Ball-flower-shaped Bi2O2 (OH) (NO3) material, preparation method thereof and application of ball-flower-shaped Bi2O2 (OH) (NO3) material in sodium / potassium ion battery
The synthesis of spherical Bi2O2(OH)(NO3) material in the hydrothermal method was used to adjust the pH and morphology using acetic acid, which solved the volume expansion and conductivity of bismuth-based materials in sodium/potassium ion batteries, significantly improving the battery circulation Stability and specific capacity achieve low-cost and high-performance electrochemical performance.
Patent Information
- Application Number
- CN202310522348.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing bismuth-based materials have volume expansion problems and poor conductivity in sodium/potassium ion batteries, resulting in reduced stability and specific capacity. Existing solutions such as carbon coating and carbon nanotube loading will introduce high pseudocapacitance. Reduce the specific capacity of the platform.
The spherical Bi2O2(OH)(NO3) material was synthesized by hydrothermal method, and acetic acid was used as a soft template and pH adjuster to prepare a material with large crystalline surface layer spacing and uniform bismuth distribution, overcoming the volume expansion problem and improving cycle stability .
It significantly improves the electrochemical performance of sodium/potassium ion batteries. The material has chemical stability and high specific capacity, is low in cost and is easy to prepare, and is suitable for the negative electrode materials of sodium/potassium ion batteries.
Smart Images

Figure HDA0004221364410000011 
Figure HDA0004221364410000012 
Figure HDA0004221364410000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of secondary sodium / potassium ion battery negative electrode materials, and specifically relates to a preparation method of a flower ball-shaped Bi2O2(OH)(NO3) material and application thereof in sodium / potassium ion batteries. Background Art
[0002] With the rapid development of society and the requirements for carbon reduction and emission reduction, people have an increasing demand for batteries with high energy density and high stability. The uneven distribution of lithium resources around the world and the relatively low reserves in the earth's crust (Li 0.0017% vs K 2.09%) have stimulated scientists' interest in developing new rechargeable batteries using other alkali metals as charge carriers. Sodium / potassium ion batteries have extremely high research value and development prospects due to their low cost and similar working principles to lithium ion batteries.
[0003] Alloy-conversion mechanism metal compound materials are widely used in electrode materials due to their high theoretical specific capacity and simple preparation process. Among them, bismuth-based materials have attracted widespread attention due to their high theoretical specific capacity and rich morphology. However, this type of material also has certain defects: ① The process of ion insertion / extraction is accompanied by a large volume change, which leads to reduced stability; ② Poor conductivity. Existing technologies usually solve the above problems through methods such as carbon coating and carbon nanotube loading, but the introduction of carbon materials usually brings higher pseudocapacitance, resulting in a decrease in platform specific capacity.
[0004] Therefore, finding a bismuth-based material with a simple preparation method, low cost, and the ability to effectively overcome the volume expansion problem of the material itself and improve the specific capacity is of great significance for improving the electrochemical performance of sodium / potassium ion batteries. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a flower ball-shaped Bi2O2(OH)(NO3) material and a preparation method thereof and application in sodium / potassium ion batteries. The present invention synthesizes the Bi2O2(OH)(NO3) material by a hydrothermal method, and the obtained material has a large interplanar spacing structure, which can provide abundant redox sites. At the same time, bismuth is evenly distributed in the material, and the large interplanar spacing of the material effectively overcomes the volume expansion problem of the material itself, greatly improving the cyclic stability of the material. The electrode material prepared using the Bi2O2(OH)(NO3) material of the present invention can achieve excellent electrochemical performance.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a flower ball-shaped Bi2O2(OH)(NO3) material comprises the following steps:
[0008] (1) adding a bismuth salt to a nitric acid solution, performing an ultrasonic treatment, adding water to dilute the solution, and then performing a heating treatment to obtain a dilute solution;
[0009] (2) adding urea solution to the dilute solution obtained in step (1) to carry out a reaction; after the reaction is completed, centrifuging, washing, and drying to obtain an intermediate Bi6O5(OH)3(NO3)5·2H2O;
[0010] (3) Add the intermediate Bi6O5(OH)3(NO3)5·2H2O obtained in step (2) to glacial acetic acid and stir to disperse it evenly; then centrifuge and dissolve the obtained solid in water to carry out a hydrothermal reaction; after the reaction is completed, filter, wash and dry to obtain a flower ball-shaped Bi2O2(OH)(NO3) material.
[0011] Preferably according to the present invention, the bismuth salt in step (1) is Bi(NO3)·5H2O or BiCl3.
[0012] Preferably, according to the present invention, the nitric acid solution in step (1) is obtained by mixing concentrated nitric acid with water, the mass fraction of the concentrated nitric acid is 65-68%; and the volume ratio of the concentrated nitric acid to water is 0.05-0.5:1.
[0013] Preferably according to the present invention, the ratio of the molar number of the bismuth salt to the volume of the nitric acid solution in step (1) is 0.2-0.5 mmol:1 mL.
[0014] Preferably, according to the present invention, the ultrasonic treatment time in step (1) is 20-40 min.
[0015] Preferably according to the present invention, in step (1), after ultrasonic treatment, the ratio of the volume of water added to the molar number of the bismuth salt is 10-50 mL:1 mmol.
[0016] Preferably, according to the present invention, the temperature of the heating treatment in step (1) is 40-80° C., and the time of the heating treatment is 20-40 min.
[0017] Preferably according to the present invention, the concentration of the urea solution in step (2) is 0.5-5 mmol / mL; and the molar ratio of the urea to the bismuth salt is 5-10:1.
[0018] Preferably, according to the present invention, the reaction temperature in step (2) is 40-80° C., and the reaction time is 5-25 min.
[0019] Preferably, according to the present invention, the centrifugation step in step (2) is: adding the obtained reaction solution to an equal volume of anhydrous ethanol, centrifuging, and separating the supernatant and the precipitate; the washing is washing the precipitate obtained by centrifugation with deionized water and anhydrous ethanol respectively for 3-5 times; the drying is drying at 60-70°C for 10-12h.
[0020] Preferably, according to the present invention, in step (3), the ratio of the mass of the intermediate Bi6O5(OH)3(NO3)5·2H2O to the volume of glacial acetic acid is 1 g:5-50 mL; and the stirring time is 0.5-1 h.
[0021] Preferably according to the present invention, the ratio of the volume of water in step (3) to the mass of the intermediate Bi6O5(OH)3(NO3)5·2H2O is 50-300mL:1g.
[0022] Preferably, according to the present invention, the temperature of the hydrothermal reaction in step (3) is 120-180° C., and the time of the hydrothermal reaction is 2-10 h.
[0023] Preferably, in step (3), the washing is performed by sequentially washing with water and ethanol; and the drying is performed by drying the solid material obtained by washing at 60-70° C. for 10-12 h.
[0024] The present invention also provides a flower ball-shaped Bi2O2(OH)(NO3) material prepared by the above preparation method; the particle size of a single flower ball of the prepared flower ball-shaped Bi2O2(OH)(NO3) material is 400-600nm.
[0025] According to the present invention, the application of the above-mentioned flower ball-shaped Bi2O2(OH)(NO3) material is used as a negative electrode material for sodium ion batteries or potassium ion batteries; preferably, the specific application method is:
[0026] The prepared flower-ball-shaped Bi2O2(OH)(NO3) material, carbon material, binder and conductive carbon black are mixed and fully ground with water as a dispersant to prepare a negative electrode slurry, and then the battery is assembled and the electrochemical performance is tested according to the conventional sodium ion battery or potassium ion battery related processes; the carbon material is reduced graphene oxide, carbon nanotubes or carbon fibers, and the carbon material plays the role of building a stable conductive network; the binder is sodium carboxymethyl cellulose or PVDF; the mass ratio of the flower-ball-shaped Bi2O2(OH)(NO3) material to the carbon material is 9:(1-9); the mass ratio of the total mass of the flower-ball-shaped Bi2O2(OH)(NO3) material and the carbon material to the binder is 8:1; the mass ratio of the total mass of the flower-ball-shaped Bi2O2(OH)(NO3) material and the carbon material to the conductive carbon black is 8:1; the ratio of the volume of water to the total mass of the flower-ball-shaped Bi2O2(OH)(NO3) material, carbon material, binder and conductive carbon black is 3-5mL:100mg.
[0027] The technical features and beneficial effects of the present invention are as follows:
[0028] 1. The present invention proposes a novel method for controllably synthesizing basic bismuth nitrate and preparing multi-level flower ball morphology by inducing self-assembly using glacial acetic acid as a soft template. The present invention first prepares the intermediate Bi6O5(OH)3(NO3)5·2H2O, which is the product of incomplete hydrolysis of bismuth salt. Then, based on the intermediate and using glacial acetic acid as a soft template, a flower ball-shaped Bi2O2(OH)(NO3) material is obtained through hydrothermal reaction. A specific amount of acetic acid is added in the present invention. The acetic acid molecule not only plays a role in regulating pH during the preparation process, but also reacts with [Bi2O2] 2+ The Bi atoms in the layer coordinate to inhibit the layered stacking of the material, thereby optimizing the morphology, thereby obtaining a flower-ball-shaped Bi2O2(OH)(NO3) material composed of nanosheets of relatively small thickness, and thinner nanosheets and larger interlayer spacing of the crystal planes are more conducive to the performance of excellent electrochemical performance of potassium ion batteries. The present invention controls the crystallinity of the material through the induction and regulation of the morphology by acetic acid molecules, and at the same time regulates the temperature and time in the hydrothermal process, thereby obtaining a potassium ion battery negative electrode material with excellent performance; if the temperature of the hydrothermal reaction is too low, the crystallinity of the obtained product is poor, and if the hydrothermal temperature is too high, the morphology of the obtained material cannot be maintained, and the performance is reduced; if the hydrothermal time is too short, a material with a good morphology cannot be obtained, and if the hydrothermal time is too long, new impurities will be generated, therefore, it is necessary to strictly control the hydrothermal conditions within the scope of the present invention.
[0029] 2. The Bi2O2(OH)(NO3) material prepared by the present invention has the characteristics of stable chemical properties, easy storage, safety, etc. At the same time, the material has structural advantages such as large interlayer spacing, flower ball morphology and large specific surface area. It is used to prepare secondary sodium ion battery / potassium ion battery negative electrode material, and shows electrochemical properties far superior to traditional bismuth-based materials. The soft-pack battery application test shows that the Bi2O2(OH)(NO3) material has practical potential.
[0030] 3. The raw materials used in the present invention, such as bismuth salt, urea, glacial acetic acid, etc., are simple and easy to obtain, low in cost, and the preparation process is simple and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The scanning electron microscope photograph (a) and X-ray powder diffraction pattern (b) of the intermediate Bi6O5(OH)3(NO3)5·2H2O prepared in Example 1.
[0032] Figure 2 The scanning electron microscope photograph (a), transmission electron microscope photograph (b) and powder X-ray diffraction pattern (c) of the flower ball-shaped Bi2O2(OH)(NO3) material prepared in Example 1.
[0033] Figure 3 These are the specific capacity and efficiency-cycle diagrams of the potassium ion battery prepared with the Bi2O2(OH)(NO3)-rGO negative electrode in Example 1 at current densities of 100 mA / g (a) and 50 mA / g (b).
[0034] Figure 4 This is the constant current charge and discharge curve of the potassium ion battery prepared with the Bi2O2(OH)(NO3)-rGO negative electrode in Example 1 at a current density of 50 mA / g.
[0035] Figure 5 This is the charge-voltage differential curve of the potassium ion battery prepared with the Bi2O2(OH)(NO3)-rGO negative electrode in Example 1.
[0036] Figure 6 This is the constant current charge and discharge curve of the sodium ion battery prepared with the Bi2O2(OH)(NO3)-rGO negative electrode in Example 1 at a current density of 25 mA / g.
[0037] Figure 7 This is the charge-voltage differential curve of the potassium ion battery prepared with the Bi2O2(OH)(NO3)-rGO negative electrode in Example 2.
[0038] Figure 8 This is a scanning electron microscope photograph of the flower ball-shaped Bi2O2(OH)(NO3) material prepared in Example 3.
[0039] Fig. 9 : is the X-ray powder diffraction pattern of the bismuth oxide material prepared in Comparative Example 1.
[0040] Fig.10 This is a cycle diagram of a potassium ion battery prepared from the bismuth oxide material obtained in Comparative Example 1 at a current density of 50 mA / g.
[0041] Fig.11 This is a transmission electron microscope scanning image of the large block Bi2O2(OH)(NO3) obtained in Example 2 (a) and the constant current charge and discharge performance of the potassium ion battery prepared with it as the negative electrode at a current density of 50 mA / g (b, c, d). DETAILED DESCRIPTION
[0042] The present invention is specifically described below through embodiments, which are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential improvements and adjustments to the present invention based on the contents of the above invention.
[0043] The mass fraction of concentrated nitric acid used in the embodiment is 65-68%; the nitric acid solution used is obtained by mixing concentrated nitric acid with water.
[0044] Example 1
[0045] A method for preparing a flower ball-shaped Bi2O2(OH)(NO3) material comprises the following steps:
[0046] (1) 4 mmol Bi(NO3)·5H2O was added to 15 mL nitric acid solution (the volume ratio of concentrated nitric acid to water in the nitric acid solution was 2:13), and after ultrasonic treatment for 30 min, 80 mL deionized water was added to dilute it, and then heated in a water bath at 60°C and stirred for 30 min to obtain a dilute solution.
[0047] (2) Add urea solution (prepared by 40 mmol urea and 20 mL deionized water) to the dilute solution obtained in step (1), continue to heat in a water bath at 60°C and stir to react for 15 min; after the reaction is completed, pour the resulting reaction solution into an equal volume of anhydrous ethanol, centrifuge, and separate the supernatant and the precipitate; wash the resulting precipitate with deionized water and anhydrous ethanol three times respectively, and dry the washed material at 60°C for 10 h to obtain the intermediate Bi6O5(OH)3(NO3)5·2H2O.
[0048] (3) Weigh 0.4 g of the intermediate Bi6O5(OH)3(NO3)5·2H2O obtained in step (2) and add it to 5 mL of glacial acetic acid, stir for 1 h to fully disperse it; centrifuge the obtained suspension at 10,000 rpm for 5 min, decant to remove the glacial acetic acid, and then add 30 mL of deionized water to the centrifuge tube to dissolve the solid at the bottom of the tube to obtain a clear solution; transfer the obtained clear solution to a 40 mL Teflon liner and perform hydrothermal reaction at 150° C. in an autoclave for 5 h; after the reaction is completed, cool naturally to room temperature, filter, wash the obtained solid with deionized water and ethanol, and then dry the obtained solid material at 60° C. for 10 h to obtain a flower ball-shaped Bi2O2(OH)(NO3) material.
[0049] Figure 1 a is a scanning electron microscope photo of the intermediate prepared in this example, and it can be found that the material is a large block morphology; and from its XRD characterization results ( Figure 1 b) It can be seen that the intermediate is Bi6O5(OH)3(NO3)5·2H2O (PDF#54-0627).
[0050] Figure 2 a, Figure 2 b is a scanning electron microscope photo and a transmission electron microscope photo of the flower-ball-shaped Bi2O2(OH)(NO3) material obtained in this example. It can be found that the material has a multi-level flower-ball structure and a large specific surface area; and according to its XRD characterization results ( Figure 2 c) It can be seen that the material has strong crystallinity and strong diffraction peaks at small angles, which proves that its large interlayer spacing crystal planes account for a large proportion in the entire crystal structure, which is beneficial to its stability.
[0051] The flower-ball-shaped Bi2O2(OH)(NO3) material prepared in this embodiment is used as a negative electrode material to prepare a potassium ion battery, and its electrochemical performance is tested. The specific steps are as follows:
[0052] The prepared flower-ball-shaped Bi2O2(OH)(NO3) material, reduced graphene oxide, sodium carboxymethyl cellulose, and conductive graphite were mixed in a mass ratio of 4:4:1:1 and fully ground in a mortar with water as a dispersant for 30 minutes to prepare a negative electrode slurry, and the ratio of the volume of water to the total mass of the flower-ball-shaped Bi2O2(OH)(NO3) material, reduced graphene oxide, sodium carboxymethyl cellulose, and conductive graphite was 4mL:100mg. The slurry was coated on aluminum foil and scraped to obtain a negative electrode sheet. The loading amount of the flower-ball-shaped Bi2O2(OH)(NO3) material was 1.2mg / mm 2 .
[0053] Battery assembly and testing: The negative electrode sheet was pressed into an electrode sheet, and the metal potassium was used as the positive electrode. The electrolyte was 5 mol / L KFSI electrolyte, and the battery was assembled in a glove box filled with argon. At room temperature, the charge and discharge cycle test was carried out at a current density of 50 mA / g and 100 mA / g.
[0054] Figure 3 The charge-discharge cycle diagrams in a and b prove that the material has extremely high specific capacity and cycle stability at different current densities. Figure 4 The constant current charge and discharge curves in the figure prove that the potassium ion battery built on the basis of Bi2O2(OH)(NO3) material has a voltage platform consistent with the theoretical value: the 0.8V and 0.4V platforms prove that the Bi2O2(OH)(NO3) material participates in the electrochemical storage of potassium, and there is no charge and discharge platform corresponding to the side reaction.
[0055] Figure 5 The voltage differential curve of the potassium ion battery prepared with Bi2O2(OH)(NO3)-rGO negative electrode was tested by cyclic voltammetry at a rate of 50mV / s, with a voltage range of 0 to 3V. Figure 5 It can be seen that the redox process of Bi2O2(OH)(NO3) material during potassium storage is similar to Figure 4 The voltage platforms of the constant current charge and discharge curves confirm each other.
[0056] The flower-ball-shaped Bi2O2(OH)(NO3) material prepared in this embodiment is used as the negative electrode material to prepare a sodium ion battery and test its electrochemical performance. The specific steps are as follows: the preparation of the negative electrode sheet is the same as that of the potassium ion battery; the battery assembly and testing: the negative electrode sheet is pressed into an electrode sheet, and the battery is assembled in a glove box filled with argon gas using metallic sodium as the positive electrode, the electrolyte is 5 mol / L sodium hexafluorophosphate electrolyte, and the diaphragm is a conventional sodium electric diaphragm (glass fiber diaphragm). At room temperature, the charge and discharge cycle test is carried out at a current density of 25 mA / g.
[0057] Figure 6 The sodium ion battery prepared with Bi2O2(OH)(NO3)-rGO negative electrode was charged and discharged at a constant current density of 25mA / g, and it was found that it also had high reversibility and specific capacity.
[0058] Example 2
[0059] A method for preparing a flower ball-shaped Bi2O2(OH)(NO3) material comprises the following steps:
[0060] (1) 4.8 mmol Bi(NO3)·5H2O was added to 15 mL nitric acid solution (the volume ratio of concentrated nitric acid to water in the nitric acid solution was 3:12), and after ultrasonic treatment for 30 min, 85 mL deionized water was added for dilution, and then heated in a water bath at 80°C and stirred for 30 min to obtain a dilute solution.
[0061] (2) Add urea solution (composed of 30 mmol urea and 20 mL deionized water) to the dilute solution obtained in step (1), continue heating in a water bath at 80°C and stirring the reaction for 15 min; after the reaction is completed, pour the resulting reaction solution into an equal volume of anhydrous ethanol, centrifuge, and separate the supernatant and the precipitate; wash the resulting precipitate with deionized water and anhydrous ethanol three times respectively, and dry the washed material at 60°C for 10 h to obtain the intermediate Bi6O5(OH)3(NO3)5·2H2O.
[0062] (3) Weigh 0.4 g of the intermediate Bi6O5(OH)3(NO3)5·2H2O obtained in step (2) and add it to 10 mL of glacial acetic acid, stir for 1 h to fully disperse it; centrifuge the obtained suspension at 10,000 rpm for 5 min, decant to remove the glacial acetic acid, and then add 30 mL of deionized water to the centrifuge tube to dissolve the solid at the bottom of the tube to obtain a clear solution; transfer the obtained clear solution to a 40 mL Teflon liner and perform a hydrothermal reaction at 150° C. in an autoclave for 5 h; after the reaction is completed, cool naturally to room temperature, filter, wash the obtained solid with deionized water and ethanol, and then dry the obtained solid material at 60° C. for 10 h to obtain a flower ball-shaped Bi2O2(OH)(NO3) material.
[0063] The battery was assembled as described in Example 1. Cyclic voltammetry was performed at a rate of 50 mV / s with a voltage range of 0 to 3 V. Figure 7 Its charge voltage differential curve.
[0064] Example 3
[0065] A method for preparing a flower-ball-shaped Bi2O2(OH)(NO3) material is as described in Example 1, except that in step (3), a hydrothermal reaction is carried out at 180°C for 5 hours to obtain a flower-ball-shaped Bi2O2(OH)(NO3) material.
[0066] The scanning electron microscope photograph of the flower-shaped Bi2O2(OH)(NO3) material obtained in this example is as follows: Figure 8 As shown by Figure 8 It can be seen that compared with Example 1, the product obtained at this temperature is larger in size and has a slightly worse morphology.
[0067] Comparative Example 1
[0068] A method for preparing a bismuth oxide material is as described in Example 1, except that in step (3), a hydrothermal reaction is performed at 60° C. for 5 h to obtain a bismuth oxide material.
[0069] The XRD spectrum of the bismuth oxide material obtained in this comparative example is as follows Fig. 9 As shown by Fig. 9 It can be seen that the crystallinity of the material deteriorates.
[0070] The battery was assembled as described in Example 1 and was heated at 50 mA g -1 The cycle curve under current density is as follows Fig.10 As shown by Fig.10 It can be seen that the crystallinity of the material deteriorates, the capacity of the prepared battery is significantly attenuated and the stability is reduced.
[0071] Comparative Example 2
[0072] A method for preparing a bulk Bi2O2(OH)(NO3) material comprises the following steps:
[0073] 1 mmol Bi(NO3)·5H2O was added to 30 mL water, ultrasonicated for 30 min and stirred for 30 min, and the evenly dispersed solution was poured into a 40 mL Teflon liner; then placed in a high temperature and high pressure reactor, hydroheated at 150°C for 5 h, and the obtained precipitate was washed three times with deionized water and anhydrous ethanol respectively, and the washed material was dried at 60°C for 10 h to obtain large block morphology of Bi2O2(OH)(NO3).
[0074] Fig.11 (a) is the TEM characterization result of the material. It can be found that the product morphology obtained without intermediates and acetic acid regulation is large block-like.
[0075] The battery was assembled and tested as described in Example 1. Fig.11 (b) The specific capacity-cycle number curve shows that the capacity of the material is constantly decreasing. Fig.11 (c-d) The charge-discharge curves show that the bulk Bi2O2(OH)(NO3) completely loses its platform capacity after ten cycles and has no use value, indicating the key role of intermediate processing and acetic acid regulation.
Claims
1. A method for preparing a flower-shaped Bi2O2(OH)(NO3) material, comprising the following steps: (1) adding a bismuth salt to a nitric acid solution, ultrasonically treating the solution, diluting the solution with water, and then heating the solution to obtain a dilute solution; (2) adding urea solution to the dilute solution obtained in step (1) to carry out a reaction; after the reaction is completed, centrifuging, washing, and drying to obtain an intermediate Bi6O5(OH)3(NO3)5·2H2O; (3) The intermediate Bi6O5(OH)3(NO3)5·2H2O obtained in step (2) is added to glacial acetic acid and stirred to disperse uniformly; then centrifuged, the obtained solid is dissolved in water, and a hydrothermal reaction is carried out; after the reaction is completed, the mixture is filtered, washed, and dried to obtain a flower ball-shaped Bi2O2(OH)(NO3) material.
2. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The bismuth salt in step (1) is Bi(NO3)·5H2O or BiCl3; The nitric acid solution is obtained by mixing concentrated nitric acid with water, wherein the mass fraction of the concentrated nitric acid is 65-68%; and the volume ratio of the concentrated nitric acid to water is 0.05-0.5:1; The ratio of the molar number of the bismuth salt to the volume of the nitric acid solution is 0.2-0.5 mmol:1 mL.
3. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The ultrasonic treatment time in step (1) is 20-40 min; after the ultrasonic treatment, the ratio of the volume of water added to the molar number of the bismuth salt is 10-50 mL:1 mmol.
4. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The temperature of the heating treatment is 40-80° C., and the time of the heating treatment is 20-40 minutes.
5. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The concentration of the urea solution in step (2) is 0.5-5 mmol / mL; the molar ratio of the urea to the bismuth salt is 5-10:
1.
6. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The reaction temperature in step (2) is 40-80° C., and the reaction time is 5-25 min; The centrifugation step comprises: adding the obtained reaction solution to an equal volume of anhydrous ethanol, centrifuging, and separating the supernatant and the precipitate; the washing step comprises washing the precipitate obtained by centrifugation with deionized water and anhydrous ethanol respectively for 3-5 times; and the drying step comprises drying at 60-70° C. for 10-12 hours.
7. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: In step (3), the ratio of the mass of the intermediate Bi6O5(OH)3(NO3)5·2H2O to the volume of glacial acetic acid is 1 g:5-50 mL; and the stirring time is 0.5-1 h.
8. The method for preparing the flower-shaped Bi2O2(OH)(NO3) material according to claim 1, characterized in that: The ratio of the volume of water in step (3) to the mass of the intermediate Bi6O5(OH)3(NO3)5·2H2O is 50-300 mL:1 g; The temperature of the hydrothermal reaction is 120-180°C, and the time of the hydrothermal reaction is 2-10 hours; The washing step comprises washing with water and ethanol in sequence; and the drying step comprises drying the solid material obtained by washing at 60-70° C. for 10-12 hours.
9. A flower ball-shaped Bi2O2(OH)(NO3) material, characterized in that: The preparation method according to claim 1 is used for preparation.
10. Use of the flower-ball-shaped Bi2O2(OH)(NO3) material according to claim 9 as a negative electrode material for sodium ion batteries or potassium ion batteries.
Citation Information
Patent Citations
Basic bismuth nitrate nonlinear crystal material and preparation method and application thereof
CN102127810A
Flaky bismuth subnitrate and preparation method thereof
CN109911936A
Method for synthesizing basic bismuth nitrate / bismuth oxide composite material
CN114367301A