redox peaks in the high-voltage region, while no similar electrochemical behavior occurs in the commercial activated carbon positive electrode, indicating that anion insertion / extraction reactions occur in the graphitized activated carbon positive electrode. Fig.12 is the charge-discharge curve of the dual-ion battery containing the graphitized activated carbon positive electrode in Example 1, from Fig.12 It can be seen that the battery has a specific capacity of up to 240 mAh / g at a current density of 200 mA / g, and can still release a specific capacity of 95 mAh / g at 1000 mA / g, indicating that the graphite material prepared in Example 1 has excellent anion storage capacity. Fig.13 The rate performance diagram of the dual-ion battery containing the graphitized activated carbon positive electrode in Example 1 is shown in FIG. Fig.13 It can be seen that the graphitized activated carbon positive electrode material prepared in Example 1 has good rate performance and reversible performance. Fig.14 The cycle performance diagram of the dual-ion battery containing the graphitized activated carbon positive electrode in Example 1 is shown in FIG. Fig.14 It can be seen that after 600 charge and discharge tests, the capacity of the battery slowly decays to 82 mAh / g, indicating that the graphitized activated carbon positive electrode has good cycle stability. Fig.15 The energy density and power density of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 1 and the commercial activated carbon positive electrode are compared. Fig.15It can be seen that when the power density is 530 W / kg, the energy density can reach 630 Wh / kg (the energy density of the commercial activated carbon positive electrode is only 350 Wh / kg). Even at 2850 W / kg, it can still release an energy density of up to 268 Wh / kg, indicating that the dual-ion battery containing the graphitized activated carbon positive electrode in Example 1 has good power-energy characteristics.

[0083] Fig.16 and Fig.17 is the charge-discharge curve of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Example 2, from Fig.16 and Fig.17 It can be seen that the battery has a specific capacity of 165mAh / g at a current density of 200mA / g, and a specific capacity of 76mAh / g at 1000mA / g, indicating good rate performance and good ion storage capacity. In addition, after undergoing a high current test, the battery specific capacity recovered to more than 90% of the original, indicating that the graphite positive electrode prepared in Example 2 has good reversible performance. At the same time, from Fig.18 From the long cycle curve in FIG, the capacity of the dual-ion battery containing the graphitized activated carbon positive electrode in Example 2 decays slowly to 56 mAh / g after 600 cycles.

[0084] Fig.19 and Fig. 20 The charge-discharge curves of dual-ion batteries containing commercial activated carbon are shown in Figure 2. Fig.19 and Fig. 20 It can be seen from the rate test that the battery has a specific capacity of 114mAh / g at a current density of 200mA / g, and a specific capacity of 20mAh / g at 1000mA / g, indicating that the battery's rate performance is poor. In addition, after undergoing a high current test, the battery's specific capacity cannot be restored, and is even less than 50% of the original. At the same time, it can be observed that when the activated carbon positive electrode is tested at a low rate, the battery capacity decays rapidly. Fig.21 The cycle stability test diagram of the dual-ion battery containing commercial activated carbon positive electrode is shown in Figure 2. Fig.21 From the long cycle curve in Figure 2, the specific capacity of the dual-ion battery containing commercial activated carbon cathode decays rapidly to 48 mAh / g after 600 cycles, indicating that there are many irreversible defect sites (disordered structure) in the carbon material, which will lead to a decrease in battery reversibility. These data show that the overall electrochemical performance is poor.

[0085] Fig. 22 and Fig.23 The charge-discharge curve of the dual-ion battery containing the graphitized activated carbon positive electrode in Comparative Example 2 is shown in FIG. Fig. 22 and Fig.23It can be seen that the battery has a specific capacity of 158mAh / g at a current density of 200mA / g, and a specific capacity of 55mAh / g at 1000mA / g. In addition, after undergoing a high current test, the battery specific capacity cannot be restored, and is even less than 70% of the original; it can also be observed that the battery capacity decays rapidly when the battery is tested at a low rate. In addition, Fig.24 The cycle stability test diagram of the dual-ion battery containing the graphitized activated carbon positive electrode prepared in Comparative Example 2 is shown in FIG. Fig.24 From the long cycle curve in , the specific capacity of the dual-ion battery containing the graphitized activated carbon positive electrode in Comparative Example 2 decays to 52 mAh / g after 600 cycles, indicating that the graphitized activated carbon positive electrode material in Comparative Example 2 still has many irreversible defect sites.

[0086] Fig.25 and Fig.26 The charge-discharge curve of the dual-ion battery with commercial graphite cathode is shown in Figure 2. Fig.25 and Fig.26 It can be seen that the battery has a specific capacity of 102mAh / g at a current density of 200mA / g, which is the lowest among several positive materials. This is due to the limited ion storage sites inside the graphite. The specific capacity is 43mAh / g at 1000mA / g, indicating that the narrow ion transport channels in the graphite affect the rate performance. In addition, Fig. 27 This is a test diagram of the cycle stability of a dual-ion battery containing a commercial graphite carbon positive electrode. Fig. 27 Judging from the long cycle curve in the figure, the dual-ion battery containing commercial graphite positive electrode has good cycle stability. After 600 charge-discharge cycles, the capacity is 52mAh / g, which is related to its fewer internal defects and better oxidation resistance.

[0087] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a graphite positive electrode material, the method comprising the following steps: 1) Disperse the activated carbon and the Group VIII metal salt in water and stir for 2-24 hours to mix evenly; 2) drying and fully grinding the mixed solution obtained in step 1) to obtain a precursor, and then calcining and carbonizing it under an inert atmosphere; 3) Cooling the product obtained in step 2) and washing it with acid and water to remove residual metal particles, and drying it to obtain a graphitized carbon positive electrode material.

2. The preparation method according to claim 1, characterized in that: Preferably, the Group VIII metal salt in step 1) is selected from one or more of potassium ferrocyanide, potassium ferrate, potassium ferric trioxalate, ferric chloride, nickel acetate, and cobalt acetate, preferably potassium ferrocyanide; Preferably, in step 1), the weight ratio of the activated carbon to the Group VIII metal salt is 1:0.2 to 1:5, preferably 1:0.5 to 1:3, and more preferably 1:1 to 1:2; Preferably, the activated carbon concentration in step 1) is 5 g / L to 70 g / L, preferably 10 g / L to 40 g / L; Preferably, the concentration of the Group VIII metal salt in step 1) is 5 g / L to 80 g / L, preferably 10 g / L to 60 g / L.

3. The preparation method according to claim 1, characterized in that: Preferably, the drying temperature in step 2) is 70-160°C, preferably 70-100°C; Preferably, the drying time in step 2) is 6-24 hours, preferably 10-14 hours; Preferably, the calcination carbonization temperature in step 2) is 600-1000°C, preferably 600-800°C, more preferably 750°C; Preferably, the heating rate of the calcination carbonization in step 2) is 1-10°C / min, preferably 1-8°C / min, preferably 5°C / min; Preferably, the inert atmosphere in step 2) is selected from nitrogen atmosphere or argon atmosphere.

4. The preparation method according to claim 1, characterized in that: Preferably, the acid used for washing in step 3) is dilute hydrochloric acid or dilute nitric acid; Preferably, the drying temperature in step 3) is 80°C.

5. The preparation method according to claim 1, characterized in that: The preparation method is as follows: 1.5 g of potassium ferrocyanide is dissolved in 50 ml of deionized water, and then 1 g of activated carbon is added to the solution and dispersed by magnetic stirring for 12 hours. After being placed in an oven at 100 degrees Celsius for 20 hours, the precursor is fully ground to obtain the precursor; the precursor is placed in a tubular furnace and heated to 750 degrees Celsius at 5 degrees Celsius / min, kept warm for 2 hours, and after natural cooling, the residual metal substances are repeatedly washed with dilute hydrochloric acid and deionized water, and the graphitized activated carbon material is obtained after drying in an oven at 80 degrees Celsius.

6. A graphite positive electrode material prepared according to the preparation method according to any one of claims 1 to 5, wherein the graphite positive electrode material comprises an ordered structure and a disordered structure portion, wherein the ordered structure portion accounts for approximately 0-60% of the graphite positive electrode material, and the disordered structure portion accounts for approximately 40-100% of the graphite positive electrode material.

7. The graphite positive electrode material according to claim 6, characterized in that Preferably, the ordered structure portion in the graphite positive electrode material accounts for about 5-40% of the graphite positive electrode material, and the disordered structure portion accounts for about 50-90% of the graphite positive electrode material.

8. The graphite positive electrode material according to claim 7, characterized in that More preferably, the ordered structure portion in the graphite positive electrode material accounts for about 10-30% of the graphite positive electrode material, and the disordered structure portion accounts for about 65-85% of the graphite positive electrode material.

9. Use of the graphite positive electrode material according to claim 7 or 8 as a positive electrode material for a dual ion battery.

10. A dual-ion battery, wherein the dual-ion battery uses the graphite positive electrode material prepared according to any one of claims 1 to 5 as a positive electrode material.

Citation Information

Patent Citations

  • Preparation method for synthesizing graphite porous carbon material with activated carbon serving as raw material

    CN103318871A

  • Preparation method of double-ion battery using hard carbon cathode material

    CN107634225A

  • Method for preparing capacitor active carbon with high volume energy density

    CN108373155A