Preparation method of high-performance porous manganese oxide material for aqueous zinc ion battery positive electrode
By using potassium permanganate and maleic acid to prepare porous manganese oxide, the problems of low capacity and poor circulation stability of zinc ion battery positive electrode material are solved, and a zinc ion battery positive electrode material with high specific capacity and good circulation stability are achieved.
Patent Information
- Application Number
- CN202411177593.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The performance of the positive electrode material of zinc ion batteries is limited, resulting in the problems of low capacity and poor cycle stability.
Potassium permanganate and maleic acid were used as raw materials to prepare porous manganese oxide by water bath heating method and high-temperature carbonization method to form a positive electrode material with high specific surface area and active sites.
The high specific capacity and good cycle stability of the positive electrode material of zinc ion battery are achieved, reducing the preparation cost and improving performance.
Smart Images

Figure CN118929759A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing high-performance porous manganese oxide for positive electrode materials of aqueous zinc ion batteries, and belongs to the field of zinc ion battery energy storage. Background Art
[0002] With the intensification of the global energy crisis and the continuous exploration of electrochemical energy storage, high-performance batteries have been constantly coming into people's eyes. At present, lithium-ion batteries with high energy density and high specific capacity are the most common commercial batteries. However, the lack of lithium resources and high cost, low power density, safety issues and environmental pollution still hinder its further application. In recent years, aqueous zinc-ion batteries have been considered as a very promising alternative due to their low cost, high safety, green and pollution-free advantages. Aqueous zinc-ion batteries have suitable redox potentials and high specific capacity, etc. However, due to the constraints of the performance of the positive electrode materials, it is still challenging to find suitable positive electrode materials to develop zinc-ion batteries.
[0003] Manganese oxide is one of the strong candidates for positive electrode materials because of its low price, easy availability, and non-toxicity. Manganese-based materials can store zinc ions in various oxidation states and crystal structures. The basic crystal structure of manganese dioxide is an octahedral unit composed of 6 oxygen atoms and 1 manganese atom. The MnO6 octahedral units are interconnected to form a tunnel structure, and the size of the tunnel structure is determined by the number of MnO6 octahedra. These tunnel structures can allow Zn 2+ Shuttle, realize Zn 2+ Storage. Manganese-based materials also face problems such as dissolution, insufficient conductivity, and insufficient specific capacity when applied on a large scale. MnO has been shown to be a viable cathode material for aqueous zinc-ion batteries, but its lack of tunnel structure and strong electrostatic interaction with guest ions lead to poor performance of Zn / MnO batteries. The porous manganese oxide structure not only introduces abundant Mn vacancies to improve the Zn 2+ The diffusion of MnO is improved, and the specific surface area and pore size of MnO are increased to improve the wettability of the cathode to the electrolyte. Summary of the invention
[0004] In view of the problem of low capacity of existing zinc ion manganese-based positive electrode materials, the purpose of the present invention is to provide a method for preparing porous manganese oxide for manganese-based positive electrodes of zinc ion batteries. The preparation method is simple to synthesize and has low cost. When used as a positive electrode material for zinc ion batteries, it exhibits high specific capacity and good cycle stability.
[0005] The method for preparing porous manganese oxide for the positive electrode of a zinc ion battery provided by the present invention mainly comprises the following steps:
[0006] Step (1) measuring a certain amount of KMnO4 and pouring it into a beaker, measuring an appropriate amount of deionized water and pouring it into the beaker and stirring to prepare a KMnO4 solution;
[0007] Step (2) adding a certain amount of maleic acid to the KMnO4 solution obtained in step (1) and continuously stirring until the maleic acid is completely dissolved to obtain a mixed solution;
[0008] Step (3) transferring the mixed solution obtained in step (2) into a round-bottom flask and heating it in a water bath. After the reaction is completed, a manganese oxide mixed solution is obtained;
[0009] Step (4) centrifuging the manganese oxide mixed solution obtained in step (3), and then drying to obtain a dry manganese oxide precursor;
[0010] Step (5) The manganese oxide precursor obtained in step (4) is transferred to a clean magnetic boat and placed in a tubular carbonization furnace for high-temperature carbonization in an inert gas to obtain porous manganese oxide.
[0011] Preferably, in step (1), the concentration of KMnO4 solution is 0.1-1M; the stirring time is between 0.5-1 hour;
[0012] Preferably, in step (2), the molar ratio of KMnO4 to maleic acid is 1:1-1:5, and the vigorous stirring time should be between 0.2-0.5 hours;
[0013] Preferably, the water bath heating temperature in step (3) is 30°C-60°C, and the time is 12-18 hours;
[0014] Preferably, in step (4), the oven temperature is set to 80-120° C. for 6-12 hours;
[0015] Preferably, in step (4), the carbonization temperature is 350° C.-700° C., and the carbonization time is 4-8 hours; the carbonization yield of the sample is between 30% and 50%.
[0016] The present invention has the following advantages:
[0017] (1) Using potassium permanganate as a manganese source, the manganese oxide prepared by a water bath heating method and a high temperature carbonization method has a high specific surface area;
[0018] (2) Compared with other manganese oxides, porous manganese oxide has more active sites;
[0019] (3) The prepared porous manganese oxide has a high specific capacity and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the rate curve of the sample obtained in Example 3.
[0021] Figure 2 This is a scanning electron microscope image of the sample obtained in Example 3. DETAILED DESCRIPTION
[0022] The present invention is further described below by way of specific embodiments, but is not intended to limit the present invention.
[0023] Embodiment 1:
[0024] Weigh 7.9g potassium permanganate and dissolve it in 200mL distilled water, stir for 0.5h to prepare 0.25M potassium permanganate solution, measure 0.2mol maleic acid solution and add it to the potassium permanganate solution, stir for 0.5h to obtain a uniform mixed solution. Add the mixed solution to a round-bottom flask and heat it in a water bath at 50°C for 12h. Filter the prepared suspension and then wash it, and dry the prepared sample at 80°C for 12h. Transfer the dried sample to a magnetic boat and place it in a tubular carbonization furnace for high-temperature carbonization in an Ar atmosphere, starting from 25°C, heating at a heating rate of 5°C / min to 600°C, and keep it warm for 4 hours.
[0025] Embodiment 2:
[0026] The mass of potassium permanganate was changed to 15.8 g, and the other conditions were the same as in Example 1.
[0027] Embodiment 3:
[0028] The mass of potassium permanganate was changed to 11.85 g, and the other conditions were the same as in Example 1.
[0029] Embodiment 4:
[0030] The amount of maleic acid was changed to 0.4 mol, and the other conditions were the same as in Example 1.
[0031] Embodiment 5:
[0032] The water bath temperature was changed to 40°C, and other conditions were the same as in Example 1.
[0033] Embodiment 6:
[0034] The water bath time was changed to 18 h, and other conditions were the same as in Example 1.
[0035] Embodiment 7:
[0036] The carbonization temperature was changed to 400°C, and the other conditions were the same as in Example 1.
[0037] Embodiment 7:
[0038] The carbonization time was changed to 6 h, and the other conditions were the same as in Example 1.
[0039] Some embodiments of the present invention have been described in detail above, but the present invention is not limited to the embodiments. Those skilled in the art may make equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. The method for preparing porous manganese oxide for positive electrode of zinc ion battery provided by the present invention uses potassium permanganate as manganese source and prepares a precursor by heating in a water bath; then carbonizes the precursor in an Ar atmosphere to obtain a porous manganese oxide material. The main preparation steps are as follows: (1) Weigh a certain amount of KMnO4 into a beaker, add an appropriate amount of deionized water and stir to prepare a KMnO4 solution; (2) adding a certain amount of maleic acid to the KMnO4 solution obtained in step (1) and continuously stirring until the KMnO4 solution is completely dissolved to obtain a mixed solution; (3) transferring the mixed solution obtained in step (2) into a round-bottom flask and heating it in a water bath. After the reaction is completed, a manganese oxide mixed solution is obtained; (4) centrifuging the manganese oxide mixed solution obtained in step (3), and then drying to obtain a dry manganese oxide precursor; (5) The manganese oxide precursor obtained in step (4) is transferred to a clean magnetic boat and placed in a tubular carbonization furnace for high-temperature carbonization in an inert gas to obtain porous manganese oxide.
2. The method according to claim 1, characterized in that The concentration of the KMnO4 solution in step (1) is 0.1-1M; the stirring time is between 0.5-1 hour.
3. The method according to claim 1, characterized in that In step (2), the molar ratio of KMnO4 to maleic acid is 1:1-1:5, and the vigorous stirring time should be between 0.2-0.5 hours.
4. The method according to claim 1, characterized in that The water bath heating temperature in step (3) is 30°C-60°C and the heating time is 12-18 hours.
5. The method according to claim 1, characterized in that In step (4), the oven temperature is set to 80-120° C. and the time is 6-12 hours.
6. The method according to claim 1, characterized in that The carbonization temperature of step (5) is 350° C.-700° C., and the carbonization time is 4-8 hours; the carbonization yield of the sample is between 30% and 50%.
7. A porous manganese oxide material for a positive electrode of a zinc ion battery prepared by the method according to any one of claims 1 to 6, characterized in that: The prepared material has a high specific capacity and good cycle performance. Its electrochemical performance is tested with 2mol / LZnSO4 and 0.5mol / LMnSO4 as electrolytes. The rate performance is excellent, and the specific capacity reaches 151mAh / g at a current density of 0.1A / g; after a series of rate changes, its performance can be restored to the initial performance. The coulombic efficiency is close to 100%, and the electrochemical performance is excellent.
Citation Information
Patent Citations
Method for preparing porous MnO2 by simple calcining method
CN111533171A
Preparation method of porous manganese sesquioxide positive electrode material and application of porous manganese sesquioxide positive electrode material in aqueous zinc ion battery
CN115440972A
Carbon-coated manganous-manganic oxide submicron spherical shell material as well as preparation method and application thereof
CN115724469A
Method for preparing self-supporting manganese-carbon positive electrode material of aqueous zinc ion battery
CN117766724A
Method for producing manganese dioxide porous material, manganese dioxide porous material, electrode material and power storage device