Method for preparing arsine through electro-catalysis by taking ash arsenic as arsenic source
By using PdFe bimetallic alloy nanoparticle electrode loaded on nickel foil to perform constant current electrolysis in alkaline electrolyte, arsenic was successfully prepared efficiently at room temperature, solving the incomplete reaction, numerous by-products and safe in the prior art. The problem of low performance has achieved a green and safe arsenane synthesis process.
Patent Information
- Application Number
- CN202411139730.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing arsenane preparation methods have problems such as incomplete reactions, many by-products, low safety, and the need for high temperature, high pressure and large amounts of chemical reducing agents, making it difficult to achieve a green and efficient preparation process.
The PdFe bimetallic alloy nanoparticle electrode loaded on nickel foil is used as the working cathode. The conversion of ash arsenic into arsenic by constant current electrolysis in the alkaline electrolyte is avoided, and the use of high temperature, high pressure and chemical reducing agents are avoided. The catalyst can be reused.
The efficient synthesis of arsenic is achieved under room temperature, with a concentration of up to 43.1%, and it is easy to operate and has high safety, avoiding waste liquid pollution, and the durability and stability of the electrocatalyst are good.
Smart Images

Figure CN118929748A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of arsine synthesis, and in particular relates to a method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source. Background Art
[0002] Arsine is a key dopant in the semiconductor industry, especially in the manufacture of III-V compound semiconductors such as gallium arsenide. By using arsine in vapor phase epitaxy and molecular beam epitaxy processes, the arsenic content in semiconductor materials can be precisely controlled to adjust their electrical properties. This control ability makes arsine play a vital role in high-tech fields such as semiconductor manufacturing, flat panel display production, and photovoltaic cell manufacturing.
[0003] At present, the preparation of arsine mainly relies on thermochemical reduction. This production process requires a large amount of chemical reducing agents and produces a large amount of waste liquid, which is not only inconsistent with the concept of green development, but also has great safety hazards. In recent years, electrochemical technology has become a powerful green and efficient tool in chemical synthesis. Electrochemistry achieves the reduction and oxidation of substances through the gain and loss of electrons, avoiding the need for oxidants and reducing agents in traditional chemical reactions. The current and potential in the electrochemical process can be controlled at will, and it has the advantages of simple operation, green environmental protection and mild conditions. Therefore, the application prospect of electrochemical methods in the preparation of arsine is broad. Summary of the invention
[0004] The present invention provides a method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source at room temperature. At present, the preparation methods of arsine mainly include chemical reduction method, gas phase reaction method, etc. Although these methods can produce arsine, there are problems such as incomplete reaction, many by-products, and low safety. The present invention uses a PdFe bimetallic alloy nanoparticle electrode loaded on a nickel foil as a working cathode, and gray arsenic as an arsenic source. In an alkaline electrolyte, a constant current electrolysis method is used to catalytically reduce gray arsenic to arsine at room temperature. In a wide current density range, efficient synthesis of arsine can be achieved. In addition, common and easily available gray arsenic is used as an arsenic source, and a PdFe / NF electrode easily prepared by electrodeposition is used as a catalytic working cathode. The reaction conditions are mild, high temperature and high pressure and chemical reducing agent are not required, and the electrocatalyst can be reused. A green, safe and efficient method is provided for the synthesis of arsine.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source uses a PdFe bimetallic alloy nanoparticle electrode loaded on a nickel foil as a working cathode, and a counter electrode anode is provided. Gray arsenic is used as an arsenic source, and gray arsenic is catalytically reduced by constant current electrolysis in an alkaline electrolyte to prepare arsine.
[0007] Furthermore, the method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source specifically comprises the following steps:
[0008] 1) A PdFe bimetallic alloy nanoparticle electrode loaded on a nickel foil is used as a working cathode, a carbon or Pt sheet is used as a counter electrode anode, and a double-chamber standard flow electrolytic cell is used as an electrocatalytic reaction device, wherein the cathode chamber and the anode chamber are separated by a proton membrane;
[0009] 2) adding gray arsenic and alkaline electrolyte into the cathode chamber, adding alkaline electrolyte into the anode chamber, and stirring the electrolyte in the cathode chamber to fully disperse the gray arsenic;
[0010] 3) The working cathode and the counter electrode anode are connected to the electrochemical workstation through wires, and the electrolysis system performs constant current electrolysis with a current density of 5-40 mA / cm 2 , to prepare arsine.
[0011] Furthermore, in step 2), the alkaline electrolyte is an aqueous solution of one or more of sodium carbonate, potassium carbonate, potassium hydroxide, and sodium hydroxide, and its concentration is 0.1-1.5M, preferably 0.5-1M.
[0012] Furthermore, in step 2), the amount of gray arsenic added to the cathode chamber electrolyte is 300-800 g / L, preferably 600-700 g / L.
[0013] Furthermore, the electrocatalytic reaction time is 5-100h.
[0014] Furthermore, the PdFe bimetallic alloy nanoparticle electrode loaded on nickel foil is marked as PdFe / NF electrode, and its preparation method comprises the following steps:
[0015] S1: Pre-treating the nickel foil to remove the surface oxide layer and impurities;
[0016] S2: placing the nickel foil obtained in step S1 in a mixed aqueous solution containing Fe salt and Pd salt, and performing electrodeposition in a standard three-electrode system, wherein the nickel foil is used as a cathode working electrode, the Pt sheet is used as a counter electrode, and a saturated calomel electrode is used as a reference electrode. During the electrodeposition process, Pd and Fe elements are deposited on the nickel foil, and then the nickel foil is rinsed and dried for later use;
[0017] S3: calcining the electrode obtained in step S2 at 400-600° C. for 1-4 h in an inert gas atmosphere, and cooling to room temperature to obtain the PdFe / NF electrode.
[0018] Furthermore, the pretreatment step in step S1 is: placing the nickel foil in a 2-4M hydrochloric acid solution and ultrasonically removing the surface oxide layer for 2-20 minutes, then rinsing the surface acidic solution with deionized water, and then placing it in acetone and ultrasonically removing residual organic matter on the surface, and finally rinsing it with deionized water and drying it, and the treatment is completed.
[0019] Furthermore, in step S2, the Pd salt is one of K2PdCl4, Na2PdCl4, PdCl2 and K2PdCl6, and its concentration in the mixed aqueous solution is 0.1-1M; the Fe salt is one of FeCl3, Fe2(SO4)3 and Fe(NO3)3, and its concentration in the mixed aqueous solution is 0.1-1M, preferably 0.5M.
[0020] Further, in step S2, the concentration of Pd salt in the mixed aqueous solution is 0.1-0.3 M, preferably 0.2 M. During the electrodeposition, the deposition is stopped when the charge reaches 300-1500C, preferably when the charge reaches 400-500C.
[0021] The beneficial effects of the present invention are:
[0022] 1) The present invention realizes the electrocatalytic preparation of arsine using gray arsenic as an arsenic source at room temperature, and realizes the efficient synthesis of arsine in a wide current density range. In the wide current density range, the concentration of arsine can reach 43.1%.
[0023] 2) The present invention uses PdFe bimetallic alloy nanoparticles loaded on nickel foil as the electrocatalyst, does not require high temperature, high pressure and chemical reducing agents, has mild reaction conditions, is easy to operate, and the catalyst is reusable and easy to recycle, effectively avoiding the problems of complex processes, low safety, and large waste liquid pollution in other synthesis methods.
[0024] 3) The working electrode of the present invention has good durability and stability and can be used repeatedly. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 TEM image of the cathode working electrode PdFe / NF of the present invention; DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0027] The size of the nickel foil in the embodiment of the present invention is 10×10 cm 2 .
[0028] Example 1: Synthesis of Arsine
[0029] 1) Preparation of cathode working electrode
[0030] Step 1, placing the nickel foil in a 3M hydrochloric acid solution for 10 minutes to remove the surface oxide layer; then rinsing the surface acid solution with deionized water, and then placing it in acetone for 10 minutes to remove residual organic matter on the surface; finally, rinsing it with deionized water and drying it for later use;
[0031] Step 2, placing the nickel foil obtained in step 1 in a mixed aqueous solution containing 0.5M Fe(NO3)3 and 0.2M K2PdCl4, and performing electrodeposition at a current of 20 mA in a standard three-electrode system, wherein the nickel foil is used as a cathode working electrode, the Pt sheet is used as a counter electrode, and a saturated calomel electrode is used as a reference electrode. During the electrodeposition process, Pd and Fe elements are deposited on the nickel foil. When the charge reaches 500C, the deposition is stopped, and the nickel foil is rinsed and dried for later use;
[0032] Step 3, the electrode obtained in step 2 is calcined at 500°C for 3h in an Ar atmosphere, cooled to room temperature, rinsed with deionized water and dried to obtain a PdFe / NF electrode. The TEM image of the PdFe / NF electrode is shown in FIG. Figure 1 As shown, there are uniformly dispersed PdFe nanoparticles on the surface of the nickel foil substrate.
[0033] 2) Catalytic reduction of gray arsenic to prepare arsine by constant current electrolysis
[0034] 10×10cm 2 The double-chamber standard flow electrolytic cell with an effective area is used as a container, and the cathode chamber and the anode chamber are separated by a proton exchange membrane (Nafion 117). 1L 1M KOH alkaline aqueous solution is added to the cathode chamber, and 1L 1M KOH alkaline aqueous solution is added to the anode chamber, and then 700g gray arsenic is added to the cathode chamber, and a magnetic particle is added to the cathode chamber and the cathode chamber is prevented from being placed on a magnetic stirrer to stir the electrolyte in the cathode chamber. PdFe / NF is used as the cathode working electrode, a Pt sheet is used as the counter electrode, and a Hg / HgO (1.0M KOH) electrode is used as a reference electrode. The negative and positive electrodes are connected to an electrochemical workstation through wires, and a constant current of 1A-5A is selected for reaction. After reacting for 5 hours / 10 hours, the concentration of arsine is analyzed by gas chromatography.
[0035] According to the above operation process, the test was carried out under different constant currents, and the results are shown in Table 1.
[0036] In the experiment of preparing arsine by catalytic reduction of gray arsenic by constant current electrolysis of the present invention, there are only two cathode outputs, namely, arsenic hydrogenation product (arsine AsH3) and hydrogen. The arsine concentration in Table 1 refers to the volume fraction of arsine in the mixed system of arsine and hydrogen. In the experiment of the present invention, the gas outlet of the cathode chamber is connected to the tail gas treatment device (a plurality of absorption tanks in series containing saturated potassium permanganate aqueous solution). When sampling and analyzing, the valve of the gas outlet is switched to connect to the gas chromatograph to measure the arsine concentration in the mixed gas.
[0037] Table 1. Arsenic concentration at different currents (%)
[0038]
[0039]
[0040] As shown in Table 1, under different current test conditions, the concentration of arsine produced at the cathode exceeded 20%. In particular, under the action of 3A current, after 10 hours of testing, the arsine concentration reached 43.1%. When the current was low, the conversion rate of gray arsenic was slow; as the current increased further, the arsine concentration decreased due to the competition of the hydrogen evolution reaction.
[0041] Example 2: Regulating the electrolyte concentration
[0042] The experimental conditions of Example 2 are repeated in Example 1, with the only difference being that "in step 2), the concentration of the alkaline aqueous solution of KOH is replaced with 0.5M, 1M, 1.5M, 2M, 2.5M or 3M, the concentration of the alkaline aqueous solution of KOH in the cathode chamber and the anode chamber is the same, and a constant current of 3A is selected for the reaction", and other conditions remain unchanged. After 5h / 10h of reaction, the arsine concentration is analyzed by gas chromatography.
[0043] According to the above operation process, tests were carried out at different electrolyte concentrations. The results are shown in Table 2.
[0044] Table 2. Arsine concentrations at different electrolyte concentrations (%)
[0045]
[0046] As shown in Table 2, tests were conducted at different electrolyte concentrations. The results show that the concentration of the electrolyte has a great influence on arsine, presenting a volcano-shaped curve. Specifically, when the electrolyte concentration is 1 M or below, the concentration of arsine can reach more than 30%; when the electrolyte concentration is increased (1.5-3 M), the concentration of arsine decreases rapidly. This is because the ion transfer flux in the electrolyte becomes larger, the competitive reaction hydrogen evolution reaction rate is faster, and the active hydrogen present in the solution is insufficient to be converted into arsine.
[0047] Example 3: Regulating the concentration of Pd salt to prepare the cathode electrode
[0048] In this Example 3, the Pd salt concentration in the PdFe / NF electrode is regulated to control the ratio of Pd and Fe. The preparation steps of the PdFe / NF electrode are repeated in Example 1. The only difference is that "in the preparation steps of the cathode working electrode, the concentration of K2PdCl4 in the mixed aqueous solution in step 2 is replaced by XM (X refers to the concentration of K2PdCl4)", and other conditions remain unchanged, and the PdFe / NF electrode is finally obtained.
[0049] The PdFe / NF electrode of Example 3 was used to catalytically reduce gray arsenic to prepare arsine by constant current electrolysis. The experimental steps were repeated in Example 1, and a constant current of 3A was selected for the reaction. Other conditions remained unchanged. The arsine concentration was analyzed by gas chromatography after 5 hours / 10 hours of reaction. The test results are shown in Table 3.
[0050] Table 3. Arsenic production at different Pd salt concentrations
[0051]
[0052] As shown in Table 3, the Pd content has a significant effect on the efficiency of converting gray arsenic to arsine. The Pd content in the cathode working electrode can be controlled by regulating the content of the Pd precursor. Specifically, as the Pd content increases, the arsine concentration first increases and then decreases (reaching the best at 0.2M K2PdCl4). This phenomenon may be due to the good adsorption capacity of Pd for the active hydrogen produced by cathode electrolysis. When the content of adsorbed hydrogen reaches a certain level, it is more easily converted into hydrogen, thereby affecting the output of arsine.
[0053] Comparative Example 1: Preparation of cathode working electrode using other metals and Pd doping
[0054] Step 1, placing the nickel foil in a 3M hydrochloric acid solution for 10 minutes to remove the surface oxide layer; then rinsing the surface acid solution with deionized water, and then placing it in acetone for 10 minutes to remove residual organic matter on the surface; finally, rinsing it with deionized water and drying it for later use;
[0055] Step 2, placing the nickel foil obtained in step 1) in a mixed aqueous solution containing 0.5M Y (Y refers to other nitrates) and 0.2M K2PdCl4, and performing electrodeposition at a current of 20 mA in a standard three-electrode system, stopping the deposition when the charge reaches 500C, and washing and drying it for later use;
[0056] Step 3: calcine the electrode obtained in step 2) at 500° C. for 3 h in an Ar atmosphere, cool it to room temperature, rinse it with deionized water and dry it to obtain a PdY / NF electrode.
[0057] Comparative Example 1: PdY / NF electrodes doped with different metals were used to catalytically reduce gray arsenic to prepare arsine by constant current electrolysis. The experimental steps were repeated in Example 1, and a constant current of 3A was selected for the reaction. Other conditions remained unchanged. The arsine concentration was analyzed by gas chromatography after 5 hours / 10 hours of reaction. The test results are shown in Table 4.
[0058] Table 4. Arsenic concentrations of electrodes doped with different metals and Pd (%)
[0059]
[0060] As shown in Table 4, the performance test results of different metals and Pd doping indicate that the Fe element has a unique electronic regulation effect on Pd and can inhibit the hydrogen evolution reaction to a certain extent.
[0061] Comparative Example 2: Preparation of PdFe / Z electrodes by electrodeposition using different substrate materials
[0062] The preparation steps of the cathode working electrode of Comparative Example 2 repeat those of Example 1, with the only difference being that "the nickel foil is replaced by a substrate material Z of the same size (Z refers to other substrate materials, selected from nickel foam, titanium foam, copper foil, nickel foil or platinum sheet)", and other conditions remain unchanged, and finally a PdFe / Z electrode is obtained.
[0063] Comparative Example 2 uses different substrate materials to prepare PdFe / Z electrodes for constant current electrolysis to catalytically reduce gray arsenic to prepare arsine. The experimental steps repeat Example 1, and a constant current of 3A is selected for the reaction. Other conditions remain unchanged. After 5h / 10h of reaction, the arsine concentration is analyzed by gas chromatography. The test results are shown in Table 5.
[0064] Table 5. Arsenic concentration of electrodes prepared from different substrate materials (%)
[0065]
[0066] As shown in Table 5, the performance test results of PdFe / Z electrodes prepared by electrodeposition using different substrate materials show that the nickel substrate material has outstanding performance in the synthesis of arsine due to its good weak hydrogen evolution properties, among which nickel foil is the best substrate.
[0067] Comparative Example 3: Synthesis of Arsine Using Different Arsenic Sources
[0068] 10×10cm 2The double-chamber standard flow electrolyzer with an effective area is a container, and the cathode chamber and the anode chamber are separated by a proton exchange membrane (Nafion 117). 1L 1M KOH alkaline aqueous solution is added to the cathode chamber, and 1L 1M KOH alkaline aqueous solution is added to the anode chamber. Then 700g of different arsenic sources (see Table 6 for details) are added to the cathode and stirred by a magnet. The PdFe / NF prepared in Example 1 is used as the cathode working electrode, the Pt sheet is used as the counter electrode, and the Hg / HgO (1.0M KOH) electrode is used as the reference electrode. The negative and positive electrodes are connected to the electrochemical workstation through wires, respectively, and a constant current of 3A is selected to react. After reacting for 5 hours / 10 hours, the concentration of arsine is analyzed by gas chromatography, and the test results are shown in Table 6.
[0069] Table 6. Arsane concentrations synthesized from different arsenic sources (%)
[0070]
[0071] As shown in Table 6, the performance test results of synthesizing arsine using different arsenic sources indicate that gray arsenic has the best performance in producing arsine, which is attributed to the zero-valent chemical state of gray arsenic. In addition, gray arsenic has better electrical conductivity than other arsenic sources, and this good electron transfer ability has a significant effect on the production of arsine.
[0072] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.
Claims
1. A method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source, characterized in that: A PdFe bimetallic alloy nanoparticle electrode loaded on a nickel foil is used as a working cathode, a counter electrode anode is set, and gray arsenic is used as an arsenic source. Arsine is prepared by catalytic reduction of gray arsenic in an alkaline electrolyte through constant current electrolysis.
2. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 1, characterized in that: The specific steps include: 1) A PdFe bimetallic alloy nanoparticle electrode loaded on nickel foil is used as the working cathode, a carbon or Pt sheet is used as the counter electrode anode, and a double-chamber standard flow electrolytic cell is used as the electrocatalytic reaction device, with the cathode chamber and the anode chamber separated by a proton membrane; 2) Add gray arsenic and alkaline electrolyte to the cathode chamber, add alkaline electrolyte to the anode chamber, and stir the electrolyte in the cathode chamber to fully disperse the gray arsenic; 3) The working cathode and the counter electrode anode are connected to the electrochemical workstation through wires, and the electrolysis system performs constant current electrolysis with a current density of 5-40 mA / cm 2 , to prepare arsine.
3. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 2, characterized in that: In step 2), the alkaline electrolyte is an aqueous solution of one or more of sodium carbonate, potassium carbonate, potassium hydroxide, and sodium hydroxide, and its concentration is 0.1-1.5 M, preferably 0.5-1 M.
4. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 2, characterized in that: In step 2), the amount of gray arsenic added to the cathode electrolyte is 300-800 g / L, preferably 600-700 g / L.
5. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 2, characterized in that: The electrocatalytic reaction time is 5-100 h.
6. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 1, characterized in that: The PdFe bimetallic alloy nanoparticle electrode loaded on nickel foil is marked as PdFe / NF electrode, and its preparation method comprises the following steps: S1: Pre-treating the nickel foil to remove the surface oxide layer and impurities; S2: placing the nickel foil obtained in step S1 in a mixed aqueous solution containing Fe salt and Pd salt, and performing electrodeposition in a standard three-electrode system, wherein the nickel foil is used as a cathode working electrode, the Pt sheet is used as a counter electrode, and a saturated calomel electrode is used as a reference electrode. During the electrodeposition process, Pd and Fe elements are deposited on the nickel foil, and then the nickel foil is rinsed and dried for later use; S3: calcining the electrode obtained in step S2 at 400-600° C. for 1-4 h in an inert gas atmosphere, and cooling to room temperature to obtain the PdFe / NF electrode.
7. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 6, characterized in that: The pretreatment steps in step S1 are: placing the nickel foil in a 2-4 M hydrochloric acid solution and ultrasonically removing the surface oxide layer for 2-20 min, then rinsing the surface acid solution with deionized water, and then placing it in acetone and ultrasonically removing the residual organic matter on the surface, and finally rinsing it with deionized water and drying it, and the treatment is completed.
8. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 6, characterized in that: In step S2, the Pd salt is one of K2PdCl4, Na2PdCl4, PdCl2 and K2PdCl6, and its concentration in the mixed aqueous solution is 0.1-1M; the Fe salt is one of FeCl3, Fe2(SO4)3 and Fe(NO3)3, and its concentration in the mixed aqueous solution is 0.1-1M, preferably 0.5M.
9. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 8, characterized in that: In step S2, the concentration of the Pd salt in the mixed aqueous solution is 0.1-0.3 M, preferably 0.2 M.
10. The method for preparing arsine by electrocatalysis using gray arsenic as an arsenic source according to claim 6, characterized in that: During the electrodeposition, the deposition is stopped when the charge reaches 300-1500 C, preferably when the charge reaches 400-500 C.