Silica hollow microsphere and preparation method thereof

By using ammonium bicarbonate and ammonium carbonate as template agents and coating and removing template agents under mild conditions, the problems of template removal difficulties and particle size control in the prior art are solved, and the particle size uniformity and Economical preparation of hollow silica microspheres.

CN118929670APending Publication Date: 2024-11-12UNIV OF ELECTRONICS SCI & TECH OF CHINA +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410988298.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing preparation methods for hollow silica microspheres, template removal is difficult, high temperature conditions are required, and expensive chemical reagents are difficult to control the particle size uniformity of the microspheres.

Method used

Ammonium bicarbonate and ammonium carbonate are used as template agents, and the template agent is coated by mixing with alcohol solvents and adding orthosilicate dropwise. Then, the template agent is removed in water at 35 to 55°C to avoid high temperature treatment, and the particle size of the template agent is controlled to Regulate the particle size of microspheres.

Benefits of technology

It realizes effective removal of template agent under mild conditions and obtains hollow silica microspheres with uniform particle size. The raw materials are cheap and easy to obtain and the particle size is controllable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929670A_ABST
    Figure CN118929670A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of silicon dioxide, and discloses a silicon dioxide hollow microsphere and a preparation method thereof. The preparation method comprises the following steps: suspending a template agent in an alcohol solvent, wherein the template agent comprises at least one of ammonium bicarbonate and ammonium carbonate; the preparation method comprises the following steps: dropwise adding orthosilicate, carrying out a heat preservation reaction after dropwise adding is completed to obtain a first reaction solution, carrying out solid-liquid separation to obtain a first solid, and washing and drying the first solid; suspending the dried matter in water, raising the temperature to 35-55 DEG C, and carrying out heat preservation reaction for 1-3 hours to obtain a second reaction solution; and carrying out solid-liquid separation on the second reaction liquid to obtain a second solid, and washing and drying the second solid to obtain the silicon dioxide hollow microspheres. According to the method, the template agent can be removed without high temperature and can be removed only by water, solvents such as acid or alkali are not needed, conditions are mild, raw materials are cheap and easy to obtain, the particle size of the obtained product can be controlled by controlling the particle size of the added template agent, and the particle size of the product is uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon dioxide preparation, and in particular to silicon dioxide hollow microspheres and a preparation method thereof. Background Art

[0002] Hollow silica is a special new type of inorganic material with a cavity structure inside. Due to its non-toxicity, high melting point and stability, and easy modification, it has many applications in drug controlled release, refractory materials, capsule encapsulation, nanocatalysts, etc. The preparation of hollow silica microspheres has received widespread attention. Currently, the two main preparation methods of hollow silica microspheres are spray drying and template method.

[0003] The spray drying method is to pass liquid raw materials such as solutions, emulsions, suspensions, etc. through an atomizer to form extremely fine mist droplets, which are then solidified instantly after contact with hot air, and finally dried to obtain the desired product. Although this method is simple to prepare, it is difficult to control the diameter of the microspheres, and grading and screening are still required in the later stage to obtain products within the target size range.

[0004] The template method is a method of using a substance with a certain shape and structure as an auxiliary template, and then filling or coating the template according to the needs to obtain a microsphere of the desired shape. The template method is divided into hard template method, soft template method, double template method and self-template method. The microspheres obtained by the template method need to be removed by chemical reagents in the later process. The difficulties faced include how to choose the remover, microsphere breakage, remover residue, expensive process, etc. For example, Tang et al. used PS microspheres as templates to obtain hollow silica spheres, and then used magnesium thermal reduction method to obtain hollow silicon spheres with an inner pore diameter of about 50nm (TANG H, XU YY, LIUL, et al. A hollow silicon nanosphere / carbon nanotube composite as an anode material for lithium-ion batteries [J]. Coatings, 2022, 12 (10): 1515.). For example, Neda et al. used silica nanoparticles as templates and synthesized them according to the Stober method. They first synthesized core-shell particles by a one-step method, and then selectively etched the silica particles with a hydrofluoric acid solution to obtain a monodisperse hollow structure (ARABIN, NADERIM, REZAEIM, et al. Designing highly active unique hollow@(Au@Pt) core-shell nanostructure as electro-catalyst for ethanol oxidation reactions[J]. Journal of the Iranian Chemical Society, 2022, 19(10): 4261-4274.).

[0005] However, the above-mentioned methods for removing the template are difficult to remove and require high temperature removal, and the conditions are difficult to control.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a hollow silicon dioxide microsphere and a preparation method thereof, which can avoid the use of high temperature to remove the template agent, has mild conditions, cheap and easily available raw materials, and the particle size of the obtained product is uniform and controllable.

[0008] The present invention is achieved in that:

[0009] In a first aspect, the present invention provides a method for preparing hollow silica microspheres, comprising:

[0010] suspending a template agent in an alcohol solvent, wherein the template agent comprises at least one of ammonium bicarbonate and ammonium carbonate;

[0011] Add orthosilicate dropwise, and after the addition is complete, heat-retaining for reaction to obtain a first reaction liquid, perform solid-liquid separation to obtain a first solid, and wash and dry the first solid;

[0012] The dried product is suspended in water, the temperature is raised to 35-55°C, and the reaction is kept at this temperature for 1-3 hours to obtain a second reaction solution;

[0013] The second reaction liquid is separated into a solid and liquid state to obtain a second solid, and the second solid is washed and dried to obtain hollow silica microspheres.

[0014] In an optional embodiment, the mass ratio of the template to the alcohol solvent is 1:(10-20).

[0015] In an optional embodiment, the alcohol solvent includes at least one of n-octanol, ethanol, n-butanol and isopropanol.

[0016] In an optional embodiment, the temperature of the alcohol solvent is -10°C to -5°C.

[0017] In an optional embodiment, the orthosilicate includes at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate and butyl orthosilicate.

[0018] In an optional embodiment, the mass ratio of the amount of the orthosilicate added to the template is (1-3):1.

[0019] In an optional embodiment, the insulation time of the insulation reaction is 5-20 hours.

[0020] In an optional embodiment, the solid-liquid separation of the first reaction liquid and the second reaction liquid comprises filtration, centrifugation or suction filtration;

[0021] And / or, washing the first solid includes washing with ethanol and deionized water in sequence;

[0022] And / or, drying the first solid object comprises drying at room temperature;

[0023] And / or, washing the second solid includes washing with deionized water;

[0024] And / or, drying the second solid material comprises drying under vacuum.

[0025] In an optional embodiment, the particle size of the hollow silica microspheres is controlled by controlling the particle size of the template, wherein the particle size of the template is 0.03 μm-300 μm, and the particle size D50 of the hollow silica microspheres is 0.4 μm-40 μm.

[0026] In a second aspect, the present invention provides hollow silica microspheres, which are prepared by the method for preparing hollow silica microspheres as described in any one of the aforementioned embodiments.

[0027] The present invention has the following beneficial effects:

[0028] The invention provides a method for preparing hollow silicon dioxide microspheres. The method adopts at least one of ammonium bicarbonate and ammonium carbonate as a template, disperses the template by mixing with an alcohol solution, and then drips orthosilicate to coat the surface of the template with a layer of silicon dioxide. After the coating is completed, the template can be removed in water at 35-55°C. The invention can avoid removing the template at high temperature and can remove the template only by using water without using solvents such as acid or alkali. The conditions are mild and the raw materials are cheap and easy to obtain. The particle size of the product obtained can be controlled by controlling the particle size of the added template, and the product particle size is uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 This is a SEM image of the hollow microspheres provided in Example 1 of the present invention;

[0031] Figure 2 This is a SEM image of the hollow microspheres provided in Example 7 of the present invention. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0033] The present invention provides a method for preparing hollow silicon dioxide microspheres, which comprises the following steps:

[0034] S1. Suspending the template in an alcohol solvent.

[0035] The mass ratio of the template agent to the alcohol solvent is 1:(10-20). The template agent includes at least one of ammonium bicarbonate and ammonium carbonate. The alcohol solvent includes at least one of n-octanol, ethanol, n-butanol and isopropanol. The temperature of the alcohol solvent is -10°C to -5°C.

[0036] In some embodiments, the mass ratio of the template to the alcohol solvent can be, for example, any one of 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 and 1:20, or a range value between any two of them. The mass ratio of ammonium bicarbonate and ammonium carbonate in the template can be any mass ratio, for example, the template only includes ammonium bicarbonate or ammonium carbonate, the template can also include ammonium bicarbonate and ammonium carbonate at the same time, when the template includes ammonium bicarbonate and ammonium carbonate at the same time, the mass percentage of ammonium bicarbonate and ammonium carbonate can be, for example, 10%-90%: 90%-10%. For example, typical but non-limiting examples include: the mass ratio of ammonium bicarbonate and ammonium carbonate is 9:1, 8:2, 7:3, 6:4, 5:5, 4:6, 3:7, 2:8, 1:9, or a range value between any two of them.

[0037] In the present invention, an alcohol solvent is used as the solvent of the template. Since ammonium bicarbonate and / or ammonium carbonate are both soluble in water but insoluble in alcohol, the alcohol solvent is used to disperse the template but not dissolve it. At the same time, the alcohol solvent is easily removed in the subsequent washing and drying process, ensuring the purity of the product. Furthermore, the present invention also limits the temperature of the alcohol solvent to -10°C to -5°C, and suspends at low temperature to ensure the stability of ammonium bicarbonate and / or ammonium carbonate and avoid decomposition thereof, and at low temperature, the growth of the silicon dioxide layer can become slow and dense, which is more conducive to improving mechanical properties.

[0038] Furthermore, in the present invention, the particle size of the hollow silica microspheres can be controlled by controlling the particle size of the template, wherein the particle size of the template is 0.03 μm-300 μm.

[0039] S2, adding orthosilicate dropwise, and after the addition is completed, keeping the temperature to react to obtain a first reaction liquid, separating the solid and the liquid to obtain a first solid, and washing and drying the first solid.

[0040] The mass ratio of the amount of orthosilicate added to the template is (1-3): 1. The orthosilicate includes at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate and butyl orthosilicate. The insulation temperature of the insulation reaction is 20-50° C., and the insulation time is 5-20 hours.

[0041] In the present invention, orthosilicate can be loaded on the template by dripping orthosilicate to achieve coating of the template. The mass ratio of the dripping amount of orthosilicate to the template can be, for example, any one of 1:1, 1.5:1, 2:1, 2.7:1, 3:1 or a range between any two of them.

[0042] Methods for solid-liquid separation of the first reaction liquid include but are not limited to filtration, centrifugation or suction filtration; washing the first solid includes washing with ethanol and deionized water in sequence; and drying includes drying at room temperature.

[0043] In the present invention, the similar compatibility of ethanol is first used to remove the residual solvent on the surface, and then the deionized water is used for repeated washing to further remove the solvent, so that the washing effect is better, and then it is directly dried at room temperature without being placed in a blower or oven for drying. The drying at room temperature of the present invention can be carried out by, for example, drying in a ventilated state.

[0044] S3. Suspend the dried product in water, raise the temperature to 35-55°C, and keep the temperature to react for 1-3 hours to obtain a second reaction solution.

[0045] Since it is difficult to achieve sealed coating during the coating process, a porous structure exists on the surface of the obtained dried product. When the dried product is suspended in water, water enters the interior from the porous structure on the surface of the dried product. Since ammonium bicarbonate and ammonium carbonate are both easily soluble in water, the template can be removed by simply mixing with water. The template removal effect is good and the conditions are mild.

[0046] In some other embodiments, the heating temperature can be, for example, any one of 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C, or a range between any two of them, and the insulation reaction time can be, for example, any one of 1h, 1.5h, 2h, 2.5h, 3h, or a range between any two of them.

[0047] S4, separating the second reaction liquid into a second solid by solid-liquid separation, washing and drying the second solid to obtain hollow silica microspheres.

[0048] The method of solid-liquid separation of the second reaction liquid includes but is not limited to filtration, centrifugation or suction filtration; washing the second solid includes washing with deionized water; drying includes drying under vacuum. The particle size D50 of the prepared hollow silica microspheres is 0.4μm-40μm. It can be seen that the particle size of the hollow silica microspheres in the present invention is determined by the particle size of the template (ammonium carbonate and / or ammonium bicarbonate). Therefore, in the present invention, the particle size of the hollow silica microspheres finally obtained can be regulated by controlling the particle size of the added template, so that the particle size of the hollow silica microspheres can be regulated within a larger range (0.4μm-40μm), and the particle size of the hollow silica microspheres obtained is uniform.

[0049] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0050] Example 1

[0051] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0052] S1. Suspend the template (10 g of ammonium bicarbonate with a particle size D50 of 10 μm) in an alcohol solvent (100 g of n-octanol + 50 g of n-butanol) at a temperature of -10°C.

[0053] S2, dropwise add 15 g of methyl orthosilicate, keep the mixture warm at 20° C. for 20 h to obtain a first reaction solution, filter to obtain a first solid, wash the first solid with ethanol and deionized water in sequence, and then dry at room temperature.

[0054] S3. The dried product is suspended in water, the temperature is raised to 35°C, and the reaction is carried out for 3 hours to obtain a second reaction solution.

[0055] S4, filtering the second reaction liquid to obtain a second solid, washing the second solid with deionized water, and then vacuum drying to obtain hollow silica microspheres with a particle size D50 of 12 μm. Figure 1 ,from Figure 1 It can be seen that the hollow silica microspheres prepared in this example have uniform particle size distribution, and the particle size of the hollow silica microspheres is easy to control.

[0056] Example 2

[0057] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0058] S1. Suspend the template (9 g of ammonium bicarbonate with a particle size D50 of 3 μm + 1 g of ammonium carbonate with a particle size D50 of 3 μm) in an alcohol solvent (150 g of n-octanol + 50 g of n-butanol) at a temperature of -10°C.

[0059] S2. Add 10 g of methyl orthosilicate dropwise. After the addition is complete, keep the mixture at 35° C. for 20 hours to obtain a first reaction liquid. Filter the mixture to obtain a first solid. Wash the first solid with ethanol and deionized water in sequence, and then dry it at room temperature.

[0060] S3. The dried product is suspended in water, the temperature is raised to 35°C, and the reaction is kept at this temperature for 3 hours to obtain a second reaction solution.

[0061] S4. Filter the second reaction liquid to obtain a second solid, wash the second solid with deionized water, and then vacuum dry to obtain hollow silica microspheres with a particle size D50 of 4 μm.

[0062] Example 3

[0063] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0064] S1. Suspend the template (7 g of ammonium bicarbonate with a particle size D50 of 30 μm + 3 g of ammonium carbonate with a particle size D50 of 30 μm) in an alcohol solvent (80 g of n-octanol + 100 g of n-butanol + 200 g of isopropanol) at a temperature of -10°C.

[0065] S2. Add 27 g of butyl orthosilicate dropwise. After the addition is complete, keep the mixture warm at 30° C. for 20 hours to obtain a first reaction liquid. Filter the mixture to obtain a first solid. Wash the first solid with ethanol and deionized water in sequence, and then dry it at room temperature.

[0066] S3. The dried product is suspended in water, the temperature is raised to 35°C, and the reaction is kept at this temperature for 3 hours to obtain a second reaction solution.

[0067] S4. Filter the second reaction liquid to obtain a second solid, wash the second solid with deionized water, and then vacuum dry to obtain hollow silica microspheres with a particle size D50 of 35 μm.

[0068] Example 4

[0069] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0070] S1. Suspend the template (5 g of ammonium bicarbonate with a particle size D50 of 37 μm + 5 g of ammonium carbonate with a particle size D50 of 38 μm) in an alcohol solvent (200 g of ethanol) at a temperature of -8°C.

[0071] S2. Add 30 g of butyl orthosilicate dropwise. After the addition is complete, keep the mixture warm at 35° C. for 10 hours to obtain a first reaction liquid. Filter the mixture to obtain a first solid. Wash the first solid with ethanol and deionized water in sequence, and then dry it at room temperature.

[0072] S3. Suspend the dried product in water, raise the temperature to 45°C, and keep the temperature to react for 2 hours to obtain a second reaction solution.

[0073] S4. Filter the second reaction liquid to obtain a second solid, wash the second solid with deionized water, and then vacuum dry to obtain hollow silica microspheres with a particle size D50 of 40 μm.

[0074] Example 5

[0075] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0076] S1. Suspend the template (3 g of ammonium bicarbonate with a particle size D50 of 7 μm + 7 g of ammonium carbonate with a particle size D50 of 7 μm) in an alcohol solvent (100 g of n-octanol + 100 g of n-butanol) at a temperature of -8°C.

[0077] S2. Add 10 g of propyl orthosilicate dropwise. After the addition is complete, keep the mixture at 40° C. for 10 hours to obtain a first reaction liquid. Filter the mixture to obtain a first solid. Wash the first solid with ethanol and deionized water in sequence, and then dry it at room temperature.

[0078] S3. Suspend the dried product in water, raise the temperature to 45°C, and keep the temperature to react for 2 hours to obtain a second reaction solution.

[0079] S4. Filter the second reaction liquid to obtain a second solid, wash the second solid with deionized water, and then vacuum dry to obtain hollow silica microspheres with a particle size D50 of 10 μm.

[0080] Example 6

[0081] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0082] S1. Suspend the template (1 g of ammonium bicarbonate with a particle size D50 of 0.3 μm + 9 g of ammonium carbonate with a particle size D50 of 0.5 μm) in an alcohol solvent (100 g of ethanol) at a temperature of -5°C.

[0083] S2. Add 10 g of ethyl orthosilicate and 10 g of butyl orthosilicate dropwise. After the addition is completed, keep the mixture warm at 50°C for 5 hours to obtain a first reaction liquid. Filter the liquid to obtain a first solid. Wash the first solid with ethanol and deionized water in turn, and then dry it at room temperature.

[0084] S3. The dried product is suspended in water, the temperature is raised to 55°C, and the reaction is kept at this temperature for 1 hour to obtain a second reaction solution.

[0085] S4. Filter the second reaction liquid to obtain a second solid, wash the second solid with deionized water, and then vacuum dry to obtain hollow silica microspheres with a particle size D50 of 0.6 μm.

[0086] Example 7

[0087] This embodiment provides a hollow silica microsphere, and the preparation method thereof comprises the following steps:

[0088] S1. Suspend the template (10 g of ammonium carbonate with a particle size D50 of 0.3 μm) in an alcohol solvent (100 g of n-octanol + 50 g of ethanol + 50 g of n-butanol + 100 g of isopropanol) at a temperature of -5°C.

[0089] S2. Add 5 g of propyl orthosilicate and 10 g of butyl orthosilicate dropwise. After the addition is completed, keep the mixture warm at 50°C for 5 hours to obtain a first reaction liquid. Filter the liquid to obtain a first solid. Wash the first solid with ethanol and deionized water in turn, and then dry it at room temperature.

[0090] S3. The dried product is suspended in water, the temperature is raised to 55°C, and the reaction is kept at this temperature for 1 hour to obtain a second reaction solution.

[0091] S4, filtering the second reaction liquid to obtain a second solid, washing the second solid with deionized water, and then vacuum drying to obtain hollow silica microspheres with a particle size D50 of 0.4 μm. Figure 2 ,from Figure 2 It can be seen that the hollow silica microspheres prepared in this example have uniform particle size distribution, and the particle size of the hollow silica microspheres is easy to control.

[0092] Comparative Example 1

[0093] This comparative example provides a conventional method for preparing hollow silica microspheres, which includes: using polystyrene (PS) as a template, hexadecyltrimethylammonium bromide (CTAB) as a positive surfactant, and tetraethyl orthosilicate (TEOS) as a silicon source. Weigh 0.15g of micron-sized polystyrene microspheres, add them to a mixed solution of water / ethanol with CTAB, ultrasonically disperse for 30min to obtain a uniformly dispersed suspension, and then add an appropriate amount of ammonia water and stir for 30min. At a certain stirring speed, add an appropriate amount of TEOS dropwise, continue stirring and reacting for 20h, put the obtained suspension into a centrifuge for ultracentrifugation, remove the supernatant, wash three times with high-purity water and ethanol respectively, and dry for 12h. The dried core-shell structure sample is placed in a tubular furnace and heated to 100℃ for 4h, then heated to 550℃ for 2h to remove the polystyrene template to obtain hollow silica microspheres. The results show that SiO2 hollow microspheres with a particle size of 2-5μm can be successfully prepared by this method.

[0094] Comparative Example 2

[0095] This comparative example is substantially the same as Example 1, except that the template agent in this comparative example is polystyrene.

[0096] Comparative Example 3

[0097] This comparative example is substantially the same as Example 1, except that the temperature of the alcohol solvent in this comparative example is room temperature.

[0098] Comparative Example 4

[0099] This comparative example is substantially the same as Example 1, except that the alcohol solvent in Example 1 is replaced by carbon disulfide in this comparative example.

[0100] Comparative Example 5

[0101] This comparative example is substantially the same as Example 1, except that the amount of methyl orthosilicate added in this comparative example is 50 g.

[0102] Comparative Example 6

[0103] This comparative example is substantially the same as Example 1, except that in this comparative example, the template (10 g of ammonium bicarbonate) is replaced with camellia powder.

[0104] Experimental example

[0105] The template removal temperature, particle size and dry weight of the hollow silica microspheres obtained in the above examples and comparative examples were statistically analyzed, and the statistical results are as follows:

[0106] Example Template removal temperature / ℃ Particle size D50 / μm Dry weight / g Example 1 35 12 3.8 Example 2 35 4 3.3 Example 3 35 35 5.4 Example 4 45 40 5.5 Example 5 45 10 4.8 Example 6 55 0.6 5.1 Example 7 55 0.4 3.6 Comparative Example 1 550 15 3.5 Comparative Example 2 550 2 No deposition occurred Comparative Example 3 35 16 4.0 Comparative Example 4 35 0.02 3.5 Comparative Example 5 35 30 6 Comparative Example 6 35 1 3.0

[0107] As can be seen from the above table, using ammonium carbonate or ammonium bicarbonate or a combination of the two as templates, it is possible to react at low temperatures, it is easier to adjust the deposition rate of surface silica, and it is easier to control the particle size of hollow silica microspheres by the size of the template. The particle size of hollow silica microspheres in Examples 1-7 of the present invention can be selected between microns and nanometers, and in Comparative Example 1, conventional methods are selected for preparation, and at this time, the template removal temperature is significantly higher than that of the embodiments of the present invention. Similarly, conventional template agents are selected in Comparative Example 2, and a higher removal temperature is also required, and specific hollow silica microspheres cannot be deposited and prepared, and only some template fragments are obtained. It is fully proved that the process of the present invention is mainly for ammonium carbonate or ammonium bicarbonate or a combination of the two as templates, and other templates are not applicable. Alcohol solvents are not precooled in Comparative Example 3, and at this time, ammonium bicarbonate will slowly decompose at room temperature, thereby causing the particle size of hollow silica microspheres to increase compared to Example 1, and the dry weight becomes larger. In comparative example 4, the alcohol solvent of Example 1 is replaced with carbon disulfide. Although ammonium bicarbonate is also insoluble in carbon disulfide, it will cause uneven deposition and shell fragmentation. In comparative example 5, the amount of methyl orthosilicate added is too large, which will cause the shell to thicken and the mesoporous structure of the shell to disappear. In comparative example 6, the template agent is replaced with camellia pollen, which will cause uneven deposition and shell fragmentation, and then the particle size and dry weight are significantly lower than those in Example 1. In summary, the preparation method of hollow silica microspheres provided by the present invention uses at least one of ammonium bicarbonate and ammonium carbonate as a template agent, disperses by mixing with an alcohol solution, and then drops orthosilicate to achieve a layer of silica coating on the surface of the template agent. After the coating is completed, the template agent can be removed in water at 35 to 55°C. The present invention can avoid the use of high temperature to remove the template agent, and can be removed only by water, without the use of acid or alkali solvents, mild conditions, cheap and easy to obtain raw materials, and the particle size of the product obtained can be controlled by controlling the particle size of the added template agent, and the product particle size is uniform.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing hollow silicon dioxide microspheres, It is characterized in that It includes: suspending a template agent in an alcohol solvent, wherein the template agent comprises at least one of ammonium bicarbonate and ammonium carbonate; Add orthosilicate dropwise, and after the addition is complete, heat-retaining for reaction to obtain a first reaction liquid, perform solid-liquid separation to obtain a first solid, and wash and dry the first solid; The dried product is suspended in water, the temperature is raised to 35-55°C, and the reaction is kept at this temperature for 1-3 hours to obtain a second reaction solution; The second reaction liquid is separated into a solid and liquid state to obtain a second solid, and the second solid is washed and dried to obtain hollow silica microspheres.

2. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The mass ratio of the template to the alcohol solvent is 1:(10-20).

3. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The alcohol solvent includes at least one of n-octanol, ethanol, n-butanol and isopropanol.

4. The method for preparing hollow silicon dioxide microspheres according to claim 1, It is characterized in that The temperature of the alcohol solvent is -10°C to -5°C.

5. The method for preparing hollow silicon dioxide microspheres according to claim 1, It is characterized in that The orthosilicate includes at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate and butyl orthosilicate.

6. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The mass ratio of the amount of the orthosilicate added to the template is (1-3):

1.

7. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The insulation time of the insulation reaction is 5-20h.

8. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The solid-liquid separation of the first reaction liquid and the second reaction liquid includes filtering, centrifuging or suction filtration; And / or, washing the first solid includes washing with ethanol and deionized water in sequence; And / or, drying the first solid object comprises drying at room temperature; And / or, washing the second solid includes washing with deionized water; And / or, drying the second solid material comprises drying under vacuum.

9. The method for preparing hollow silica microspheres according to claim 1, It is characterized in that The particle size of the hollow silica microspheres is controlled by controlling the particle size of the template, wherein the particle size of the template is 0.03 μm-300 μm, and the particle size D50 of the hollow silica microspheres is 0.4 μm-40 μm.

10. A hollow silicon dioxide microsphere, It is characterized in that The hollow silicon dioxide microspheres are prepared by the preparation method of hollow silicon dioxide microspheres according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Environment-friendly method for preparing hollow silicon dioxide sphere with diameter smaller than 100nm at room temperature

    CN102942186A

  • Hollow microspheres and preparation method thereof

    CN109956479A

  • Method for producing hollow silica particles

    JP2020040858A