Silicon plate for bulletproof flashboard reaction and preparation method thereof

The silicon plate is made by low-temperature curing of graphite-coated silicon particles, which solves the problems of uneven spreading of silicon particles and complex high-temperature treatment in the bulletproof insert plate silicon seepage process, and achieves the uniformity and stability of the silicon seepage reaction, reducing the Production costs and deformation risks.

CN118929666APending Publication Date: 2024-11-12HENAN UNION ABRASIVES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411107935.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing bulletproof silicon seepage process has problems such as low production efficiency and uneven spread of silicon particles, resulting in insufficient reaction, possible cracking or deformation. High-temperature silicon seepage treatment requires high temperature uniformity of the equipment, complex operation, and increased production. cost.

Method used

The silicon particles coated with graphite are cured by low temperature to make a silicon plate. The graphite slurry is mixed with the silicon particles and dried to form a graphite layer. The silicon plate is cured at low temperature to make it used for silicon permeation treatment to ensure uniform distribution of silicon particles and sufficient reaction. .

Benefits of technology

It improves the uniformity and stability of the silicon permeability reaction, reduces the waste of silicon particles, reduces production costs, avoids black core phenomena and sample deformation, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929666A_ABST
    Figure CN118929666A_ABST
Patent Text Reader

Abstract

The invention provides a silicon plate for bulletproof flashboard reaction and a preparation method thereof, the silicon plate is prepared by mixing graphite-coated silicon particles and a thickening agent to prepare modified silicon particles, and pressing and low-temperature curing the modified silicon particles, the graphite-coated silicon particles are prepared by mixing graphite slurry and silicon particles, enabling the graphite slurry to be adhered to the surfaces of the silicon particles and then drying; the graphite slurry is prepared by mixing a homogenizing agent, pure water and graphite. Graphite covers the surfaces of silicon particles in a manner of mixing a homogenizing agent and water to form a graphite layer, the silicon particles preferentially react with the graphite during high-temperature reaction to generate a layer of silicon carbide shells to trap the silicon particles in the silicon particles, the silicon carbide shells are broken through when the temperature continues to rise to the gasification temperature of the silicon particles, silicon steam is released, and the silicon particles are separated from the silicon steam. When the silicon steam reacts with a sample, the phenomenon that a siliconizing channel is blocked by silicon carbide generated by reaction of low-temperature liquid silicon and a blank can be avoided, and the phenomenon of a black core is avoided; the silicon plate is prepared through low-temperature curing, so that the requirement for equipment temperature uniformity is low during siliconizing treatment of the bulletproof flashboard; and the pressed silicon plate can reduce the operation time for workers to spread silicon particles, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diamond detection, and in particular to a silicon plate for bulletproof plug-in plate reaction and a preparation method thereof. Background Art

[0002] Ceramic composite materials have good performance because they combine the advantages of reinforcing materials and matrix. They are also the fastest-growing and most promising bulletproof materials. Bulletproof materials are gradually developing towards diversification and composites, and various new bulletproof materials with high hardness and high toughness have emerged to cope with more complex protection problems. Ceramic bulletproof substrates are lighter in weight and have better mechanical properties than metal bulletproof substrates of the same volume.

[0003] The existing siliconization process of bulletproof inserts is to first arrange a part of the silicon particles on the support plate and then place the porous green body steadily on the silicon particles and then sprinkle another layer of silicon particles on the green body. After the combination is completed, it is transferred into the crucible. Put the prepared porous green body into the furnace and start heating. During the heating process, liquid silicon and gaseous silicon will continuously enter the green body and react with the carbon inside the green body to form silicon carbide. The excess silicon will fill the sample and finally remain inside the sample when the temperature is lowered. In summary, a dense and high-strength silicon carbide composite material is produced.

[0004] This vapor phase siliconization method has the following disadvantages: 1. When assembling the support plate, silicon particles, and blanks, it is necessary to weigh the required silicon particles first and then spread them on the support plate as evenly as possible. In this process, a lot of time will be wasted due to spreading the silicon particles, resulting in low production efficiency; 2. When spreading silicon particles on the blank, it is inevitable that the thickness will be uneven due to manual placement. When the thickness of the silicon particles is uneven, the silicon particles in the thinner part have been reacted completely during the reaction process, but there are still surplus silicon particles in the thicker part, which may lead to insufficient reaction in the thinner part, and the sample cannot be completely dense, and even cracking and deformation. After the reaction, the silicon particles in the thicker part will adhere to the sample and are difficult to handle, increasing production costs; 3. Because the support plate is curved, the amount of silicon particles at the edge will be less than that in the middle, which will lead to insufficient reaction, cracking and deformation at the edge of the blank during high-temperature siliconization reaction; 4. When the assembled product is transported into the crucible and the crucible is placed in the furnace, the silicon particles at the edge of the sample may fall off due to vibration, thereby aggravating the unevenness of the silicon particles at the edge of the sample. 5. During the heating process, the silicon particles change from solid to liquid and then to gas. The liquid silicon is able to react with the porous body to generate silicon carbide. As time goes by, the silicon carbide generated at low temperature occupies the reaction channel and even blocks the reaction channel, making it impossible for the porous body to react completely, resulting in a black core.

[0005] A Chinese invention patent with a publication date of 2021.12.10 and publication number of CN 113773094 A discloses a method for treating silicon powder for melt siliconization, in which silicon powder is reacted with carbon or nitrogen as a reactive substance at a high temperature of 1200℃ to 1500℃ to form a thin shell on the surface of the silicon powder; when the reactive substance is carbon, a silicon carbide shell is formed on the surface of the silicon powder, and when the reactive substance is nitrogen, a silicon nitride shell is formed on the surface of the silicon powder. The patent for the method for treating silicon powder for melt siliconization pre-treats the silicon powder to form a thin shell on its surface, and utilizes the volume change effect during its melting and heating process to allow the silicon to break the shell and quickly enter the porous body.

[0006] However, the modification method adopted in the patent is high-temperature modification, which generates a silicon carbide or silicon nitride shell on the surface of silicon powder by introducing gas at high temperature. This production method has very high requirements for the uniformity of the temperature inside the furnace and is complicated to operate. If the temperature is too high, the silicon vapor will break through the silicon carbide shell, and if the temperature is too low, a complete covering shell cannot be generated; in addition, a large amount of energy is consumed in the process of heating and cooling.

[0007] In order to reduce production costs, improve production efficiency, and solve the problems in the siliconization process of the bulletproof insert, the present invention proposes a novel silicon plate used in the siliconization reaction of the bulletproof insert and a method for preparing the silicon plate. Summary of the invention

[0008] In view of the above technical problems, the present invention proposes a silicon plate for bulletproof plug plate reaction and a preparation method thereof, which is used to solve the problem that the siliconization treatment in the prior art has high requirements for the temperature uniformity of the equipment and the temperature control process is complicated. The siliconization reaction of the present invention adopts a silicon plate obtained by low-temperature curing, so that the bulletproof plug plate has low requirements for the temperature uniformity of the equipment during the siliconization treatment, and the silicon plate of the present invention makes the porous blank react completely, with small deformation, no cracking, and high stability, reducing the waste of silicon particles and improving production efficiency.

[0009] In order to achieve the above object, the technical solution of the present invention is achieved as follows: A silicon plate for bulletproof plug plate reaction, wherein the silicon plate is prepared by mixing graphite-coated silicon particles with a thickener to obtain modified silicon particles, and the modified silicon particles are pressed and cured at low temperature.

[0010] Furthermore, the graphite-coated silicon particles are prepared by mixing graphite slurry with silicon particles and allowing the graphite slurry to adhere to the surface of the silicon particles and then drying.

[0011] Furthermore, the graphite slurry is prepared by mixing a homogenizer, pure water and graphite.

[0012] The present invention covers the surface of silicon particles with graphite by mixing a homogenizer and water to form a graphite layer. During a high-temperature reaction, the silicon particles will preferentially react with the graphite to generate a silicon carbide shell to imprison the silicon particles inside. When the temperature continues to rise to reach the gasification temperature of the silicon particles, the silicon carbide shell is broken to release silicon vapor. When the silicon vapor reacts with the sample, the phenomenon of blocking the silicon infiltration channel due to the reaction of low-temperature liquid silicon with the blank to generate silicon carbide can be avoided, thereby avoiding the occurrence of a black core phenomenon.

[0013] The method for preparing a bulletproof plug-in plate reaction silicon plate comprises the following steps: A1. Mix a homogenizing agent, pure water and graphite to prepare a graphite slurry; A2, mixing the graphite slurry with the silicon particles, making the graphite adhere to the surface of the silicon particles, and obtaining the graphite-coated silicon particles by drying; A3, mixing the graphite-coated silicon particles obtained in step S2 with a thickener to obtain modified silicon particles; A4, pressing the modified silicon particles into a silicon plate embryonic body having the same appearance as the porous embryonic body through a mold; A5. The silicon plate blank pressed in step S4 is transferred into an oven through a support plate, and a silicon plate is obtained by low-temperature curing.

[0014] Furthermore, the method further comprises the following steps: A6. Use silicon plates for siliconization treatment of bulletproof inserts.

[0015] Furthermore, in order to produce a better silicon plate and achieve a better siliconizing effect during siliconizing, the particle size of the silicon particles is 0.5 mm-3 mm.

[0016] Furthermore, in order to prepare better modified silicon particles from the graphite-coated silicon particles, the thickener includes graphite emulsion or resin slurry.

[0017] Furthermore, in order to achieve a better homogenization effect when pure water and graphite are mixed, the homogenizer includes alcohol or ethylene glycol.

[0018] Furthermore, in order to obtain better modified silicon particles, the mixing ratio of the thickener to the graphite-coated silicon particles in step S3 is 1-1.8:9-11.

[0019] Furthermore, in order to achieve a better pressing effect, the pressing pressure in step S4 is 20-30 MPa, and the pressing time is 100-150 s.

[0020] Beneficial effects of the present invention: 1. In the present invention, graphite is covered on the surface of silicon particles by a mixture of a homogenizer and water to form a graphite layer. During high-temperature reaction, the silicon particles will preferentially react with the graphite to generate a layer of silicon carbide shell to imprison the silicon particles inside. When the temperature continues to rise to the gasification temperature of the silicon particles, the silicon carbide shell is broken to release silicon vapor. When the silicon vapor reacts with the sample, the phenomenon of blocking the silicon infiltration channel due to the reaction of low-temperature liquid silicon with the blank to generate silicon carbide can be avoided, thereby avoiding the occurrence of black core phenomenon. 2. The present invention evenly distributes the pre-weighed silicon particles through a distributor, and then cold-presses them on a hydraulic press to form a silicon plate, which can ensure that the thickness of each position of the silicon plate is completely consistent, making up for the disadvantage of artificial spreading of silicon particles, so that the sample will not have a reaction difference due to the difference in silicon amount during the siliconization reaction; 3. The silicon particles after mixing and the silicon plates after curing of the present invention can be stored for a long time; when the silicon plates are used for assembly, the assembly efficiency can be significantly increased, thereby improving the production efficiency and reducing the production cost in disguised form; 4. The present invention provides a silicon plate, which can prevent silicon particles at the edge of the sample from falling due to vibration or human factors during placement and transportation, thereby affecting the uniformity of siliconization at the edge and inside of the sample. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is a schematic diagram of the use of the silicon plate of the present invention.

[0023] In the figure: 1. silicon plate, 2. porous green body, 3. support plate. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The invention discloses a silicon plate for bulletproof plug plate reaction. The silicon plate is prepared by mixing graphite-coated silicon particles with a homogenizing agent, resin and pure water to obtain modified silicon particles, and then pressing and low-temperature curing the modified silicon particles.

[0026] Furthermore, the graphite-coated silicon particles are prepared by mixing graphite slurry with silicon particles and allowing the graphite slurry to adhere to the surface of the silicon particles and then drying.

[0027] Furthermore, the graphite slurry is prepared by mixing a homogenizer, pure water and graphite.

[0028] The method for preparing a bulletproof plug-in plate reaction silicon plate comprises the following steps: A1. Mix a homogenizing agent, pure water and graphite to prepare a graphite slurry; A2, mixing the graphite slurry with the silicon particles, making the graphite adhere to the surface of the silicon particles, and obtaining the graphite-coated silicon particles by drying; A3, mixing the graphite-coated silicon particles obtained in step S2 with a thickener to obtain modified silicon particles; A4, pressing the modified silicon particles into a silicon plate embryonic body having the same appearance as the porous embryonic body through a mold; A5. The silicon plate blank pressed in step S4 is transferred into an oven through a support plate, and a silicon plate is obtained by low-temperature curing.

[0029] Furthermore, the method further comprises the following steps: A6. Finally, the silicon plate and the porous green body are assembled for siliconization treatment of the bulletproof insert.

[0030] Furthermore, the particle size of the silicon particles is 0.5 mm-3 mm.

[0031] Furthermore, the thickener includes graphite emulsion or resin slurry.

[0032] Furthermore, the homogenizing agent includes alcohol or ethylene glycol.

[0033] Furthermore, in step S3, the mixing ratio of the thickener to the graphite-coated silicon particles is 1-1.8:9-11.

[0034] Furthermore, in step S4, the pressing pressure is 20-30 MPa, and the pressing time is 100-150 s.

[0035] Example 1 Prepare a 20% alcohol solution, take 200g of alcohol solution and 150g of graphite and put them into a blender, and stir for 30 minutes. Put the obtained graphite, alcohol solution and 1L of pure water into a stirring barrel, add 10kg of 1-3mm silicon particles and start stirring for 30 minutes. The purpose of this step is to use wet mixing to better wrap the graphite on the surface of the silicon particles. Adding alcohol can improve the uniformity of graphite in the solution. Pour the obtained slurry into a bucket and then put it into an oven to dry at 100℃-120℃ to obtain graphite-coated silicon particles.

[0036] Take 150g of alcohol and 300g of thermosetting phenolic resin and ultrasonicate for 30 minutes to obtain 450g of resin solution. The obtained resin solution is mixed with graphite emulsion and the above-made graphite-coated silicon particles in the proportion of 4:6:90, and the mixing method is stirring for 30 minutes. Among them, the role of the resin solution is to solidify the silicon plate after pressing so that it has a certain strength, and the graphite emulsion is used as a thickener to make the graphite-coated silicon particles obtain very viscous modified silicon particles. The modified silicon particles can react with the coated layer of graphite to form a silicon carbide shell during the heating process, imprisoning the liquid silicon inside. When the temperature continues to rise, the liquid silicon is converted into silicon vapor and then breaks through the silicon carbide shell to react with the sample, ensuring that the silicon vapor reacts with the sample, compensating for the black core condition that may be caused by liquid silicon infiltration.

[0037] Weigh the required modified silicon particles and put them into the distributor, and evenly distribute them into the mold through the distributor. Press them into the shape of a porous green body at 25MPa for 120s. At this time, quickly transfer the silicon plate to the support plate and put it into the oven. After curing at 150℃-170℃ for 1h, a silicon plate with a certain strength is obtained.

[0038] The prepared silicon plate is used in the siliconization process of the bulletproof plug plate. The silicon plate is assembled with the porous blank. The silicon plate obtained by pressing and curing can effectively avoid the occurrence of silicon particles spilling and the inconsistency between the amount of silicon particles around the sample and inside the sample in the process of loading into the furnace. The bulletproof plug plate after siliconization treatment can be clearly seen to have excellent internal uniformity and no black core through X-ray observation.

[0039] The density of the bulletproof plug plate made by this embodiment 1 can reach more than 99%; the three-point bending strength of the bulletproof plug plate is between 360-380MPa; the hardness of the bulletproof plug plate is 90-94HRA; the maximum pore size when fitted with the standard sample is within 0.5mm, and the cracking rate of the sample is less than 1%.

[0040] The silicon plate prepared in this embodiment can improve the uniformity of silicon infiltration, reduce the degree of deformation and cracking of the sample, and can also eliminate the operation time of workers spreading silicon particles, thereby improving production efficiency and reducing production costs.

[0041] Example 2 100g graphite, 750g pure water, 250g alcohol, and 10kg 2mm-3mm silicon particles are added to a stirring barrel. The order of adding materials can be changed. Then start stirring for 0.5-1h. Pour the obtained slurry into a tray and put it into an oven at 100℃-120℃ for drying to obtain silicon particles coated with graphite.

[0042] 150g of alcohol and 850g of thermosetting resin are placed in a stirring device and stirred for 0.5-1h to obtain 1kg of viscous resin slurry. 10kg of the silicon particles coated with graphite prepared above are mixed with 1kg of the viscous resin slurry obtained and stirred for 40min to finally obtain viscous modified silicon particles.

[0043] The modified silicon particles can react with a layer of graphite to form a silicon carbide shell during the heating process, thereby trapping the liquid silicon inside. When the temperature continues to rise, the liquid silicon is converted into silicon vapor and then breaks through the silicon carbide shell to react with the sample, ensuring that it is silicon vapor that reacts with the sample, thereby compensating for the black core condition that may be caused by liquid silicon infiltration.

[0044] Weigh the required modified silicon particles and put them into the distributor, and evenly distribute them into the mold through the distributor. Press them into the shape of a porous green body at 30MPa for 180s. At this time, quickly transfer the silicon plate to the support plate and put it into the oven. After curing at 150℃-170℃ for 0.5h, a silicon plate with a certain strength is obtained.

[0045] The prepared silicon plate is used in the siliconization process of the bulletproof plug plate. The silicon plate is assembled with the porous blank. The silicon plate obtained by pressing and curing can effectively avoid the occurrence of silicon particles spilling and the inconsistency between the amount of silicon particles around the sample and inside the sample in the process of loading into the furnace. The bulletproof plug plate after siliconization treatment can be clearly seen to have excellent internal uniformity and no black core through X-ray observation.

[0046] The density of the bulletproof plug plate made by this embodiment 2 can reach more than 98%; the three-point bending strength of the bulletproof plug plate is between 350-380 MPa; the hardness of the bulletproof plug plate is 90-94 HRA; the maximum pore between the bulletproof plug plate and the standard sample is within 0.4 mm, and the sample cracking rate is less than 0.5%.

[0047] The silicon plate prepared in this embodiment can improve the uniformity of silicon infiltration, reduce the degree of deformation and cracking of the sample, and can also eliminate the operation time of workers spreading silicon particles, thereby improving production efficiency and reducing production costs.

[0048] Example 3 Add 200g of graphite, 500g of pure water, 500g of ethylene glycol, and 10kg of 0.5-1mm silicon particles into a stirring barrel. The order of adding materials can be changed. Then start stirring for 0.5-1h. Pour the obtained slurry into a tray and put it into an oven at 100℃-120℃ for drying to obtain silicon particles coated with graphite.

[0049] 250g of alcohol and 1250g of thermosetting resin are placed in a stirring device and stirred for 0.5-1h. 10kg of the silicon particles coated with graphite prepared above are mixed with 1.5kg of the obtained viscous resin slurry and stirred for 40min to finally obtain viscous modified silicon particles.

[0050] The modified silicon particles can react with a layer of graphite to form a silicon carbide shell during the heating process, thereby trapping the liquid silicon inside. When the temperature continues to rise, the liquid silicon is converted into silicon vapor and then breaks through the silicon carbide shell to react with the sample, ensuring that it is silicon vapor that reacts with the sample, thereby compensating for the black core condition that may be caused by liquid silicon infiltration.

[0051] Weigh the required modified silicon particles and put them into the distributor, and evenly distribute them into the mold through the distributor. Press them into the shape of a porous green body at 20MPa for 100s. At this time, quickly transfer the silicon plate to the support plate and put it into the oven. After curing at 150℃-170℃ for 1h, a silicon plate with a certain strength is obtained.

[0052] The prepared silicon plate is used in the siliconization process of the bulletproof plug plate. The silicon plate is assembled with the porous blank. The silicon plate obtained by pressing and curing can effectively avoid the occurrence of silicon particles spilling and the inconsistency between the amount of silicon particles around the sample and inside the sample in the process of loading into the furnace. The bulletproof plug plate after siliconization treatment can be clearly seen to have excellent internal uniformity and no black core through X-ray observation.

[0053] The density of the bulletproof plug plate made by this embodiment 3 can reach more than 98%; the three-point bending strength of the bulletproof plug plate is between 350-380 MPa; the hardness of the bulletproof plug plate is 90-94 HRA; the maximum pore between the bulletproof plug plate and the standard sample is within 0.4 mm, and the sample has no cracks.

[0054] The silicon plate prepared in this embodiment can improve the uniformity of silicon infiltration, reduce the degree of deformation and cracking of the sample, and can also eliminate the operation time of workers spreading silicon particles, thereby improving production efficiency and reducing production costs.

[0055] Example 4 Add 250g of graphite, 375g of pure water, 625g of ethylene glycol, and 10kg of 0.5mm silicon particles into a stirring barrel. The order of adding materials can be changed. Then start stirring for 0.5-1h. Pour the obtained slurry into a tray and put it into an oven at 100℃-120℃ for drying to obtain silicon particles coated with graphite.

[0056] The modified silicon particles can react with a layer of graphite to form a silicon carbide shell during the heating process, thereby trapping the liquid silicon inside. When the temperature continues to rise, the liquid silicon is converted into silicon vapor and then breaks through the silicon carbide shell to react with the sample, ensuring that it is silicon vapor that reacts with the sample, thereby compensating for the black core condition that may be caused by liquid silicon infiltration.

[0057] 300g of alcohol and 1500g of thermosetting resin are placed in a stirring device and stirred for 0.5-1h to obtain 1.8kg of viscous resin slurry. 11kg of the above-prepared graphite-coated silicon particles are mixed with the 1.8kg of viscous resin slurry obtained by stirring for 40min. Finally, viscous modified silicon particles are obtained. Weigh the required modified silicon particles and put them into a distributor, and evenly distribute them into the mold through the distributor. Press them into the shape of a porous green body at 20MPa for 150s. At this time, quickly transfer the silicon plate to the support plate and put it into an oven. After curing at 150℃-170℃ for 1h, a silicon plate with a certain strength is obtained.

[0058] The prepared silicon plate is used in the siliconization process of the bulletproof plug plate. The silicon plate is assembled with the porous blank. The silicon plate obtained by pressing and curing can effectively avoid the occurrence of silicon particles spilling and the inconsistency between the amount of silicon particles around the sample and inside the sample in the process of loading into the furnace. The bulletproof plug plate after siliconization treatment can be clearly seen to have excellent internal uniformity and no black core through X-ray observation.

[0059] The density of the bulletproof insert made by this embodiment 4 can reach more than 99%; the three-point bending strength is between 350-380 MPa; the hardness is 90-94 HRA; the maximum pore size when fitted with the standard sample is within 0.2 mm; and the sample has no cracks.

[0060] The silicon plate prepared in this embodiment can improve the uniformity of silicon infiltration, reduce the degree of deformation and cracking of the sample, and can also eliminate the operation time of workers spreading silicon particles, thereby improving production efficiency and reducing production costs.

[0061] From the above four embodiments, it can be seen that when the particle size of silicon particles decreases, the siliconization effect will gradually become better. When the particle size of silicon particles is less than 1 mm, no cracking occurs, the density of the sample is relatively high, and the maximum pore is the smallest.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that any modification to the technical solutions described in the aforementioned embodiments, or any equivalent replacement of some or all of the technical features therein, within the spirit and principles of the present invention, and such modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.

Claims

1. A silicon plate for bulletproof plug-in reaction, characterized in that: The silicon plate is prepared by mixing graphite-coated silicon particles with a thickener to obtain modified silicon particles, and the modified silicon particles are pressed and cured at low temperature.

2. The bulletproof plug-in reaction silicon plate according to claim 1, characterized in that: The graphite-coated silicon particles are prepared by mixing graphite slurry with silicon particles, adhering the graphite slurry to the surface of the silicon particles, and then drying.

3. The bulletproof plug-in reaction silicon plate according to claim 2, characterized in that: The graphite slurry is prepared by mixing a homogenizer, pure water and graphite.

4. The method for preparing a bulletproof plug-in plate reaction silicon plate according to any one of claims 1 to 3, characterized in that: The steps include: A1. Mix a homogenizing agent, pure water and graphite to prepare a graphite slurry; A2, mixing the graphite slurry with the silicon particles, making the graphite adhere to the surface of the silicon particles, and obtaining the graphite-coated silicon particles by drying; A3, mixing the graphite-coated silicon particles obtained in step S2 with a thickener to obtain modified silicon particles; A4, pressing the modified silicon particles into a silicon plate embryonic body having the same appearance as the porous embryonic body through a mold; A5. The silicon plate embryo pressed in step S4 is transferred into an oven through a support plate, and a silicon plate is obtained by low-temperature curing.

5. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 4, characterized in that: The following steps are also included: A6. Use silicon plates for siliconization treatment of bulletproof inserts.

6. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 4, characterized in that: The particle size of the silicon particles is 0.5 mm to 3 mm.

7. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 5 or 6, characterized in that: The thickener includes graphite emulsion or resin slurry.

8. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 7, characterized in that: The leveling agent includes alcohol or ethylene glycol.

9. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 5, 6 or 8, characterized in that: In the step S3, the mixing ratio of the thickener to the graphite-coated silicon particles is 1-1.8:9-11.

10. The method for preparing a bulletproof plug-in plate reaction silicon plate according to claim 5, 6 or 8, characterized in that: In step S4, the pressing pressure is 20-30 MPa, and the pressing time is 100-150 s.

Citation Information

Patent Citations

  • Treatment method of silicon powder for molten silicon infiltration

    CN113773094A

  • Preparation method of multi-curved-surface bulletproof plate

    CN118388239A

  • High-strength carbon / ceramic brake disk with ceramic functional layer

    WO2024148738A1