High-nickel layered oxide positive electrode material with high-entropy surface and medium-entropy gradient doping inside and preparation method of high-nickel layered oxide positive electrode material
By using a variety of metal sources for bulk phase and surface doping in high-nickel layered oxide positive electrode materials, a high-entropy reconstruction layer and a medium-entropy doping structure are formed, and the stability and energy density of the material in lithium-ion batteries are solved. The improvement problem has achieved higher cycle stability and excellent performance.
Patent Information
- Application Number
- CN202410959486.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-17
AI Technical Summary
High-nickel layered oxide positive electrode materials have problems such as surface instability, deep side reactions, lithium ion inactivation and structural changes in lithium ion batteries. The prior art cannot effectively solve the micro-swell caused by the expansion of the cladding layer and the bulk phase. Crack problem.
A variety of metal sources are used for bulk-phase doping and surface reconstruction to form a surface high-entropy reconstruction layer and an internal mid-entropy doping structure. Through multivariate synergistic action, the nickel valence state is reduced and the volume expansion and contraction is alleviated, and the generation of microcracks is reduced.
It significantly improves the cycle stability and energy density of high-nickel layered oxide positive electrode materials, reduces side reactions and lithium-nickel mixed discharge, and enhances the stability and performance of the electrode materials.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion battery electrode materials, and specifically relates to a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are widely used due to their advantages such as high energy density, long cycle life, low self-discharge and no memory effect. With the rapid development of electric vehicles and portable electronic devices, the energy density of existing lithium-ion batteries can no longer meet the current demand for long battery life. Since the positive electrode material of lithium-ion batteries is the main factor limiting the improvement of battery energy density and achieving long battery life, the use of high energy density positive electrode materials has become the preferred way to improve lithium-ion batteries.
[0003] In recent years, high nickel layered oxide cathode materials have rapidly become the preferred raw materials for high energy density batteries due to their high reversible specific capacity. However, high nickel layered oxide cathode materials still face many challenges in their application: for example, during the charging process, the unstable Ni 4+ Ions can easily cause side reactions, such as electrolyte decomposition, metal ion dissolution, and lattice oxygen release. For example, during the cycle, the expansion and contraction of the lattice causes microcracks, which in turn exponentially increases the interface area between the positive electrode and the electrolyte, allowing the interface side reactions to penetrate deep into the material particles. For example, during the charge and discharge process, Ni in the transition metal layer 2+ They will migrate to the lithium layer, occupy lithium vacancies to form cation mixing, causing a large number of lithium ions to be inactivated. At the same time, the structural change will bring about adverse irreversible phase changes and lattice oxygen release.
[0004] For the problems existing in high-nickel layered oxide positive electrode materials, the common practice in the prior art is to use surface coating and bulk doping to collaboratively achieve the modification of layered oxides. Among them, surface modification (surface coating) can form a chemically inert protective layer, inhibit the decomposition of the electrolyte, slow down the decay of the surface structure, and effectively improve the stability of the electrode-electrolyte interface. Bulk doping can improve the electronic structure outside the transition metal, enhance the bond energy of the transition metal ion and the oxygen bond, and increase the electronic conductivity of the material, inhibit lithium-nickel mixing, and alleviate the crystal expansion and lattice oxygen release during the charge and discharge process. For this, there are also some reports in the prior art. For example, the Chinese patent with publication number CN105118967A discloses a metal oxide coated modified doped ternary positive electrode material and a preparation method thereof, which is modified by coating and bulk doping of high-nickel layered oxides of lithium ion batteries, so that it has higher electronic conductivity and cycle stability, but this patent cannot solve the problem of microcracks caused by different volume expansion of the coating layer and bulk phase of the high-nickel layered oxide electrode.
[0005] Based on the problems existing in the prior art, the present invention uses a variety of metal sources as dopants to perform bulk doping and surface reconstruction on high-nickel layered oxide positive electrode materials (such as NCM) for lithium-ion batteries, and adjusts the type of dopants, process parameters and specific implementation procedures to achieve improved electrochemical properties such as energy density and cycle stability of the positive electrode material. Summary of the invention
[0006] The purpose of the present invention is to address the deficiencies in the prior art and propose a high-nickel layered oxide positive electrode material with high entropy on the surface and medium entropy inside and a preparation method thereof, by doping the surface of the material with five or more elements to form a surface high entropy reconstruction layer, and at the same time doping the material with four elements inside to form a medium entropy doping structure. Among them, the high entropy reconstruction layer on the surface can utilize the synergistic effect of multiple elements to form a superlattice structure on the surface and reduce the valence state of the surface nickel to achieve the stability of the interface structure and reduce the occurrence of side reactions with the electrolyte. In addition, the hierarchical structure of the surface high entropy reconstruction layer and the internal medium entropy doping structure can alleviate the lattice mismatch during volume expansion and contraction and reduce the generation of microcracks. This method can significantly improve the cycle stability of nickel-rich layered oxide positive electrode materials, is a method with simple process, low cost, convenient operation, excellent performance, and has a prospect for industrial production and application.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0008] A method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping, comprising the following steps:
[0009] 1) uniformly mixing a high nickel layered oxide precursor, a metal doping precursor and a lithium source in a certain proportion, and then placing the mixture in an atmosphere furnace, and sintering the mixture once under a modified atmosphere to obtain a doped high nickel layered oxide positive electrode material;
[0010] 2) The high nickel layered oxide positive electrode material in step 1) is uniformly mixed with the metal doped precursor 2 in a certain proportion, and then placed in an atmosphere furnace for secondary sintering under a modified atmosphere to obtain a high nickel layered oxide positive electrode material with high surface entropy and medium internal entropy.
[0011] Furthermore, the chemical formula of the high nickel layered oxide precursor in step 1) is Ni 1-x-y-z Co x Mn y Al z (OH)2, x>0, y>0, z>0, 0.6≤(1-xyz)<1.
[0012] Further preferably, in step 1), the chemical formula of the high nickel layered oxide precursor is Ni 0.96 Co0.015 Mn 0.015 Al 0.01 (OH)2.
[0013] Furthermore, the metal-doped precursor described in step 1) is one or more of metal oxides, metal nitrates, metal sulfates, metal acetates, metal carbonates, and metal organic salts; preferably, the metal described in step 1) is one or more of sodium, magnesium, potassium, calcium, scandium, titanium, vanadium, chromium, iron, copper, zinc, gallium, germanium, yttrium, zirconium, niobium, molybdenum, tantalum, tungsten, lanthanum, neodymium, cerium, and europium.
[0014] Furthermore, the lithium source in step 1) is any one of lithium carbonate and lithium hydroxide.
[0015] Further preferably, in step 1), the molar ratio of the high nickel layered oxide precursor to the metal doping precursor and the lithium source is 1:(0.00005-0.1):(1-1.2). Further, the primary sintering in step 1) includes a first stage sintering and a second stage sintering.
[0016] Further preferably, the temperature of the first sintering stage is 200-670° C.; the time of the first sintering stage is 1-9 hours; the temperature of the second sintering stage is 600-900° C.; the time of the second sintering stage is 6-24 hours.
[0017] Furthermore, the metal-doped precursor 2 described in step 2) is one or more of metal oxides, metal nitrates, metal sulfates, metal acetates, metal carbonates, and metal organic salts; preferably, the metal element in step 2) is one or more of sodium, magnesium, potassium, calcium, scandium, titanium, vanadium, chromium, iron, copper, zinc, gallium, germanium, yttrium, zirconium, niobium, molybdenum, tantalum, tungsten, lanthanum, neodymium, cerium, and europium, and is different from the metal element selected in the metal-doped precursor 1 in step 1).
[0018] Further preferably, in step 2), the molar ratio of the high nickel layered oxide precursor to the metal doped precursor 2 is 1:(0.00005-0.1).
[0019] Furthermore, the secondary sintering temperature in step 2) is 300-900° C., and the sintering time is 0.5-15 h.
[0020] Furthermore, the modified atmosphere in step 1) and step 2) is an oxygen atmosphere, a nitrogen atmosphere, an ammonia atmosphere, a sulfur dioxide atmosphere, a hydrogen sulfide atmosphere, or a combination atmosphere of any two of these five gases, or a combination atmosphere of any three of these five gases, or a combination atmosphere of any four of these five gases, or a combination atmosphere of five gases.
[0021] Further preferably, when the modified atmosphere is a mixture of two gases, the ratio of the mixture is oxygen: other gas = (6-10): (1-4), and the other gas refers to nitrogen, ammonia, sulfur dioxide or hydrogen sulfide.
[0022] Furthermore, the present invention prepares a high-entropy surface and medium-entropy internal hierarchically doped high-nickel layered oxide positive electrode material through the above-mentioned surface modification method, which has good capacitance and charge-discharge performance and can be used to prepare lithium-ion batteries.
[0023] Furthermore, based on a general inventive concept, the present invention also provides the use of the surface high-entropy and internal medium-entropy stepwise doped high-nickel layered oxide positive electrode material in the preparation of lithium-ion batteries.
[0024] Furthermore, the present invention also provides a method for preparing a lithium-ion battery using the surface high-entropy and internal medium-entropy stepwise doped high-nickel layered oxide positive electrode material, which specifically comprises the following steps:
[0025] a. placing a certain amount of surface high entropy internal medium entropy stepwise doped high nickel layered oxide positive electrode material, a conductive agent and a binder in a container to obtain a mixed powder;
[0026] b. Add a solvent to the mixed powder in step a, ultrasonically disperse it at a power of 80 to 100 W for 8 to 12 minutes, then place a polytetrafluoroethylene magnet in a container and stir it at a speed of 300 to 400 r / min for 8 to 12 hours to uniformly disperse the high-nickel layered oxide cathode material and the conductive agent to obtain a mixed slurry;
[0027] c. Coat the mixed slurry in step b on aluminum foil (current collector), dry it at 60-80°C for 8-12h, and then make it into a button-type electrode sheet with a diameter of 12mm; then use the prepared electrode sheet as the working electrode, the metal lithium sheet as the counter electrode, install a diaphragm, and use a high-nickel 4.3V electrolyte to assemble a button battery. The battery model is a CR2032 button battery.
[0028] Specifically, in step a, the conductive agent is carbon black (Super-P); and the binder is PVDF.
[0029] Specifically, the solvent is selected from one of deionized water, ethanol and NMP.
[0030] Specifically, the mass of the solvent is 1 to 1.5 times the mass of the mixed powder.
[0031] Specifically, in the mixed slurry obtained in step b, the weight ratio of the high-entropy surface and medium-entropy internal hierarchically doped high-nickel layered oxide positive electrode material, the conductive agent, and the binder is (16-18):1:(1-2).
[0032] Specifically, the diaphragm type is a polypropylene diaphragm, and the main component of the electrolyte used in the battery is: lithium salt (lithium hexafluorophosphate); preferably, the electrolyte is 1M LiPF6 in EC:EMC=3:7Vol%, with 2wt% vinylene carbonate VC additive added.
[0033] Specifically, in step c, the loading amount of the mixed slurry on the prepared electrode sheet is 1 to 5 mg / cm 2 .
[0034] Furthermore, based on a general inventive concept, the present invention also provides a lithium-ion battery prepared by utilizing the surface high-entropy and internal medium-entropy stepwise doped high-nickel layered oxide positive electrode material.
[0035] Compared with the prior art, the advantages of the present invention are:
[0036] 1. The preparation method of the present invention reconstructs the surface of the layered oxide through high entropy doping, constructs an ultra-stable superlattice structure at the weakest interface, and reduces the occurrence of side reactions while avoiding a decrease in discharge specific capacity caused by excessive doping.
[0037] 2. The present invention performs entropy doping in the bulk phase, which can effectively enhance the bond energy between transition metals and oxygen through multi-element synergy, reduce lithium-nickel mixing, slow down unfavorable phase transitions, and inhibit lattice oxygen release.
[0038] 3. The present invention improves and alleviates the surface structure and internal lattice mismatch during volume expansion and contraction through the hierarchical structure of surface high entropy and internal medium entropy, thereby reducing the generation of microcracks during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a scanning electron microscope image of the high-nickel layered oxide positive electrode material prepared in Example 1;
[0040] Figure 2 This is a scanning electron microscope image of the high nickel layered oxide positive electrode material prepared in Example 2;
[0041] Figure 3 This is a scanning electron microscope image of the high nickel layered oxide positive electrode material prepared in Example 3;
[0042] Figure 4 1 is a cycle performance diagram of Comparative Example 1, Comparative Example 2, Example 1, Example 2 and Example 3;
[0043] Figure 5 It is a rate performance diagram of Comparative Example 1, Comparative Example 2, Example 1, Example 2 and Example 3. DETAILED DESCRIPTION
[0044] The following examples will further illustrate the present invention in conjunction with the accompanying drawings. This embodiment is implemented based on the technical solution of the present invention, and provides detailed implementation methods and processes, but the protection scope of the present invention is not limited to the following embodiments.
[0045] The experimental methods in the following examples without specifying specific conditions are generally carried out under conventional conditions, and the raw materials and reagents used are conventional commercially available products unless otherwise specified.
[0046] The comparative examples and examples all use the high nickel layered oxide precursor Ni provided by Henan Xinxiang Tianli Lithium Energy Co., Ltd. 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2 is used as a raw material, and its preparation method can adopt the conventional method in the prior art, which is not the inventive point of the present invention, so it will not be described in detail.
[0047] Comparative Example 1
[0048] Comparative Example 1: The precursor Ni 0.96 Co 0.015 Mn 0.015 Al 0.01 After (OH)2 and LiOH·H2O were uniformly mixed in a molar ratio of 1:1.03, two-stage sintering was carried out in a pure oxygen atmosphere. The first stage sintering temperature was 400℃, the sintering time was 4h, and the second stage sintering temperature was 720℃, the sintering time was 10h, and LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material.
[0049] Comparative Example 2
[0050] Comparative Example 2 provides a method for preparing a medium entropy doped high nickel layered oxide positive electrode material, the specific steps are:
[0051] 1) Ni precursor 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2, TiO2 and LiOH·H2O were uniformly mixed in a molar ratio of 1:0.003:1.03, and then sintered in two stages under an oxygen atmosphere. The first stage was sintered at a temperature of 400°C for 4 h, and the second stage was sintered at a temperature of 720°C for 10 h to obtain titanium-doped LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide cathode material;
[0052] 2) The high nickel layered oxide cathode material in step 1) and TiO2 are uniformly mixed in a molar ratio of 1:0.006, and sintered in an oxygen atmosphere at a sintering temperature of 500° C. for 4 h to obtain a medium entropy doped LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material.
[0053] Example 1
[0054] Example 1 provides a method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping, the specific steps being:
[0055] 1) Ni precursor 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2, TiO2 and LiOH·H2O were uniformly mixed in a molar ratio of 1:0.003:1.03, and then sintered in two stages under an oxygen atmosphere. The first stage was sintered at a temperature of 400°C for 4 h, and the second stage was sintered at a temperature of 720°C for 10 h to obtain titanium-doped LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide cathode material;
[0056] 2) The high nickel layered oxide positive electrode material, TiO2 and MoO3 in step 1) are uniformly mixed in a molar ratio of 1:0.004:0.002, and sintered in an oxygen atmosphere at a sintering temperature of 500°C and a sintering time of 4 hours to obtain a LiNi with a high entropy doping on the surface and a medium entropy doping on the inside. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material. The SEM image of the surface high entropy and internal medium entropy doped high nickel layered oxide positive electrode material prepared in Example 1 is as follows Figure 1 As shown, from Figure 1 It can be seen that the spherical particles are intact and the surface of the material is evenly coated with nanoparticles.
[0057] Example 2
[0058] Example 2 provides a method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping. The difference between Example 2 and Example 1 is step 2);
[0059] Specifically, step 2) is to uniformly mix the high nickel layered oxide positive electrode material, TiO2 and WO3 in step 1) in a molar ratio of 1:0.004:0.002, and sinter them in an oxygen atmosphere at a sintering temperature of 500°C and a sintering time of 4 hours to obtain a LiNi with high entropy doping on the surface and medium entropy doping on the inside. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material. The SEM image of the surface high entropy and internal medium entropy doped high nickel layered oxide positive electrode material prepared in Example 2 is as follows Figure 2 As shown, from Figure 2 It can be seen that the spherical particles are intact and the surface of the material is evenly coated with nanoparticles.
[0060] Example 3
[0061] Example 3 provides a method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping. The difference between Example 3 and Example 1 is step 2);
[0062] Specifically, step 2) is to uniformly mix the layered oxide positive electrode, TiO2 and Nb2O5 in step 1) in a molar ratio of 1:0.004:0.002, and sinter them in an oxygen atmosphere at a sintering temperature of 500°C and a sintering time of 4 hours to obtain a LiNi with high entropy doping on the surface and medium entropy doping on the inside. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material. The SEM image of the surface high entropy and internal medium entropy doped high nickel layered oxide positive electrode material prepared in Example 3 is as follows Figure 3 As shown, from Figure 3 It can be seen that the spherical particles are intact and the surface of the material is evenly coated with nanoparticles.
[0063] Example 4
[0064] Example 4 provides a method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping, the specific steps being:
[0065] 1) Ni precursor 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2, TiO2 and LiOH·H2O were uniformly mixed in a molar ratio of 1:0.003:1.03, and then sintered in two stages in a mixed gas atmosphere of oxygen and nitrogen in a molar ratio of 8:2. The first stage was sintered at a temperature of 400°C for 4 hours, and the second stage was sintered at a temperature of 720°C for 10 hours to obtain titanium-doped LiNi0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide cathode material;
[0066] 2) The high nickel layered oxide positive electrode material, TiO2 and MoO3 in step 1) are uniformly mixed in a molar ratio of 1:0.004:0.002, and sintered in a mixed gas atmosphere of oxygen and nitrogen in a molar ratio of 8:2, the sintering temperature is 500 ° C, the sintering time is 4h, and the surface high entropy doped LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material.
[0067] Example 5
[0068] Example 5 provides a method for preparing a high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping, the specific steps being:
[0069] 1) Ni precursor 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2, ZrO2 and LiOH·H2O were uniformly mixed in a molar ratio of 1:0.005:1.03, and then sintered in two stages under an oxygen atmosphere. The first stage was sintered at a temperature of 400°C for 4 hours, and the second stage was sintered at a temperature of 720°C for 10 hours to obtain zirconium-doped LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide cathode material;
[0070] 2) The high nickel layered oxide positive electrode material, ZrO2 and MoO3 in step 1) are uniformly mixed in a molar ratio of 1:0.002:0.001, and sintered in an oxygen atmosphere at a sintering temperature of 500°C and a sintering time of 4 hours to obtain a LiNi with a high entropy doping on the surface and a medium entropy doping on the inside. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2 high nickel layered oxide positive electrode material.
[0071] Application test
[0072] The products prepared in Example 1-3 and Comparative Example 1-2 were used to prepare lithium-ion batteries, and the specific preparation method was as follows:
[0073] a. The active material (the product prepared in Examples 1, 2, 3 or Comparative Examples 1 and 2) was mixed with carbon black (Super-P, conductive agent, Shenzhen Kejing Zhida Technology Co., Ltd., CAS1333-86-4) and binder PVDF (polyvinylidene fluoride) in a mass ratio of 90:5:5 to obtain a mixed powder;
[0074] b. Then the mixed powder in step a is added to a solvent (N-methylpyrrolidone, NMP) and placed in a mixing container for uniform mixing. The mass of the solvent is 1.5 times the mass of the mixed powder. Then, ultrasonic dispersion is performed at a power of 100 W for 8 minutes. Then, a polytetrafluoroethylene magnet is placed in the mixing container and stirred at a speed of 400 r / min for 10 hours to uniformly disperse the active substance and carbon black (Super-P) to obtain a mixed slurry.
[0075] c. The mixed slurry in step b was coated on aluminum foil and dried at 80 ° C for 12 h to prepare a loading of 5 mg / cm 2 electrode sheet; then in an argon-protected glove box, the prepared electrode sheet was used as the working electrode, the metal lithium sheet was used as the counter electrode, the electrolyte was a high-nickel 4.6V electrolyte (1M LiPF6, EC:EMC=3:7Vol%, with 2wt% vinylene carbonate VC additive), a polypropylene separator, a button battery was assembled, the battery model was a CR2032 button battery, and a constant current charge and discharge test was performed.
[0076] Comparing the cycle performance of the products prepared in Examples 1-3 and Comparative Examples 1-2, the cycle performance test was performed by assembling a CR2032 button battery and performing constant current charge and discharge between 3 and 4.3 V. The results are shown in Tables 1 and Figure 4 As shown, Figure 4 is the cycle performance curve at 0.5C rate, Figure 4 The corresponding coulombic efficiency after 100 cycles at 0.5C rate is shown in Table 1.
[0077] Table 1 Initial specific capacity at 0.5C cycle and capacity retention rate at 100 cycles for Comparative Example 1, Comparative Example 2, Example 1, Example 2 and Example 3.
[0078] sample First discharge specific capacity (mAh / g) 100 cycles capacity retention rate Comparative Example 1 203.9mAh / g 59.2% Comparative Example 2 205.1mAh / g 80.5% Example 1 206.7mAh / g 89.8% Example 2 205.9mAh / g 87.3% Example 3 204.2mAh / g 86.2%
[0079] From Table 1 and Figure 4 It can be concluded that the specific capacity of comparative example 1 in the first cycle discharge is 203.9 mAh / g, and the capacity retention rate after 100 cycles is 59.2%. The initial discharge specific capacity of comparative example 2 does not change significantly compared with comparative example 1, but the capacity retention rate after 100 cycles is increased to 80.5%.
[0080] Compared with Comparative Examples 1 and 2, the initial discharge specific capacities of Examples 1-3 are almost the same. After 100 cycles, the 100-cycle capacity retention rates of Examples 1-3 are higher than those of Comparative Examples 1 and 2. The above results show that the high-entropy and medium-entropy stepwise doping method of the present invention can improve the LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 Cycling stability of O2-rich nickel layered oxides.
[0081] Comparing the rate performance of the products prepared in Example 1-3 and Comparative Example 1-2, the rate performance test was performed by assembling CR2032 button batteries and performing constant current charge and discharge at different rates between 3 and 4.3 V. Figure 5 shown.
[0082] Compared with Comparative Examples 1 and 2, the discharge specific capacities of Examples 1-3 are improved at different rates. Especially at a high rate of 5C, the discharge specific capacities of Examples 1-3 are much higher than those of Comparative Examples 1 and 2. The above results show that the high-entropy and medium-entropy stepwise doping method of the present invention can improve the discharge specific capacity of LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 Rate performance of O2 high nickel layered oxides.
[0083] In summary, the preparation method of the surface high-entropy and internal medium-entropy stepwise doped high-nickel layered oxide positive electrode material described in the present invention improves the cycle stability of the high-nickel layered oxide, has good application value, and is suitable for process promotion and application.
[0084] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a high-entropy surface and medium-entropy internal layered oxide positive electrode material, characterized in that: The following steps are involved: 1) The high nickel layered oxide precursor, the metal doping precursor and the lithium source are uniformly mixed in a certain proportion, and then placed in an atmosphere furnace, and sintered once under a modified atmosphere to obtain a doped high nickel layered oxide positive electrode material; 2) The high nickel layered oxide positive electrode material in step 1) is uniformly mixed with the metal doped precursor 2 in a certain proportion, and then placed in an atmosphere furnace for secondary sintering under a modified atmosphere to obtain a high nickel layered oxide positive electrode material with high surface entropy and medium internal entropy.
2. The preparation method according to claim 1, characterized in that The chemical formula of the high nickel layered oxide precursor in step 1) is Ni 1-x-y-z Co x Mn y Al z (OH)2, x>0, y>0, z>0, 0.6≤(1-xyz)<1.
3. The preparation method according to claim 1, characterized in that: The metal-doped precursor described in step 1) is one or more of metal oxides, metal nitrates, metal sulfates, metal acetates, metal carbonates, and metal organic salts; the metal described in step 1) is one or more of sodium, magnesium, potassium, calcium, scandium, titanium, vanadium, chromium, iron, copper, zinc, gallium, germanium, yttrium, zirconium, niobium, molybdenum, tantalum, tungsten, lanthanum, neodymium, cerium, and europium.
4. The preparation method according to claim 1, characterized in that: The lithium source in step 1) is one of lithium carbonate and lithium hydroxide; in step 1), the molar ratio of the high nickel layered oxide precursor to the metal doping precursor and the lithium source is 1: (0.00005-0.1): (1-1.2).
5. The preparation method according to claim 1, characterized in that: The primary sintering in step 1) includes a first stage sintering and a second stage sintering; the temperature of the first stage sintering is 200-670°C; the time of the first stage sintering is 1-9 hours; the temperature of the second stage sintering is 600-900°C; the time of the second stage sintering is 6-24 hours.
6. The preparation method according to claim 1, characterized in that: The metal-doped precursor 2 described in step 2) is one or more of metal oxides, metal nitrates, metal sulfates, metal acetates, metal carbonates, and metal organic salts; the metal element in step 2) is one or more of sodium, magnesium, potassium, calcium, scandium, titanium, vanadium, chromium, iron, copper, zinc, gallium, germanium, yttrium, zirconium, niobium, molybdenum, tantalum, tungsten, lanthanum, neodymium, cerium, and europium.
7. The preparation method according to claim 1, characterized in that: In step 2), the molar ratio of the high nickel layered oxide precursor to the metal doping precursor 2 is 1:(0.00005~0.1).
8. The preparation method according to claim 1, characterized in that: The secondary sintering temperature in step 2) is 300-900°C, and the sintering time is 0.5-15h.
9. A high-nickel layered oxide positive electrode material with high surface entropy and medium internal entropy stepwise doping prepared by the method according to any one of claims 1 to 8.
10. Use of the surface high-entropy and internal medium-entropy stepwise doped high-nickel layered oxide positive electrode material according to claim 9 in the preparation of lithium-ion batteries.
Citation Information
Patent Citations
High-entropy doped manganese-based layered oxide, preparation method thereof, sodium ion battery positive electrode material and battery
CN116062807A
Multi-element positive electrode material and preparation method thereof
CN116344827A
Nickel-based positive electrode material with entropy gradient and preparation method thereof
CN116632186A
High-entropy surface modified lithium ion battery positive electrode material as well as preparation method and application thereof
CN117810400A
Cited By
High-entropy high-nickel single crystal lithium ion battery positive electrode material and preparation method thereof
CN119495740A
Modified ternary positive electrode material, preparation method thereof and lithium ion battery
CN121528900A