Gadolinium aluminum garnet glass and method for preparing transparent ceramic through amorphous crystallization
Through amorphous crystallization method and pneumatic suspension laser heating technology, the problems of lack of red light, low density and difficult preparation of garnet aluminate materials in applications are solved, and the efficient preparation of dense transparent ceramics is achieved, which improves the material performance and Application potential.
Patent Information
- Application Number
- CN202310514175.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the application of existing garnet aluminate materials, there are problems such as lack of red light in the illumination spectrum, low density, insufficient resistance to high energy rays, Ga2O3 decomposition and volatility during preparation, and difficulty in crystal growth, resulting in performance deterioration and limited application.
Using amorphous crystallization method, the target component material is melted and quenched into a glass state, and then crystallized by annealing to form a dense transparent ceramic. The temperature and airflow are controlled by pneumatic suspension laser heating technology to achieve container-free suspension and rapid cooling of the material. , ensure the optical transparency and grain size of the material.
It realizes efficient preparation of materials, improves the transparency and grain size of materials, solves the problems of material performance deterioration and preparation difficulties in traditional methods, and has the advantages of low preparation temperature, fast speed and short cycle, so it is difficult to achieve the traditional methods. special compound components.
Smart Images

Figure CN118930053A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for growing glass and glass ceramics by a container-free pneumatic suspension method, and in particular to a method for preparing transparent ceramics by using gadolinium aluminum garnet glass and amorphous crystallization thereof, and belongs to the field of glass growth and transparent ceramic preparation. Background Art
[0002] Transparent ceramics are a new type of optical functional material developed in recent years. They can be used as window materials, optical materials, etc., and have broad application prospects in many fields such as industrial production and people's lives. The preparation method of transparent ceramics mainly selects a material system with a cubic symmetrical crystal structure, removes micropores inside the material through high-temperature sintering of ceramics, and removes impurities that are equal to light scattering sources to form a dense structure and achieve optical transparency. The sintering methods mainly include vacuum sintering, hydrogen sintering, spark plasma sintering (SPS), and hot isostatic pressing (HIP) post-treatment. The preparation process involves the crystallization synthesis of compounds and high-temperature sintering densification. The amorphous crystallization method is also a technical solution for preparing transparent ceramics. This method requires first preparing the target compound into an amorphous glass state, and then obtaining ceramics with a certain grain size by controlling the crystallization clustering and time under certain heat treatment conditions.
[0003] Garnet aluminate, chemical formula RE3Al5O 12 , where RE is a rare earth element, is an important class of fluorescent and scintillation material systems; for example, (Ce,Y)3Al5O 12 (Ce:YAG) is the most mature commercial fluorescent material for white light LEDs, with good matching performance with blue light chips and high luminous efficiency. (Ce,Lu)3Al5O 12 (Ce:LuAG) has the characteristics of strong resistance to radiation damage and high fluorescence thermal stability. It is an alternative scintillating material in the new generation of high-energy physics large-scale magnetic calorimeters. It can be used for the study of the origin of high-energy particles and has potential in the fields of high-power LED lighting, laser lighting and display. 12 (Pr:LuAG) has the advantages of high light yield, fast decay time, and high fluorescence thermal stability. It is used as an alternative scintillating material for nuclear medical imaging and has application potential in the field of oil exploration; (Ce,Gd)3(Ga,Al)5O 12 (Ce:GGAG) is the oxide scintillating material with the highest theoretical light yield discovered so far, and has the advantages of strong radiation resistance and fast attenuation. It is considered to be a new generation of scintillation detection material with important potential in the fields of airport and station security equipment.
[0004] However, the above garnet aluminate materials also have problems and shortcomings in the application process. For example, Ce:YAG, as a yellow fluorescent material, has the problem of lack of red light in the lighting spectrum. At the same time, its density is low and its ability to block high-energy rays is not strong, so its application as a scintillating material is limited; Ce:LuAG has the problem of Lu-Al anti-position defect, that is, in the high-temperature molten state, Lu ions and Al ions exchange positions in the lattice due to their close ion radius, forming a point defect. As a trap in the carrier transmission process, it can lead to the degradation of scintillation performance; Ce:GGAG has problems such as component deviation (Ga2O3=Ga2O+O2) caused by the decomposition and volatilization of Ga2O3 during the preparation process and difficulty in crystal growth. However, Gd3Al5O 12 (GdAG) is a non-uniform melting compound, which is difficult to solidify and crystallize by conventional methods. Phase decomposition occurs at 1300℃ (Gd3Al5O 12 →Al2O3+3GdAlO3), currently the GdAG component is obtained only by low-temperature calcination into powder through a liquid phase reaction method, and it is not possible to obtain a dense block by traditional crystal growth or ceramic sintering.
[0005] For example, Chinese Patent 1 (publication number CN 111253073 A) proposes a method for preparing gadolinium aluminum garnet-based white light glass ceramics by a sol-gel method. This technical solution uses a sol-gel method to first obtain a dry gel block with uniform components and conforming to the stoichiometric ratio at a low temperature, and then prepares high-quality white light ceramics at a low sintering temperature. However, the sol-gel method requires complex control of process parameters and has shortcomings in large-scale commercial production. At the same time, in order to avoid the phase decomposition of GdAG at 1300°C, the dry gel block needs to be sintered at a low temperature. There will be bottlenecks in increasing the density of the ceramic and reducing the porosity, which will affect the thermodynamic stability of the material and the life of the device. Chinese Patent 2 (CN 112552038 A) is a green fluorescent composite ceramic and its preparation method and application. This technical solution proposes a stoichiometric ratio of Lu 3-x-z Ce z Re x Al y O 12 The melting and amorphous crystallization of glass, the material is limited to stoichiometric green fluorescent material, the material composition and application range are limited. Chinese Patent 3 (CN 111423128 A) proposes a GGAG fluorescent glass ball and a preparation method thereof, but the technical solution does not include further crystallization of the glass sample; due to the amorphous state inside the fluorescent glass, there are many non-radiative transition centers, which have a quenching effect on luminescence, and the fluorescence performance will be significantly inferior to that of crystalline materials, which is not conducive to the improvement and optimization of material performance. Summary of the invention
[0006] In order to improve the deficiencies of the prior art, the present invention proposes a method for preparing transparent ceramics by crystallization of amorphous materials. Different from the traditional method, the present technical solution first melts the material of the target component and rapidly cools it into a glassy state, and then crystallizes it through annealing and crystallization to form a dense ceramic while maintaining its optical transparency.
[0007] Specifically, on the one hand, the present invention provides a gadolinium aluminum garnet glass, the chemical formula of the gadolinium aluminum garnet glass is (M x G 1-x )3(Al y N 1-y )5O 12 -zAl2O3, wherein M is an ion replacing the dodecahedron, N is an ion replacing the octahedron and / or an ion replacing the tetrahedron; and 0≤x≤1, 0≤y≤1, z=0~150mol%.
[0008] Preferably, z=75-125 mol%.
[0009] Preferably, z=100 mol%.
[0010] Preferably, the ionic radius of the substituted dodecahedron is in the range of 0.083 to 0.129 nm; the ionic radius of the substituted octahedron is in the range of 0.053 to 0.098 nm; and the ionic radius of the substituted tetrahedron is in the range of 0.028 to 0.059 nm.
[0011] Preferably, M includes Y 3+ 、Lu 3+ 、Ce 3+ , Pr 3+ 、Eu 3+ At least one of; N includes Sc 3+ , Ga 3+ Cr 3+ At least one of them.
[0012] Preferably, when the luminescent ion (wherein M and N represent ions at the lattice position, it can be a luminescent ion such as Ce 3+ , Pr 3+ 、Eu 3+ etc., or it can be the non-luminescent ion Y 3+ 、Lu 3+ , luminescence or non-luminescence, depending on whether the ion's outermost electrons and energy level transitions are prohibited) Ce 3+ , Pr 3+ 、Eu 3+ When at least one of them occupies M position or / and N position, 0<x≤10%, 0<y≤10%;
[0013] In another aspect, the present invention provides a method for preparing gadolinium aluminum garnet glass, comprising: (1) Press (M x G 1-x )3(Al y N 1-y )5O 12 -zAl2O3 stoichiometric ratio of raw materials are weighed and mixed to obtain a mixed powder; (2) Mix the powder or (M x G 1-x )3(Al y N 1-y )5O 12 -zAl2O3 phase powder is pressed into shape to obtain a green billet; (3) pre-sintering the obtained green billet to obtain a sample block; (4) The sample block is heated to fully melt by using pneumatic levitation laser heating technology, and then the melt is rapidly cooled to solidify, finally obtaining gadolinium aluminum garnet glass.
[0014] Preferably, in step (1), the raw material includes at least one of an oxide of M, an oxide of Gd, an oxide of N, Al2O3, a nitrate of M, a nitrate of Gd, and a nitrate of N; and the mixing method includes dry grinding and / or wet grinding.
[0015] Preferably, in step (2), the pressing method is dry pressing or / cold isostatic pressing; preferably, the pressure of the dry pressing is 15 to 20 MPa; the pressure of the cold isostatic pressing is 10 to 200 MPa.
[0016] Preferably, in step (3), the pre-sintering parameters include: The pre-sintering atmosphere is selected from at least one of an oxidizing atmosphere, a reducing atmosphere, and an inert atmosphere, wherein the oxidizing atmosphere is an air atmosphere or a pure oxygen atmosphere; The pre-sintering temperature is 500-1500°C, preferably 1000°C; The pre-sintering heat preservation time ranges from 1 to 10 hours, preferably from 2 to 4 hours.
[0017] Preferably, in step (4), the parameters of the pneumatic suspension laser heating technology include: the heating power of the solid laser is 180-200W, the heating temperature is above 1000-1900°C, and the time for maintaining stable molten suspension is 20-30s; the cooling rate of the rapid cooling is 170-100°C / second.
[0018] In another aspect, the present invention provides a gadolinium aluminum garnet transparent ceramic, wherein the gadolinium aluminum garnet glass is subjected to heat treatment to achieve crystallization, thereby obtaining a crystallized gadolinium aluminum garnet transparent ceramic.
[0019] Preferably, the heat treatment method is one or a combination of pressureless firing, hot pressing firing, hot isostatic pressing firing, and discharge plasma firing; Preferably, the parameters of the pressureless firing include: a holding temperature of 900 to 1000° C. and a holding time of 100 to 240 min; Preferably, the parameters of the hot pressing sintering include: pressure 10-200 MPa, insulation temperature 900-1000° C., insulation time 100-240 min; Preferably, the parameters of the hot isostatic pressing include: pressure 10-200 MPa, holding temperature 900-1000° C., holding time 100-240 min; Preferably, the parameters of the spark plasma sintering include: pressure of 1-100 MPa, insulation temperature of 900-1000° C., sintering time of 0-10 min and not 0;.
[0020] Preferably, when the thickness of the gadolinium aluminum garnet transparent ceramic is 1 mm, its total transmittance in the visible light region is greater than 50%; preferably, the linear transmittance is greater than 50%;
[0021] Preferably, the grain size of the gadolinium aluminum garnet transparent ceramic is submicron or / and nanometer.
[0022] Beneficial effects: The present invention adopts pneumatic levitation laser heating technology to prepare glass and then forms transparent ceramics through annealing and crystallization. Its advantages include: (1) the airflow size is controlled by an airflow controller, so that the sample is supported by the spiral airflow in the conical nozzle and maintains a non-contact state with the container; a CO2 laser (power 100W) is used to heat the sample and control the temperature; a CCD camera (Charge Coupled Device) is used to observe the sample suspension, heating, melting and cooling process in real time, and an infrared thermometer is used to record the temperature data in real time. (2) The technical solution of the present invention determines the glass transition temperature and crystallization temperature of the component according to the thermal analysis DSC-DTA results, thereby determining its crystallization temperature range. By annealing at a lower crystallization temperature, amorphous crystallization can be achieved to realize the preparation of transparent ceramics; (3) The technical solution of the present invention has the advantages of low preparation temperature, fast preparation speed and short cycle; (4) The technical solution of the present invention can realize the preparation of special compound components that cannot be prepared by traditional methods, such as the non-uniform melting compound GdAG. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the working principle of containerless air suspension technology; Figure 2This is a real-life photo of the melting process of the sample using the containerless gas suspension technology; Figure 3 A series of photos of GGAG glasses with different Ga / Al ratios prepared by containerless air suspension technology. From left to right, they are Gd3Ga3Al2O 12 , Gd3Ga 2.5 Al 2.5 O 12 、Gd3Ga2Al3O 12 、Gd3GaAl4O 12 、Gd3Al5O 12 ,From the figure, we can see that GGAG glass is colorless, transparent, and spherical, with a diameter of about 3 mm; Figure 4 (Ce,Gd)3(Ga,Al)5O for different Ga / Al ratios 12 The DTA diagram of the glass shows that the crystallization peak Tp of GGAG with different Ga / Al ratios is different and distributed around 900℃. With the increase of Ga content, the crystallization temperature tends to decrease gradually. Figure 5 The actual photos of GdAG-Al2O3 glass and amorphous crystallized transparent ceramics (double-sided polishing 1.0mm) prepared by containerless air suspension technology. From the picture, we can see that transparent GdAG-Al2O3 glass balls with a diameter of about 3mm can be prepared by air suspension technology. After double-sided polishing of amorphous crystallization, the sample can still maintain a certain degree of transparency. Figure 6 The XRD patterns of GdAG glass and amorphous glass after crystallization. From the figure, we can see that the XRD spectrum of GdAG glass shows obvious bun peak characteristics, indicating that the material is in an amorphous glass state; and after amorphous glass is crystallized, sharp diffraction peaks appear, indicating that the material changes from amorphous state to crystalline state; Figure 7 The SEM microstructure morphology of GdAG glass and amorphous glass after crystallization shows that there are a large number of grains and a small number of pores inside the material, and the grain size distribution is uniform, about 50nm or smaller; Figure 8 Different rare earth ions (Ce 3+ , Pr 3+ 、Nd 3+ 、Sm 3+ ) Actual photo of GdAG glass doped with ions, double-sided polished, thickness 1.0 mm. From the figure, we can see that GdAG glass presents different colors with different doping ions; Fig. 9These are photos of a series of GGAG glasses with different Ce concentrations prepared by containerless air suspension technology. It can be seen from the figure that transparent glass balls can still be formed after Ce doping, and the color gradually changes from light yellow to dark yellow with the increase of doping concentration; Fig.10 The fluorescence spectrum (λ ex =450nm), its excitation spectrum shows that there are two characteristic peaks at 325nm and 450nm, which are derived from Ce 3+ The 4f-5d1 and 5d2 transitions of Ce can be observed near 550nm with obvious broadband emission peaks. 3+ 5d-4f transition of Ce 3+ Solid solution into the crystal lattice and achieved characteristic luminescence; Fig.11 X-ray excitation emission spectra (X-ray tube) of Ce-doped GdAG-Al2O3 transparent ceramics treated at different annealing temperatures. DETAILED DESCRIPTION
[0024] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0025] In the present disclosure, the chemical formula of gadolinium aluminum garnet glass is (M x G 1-x )3(Al y N 1-y )5O 12 , where M includes but is not limited to Y 3+ 、Lu 3+ 、Ce 3+ , Pr 3+ 、Eu 3+ Ions that can substitute in the dodecahedral lattice of the GAG matrix, N including but not limited to Sc 3+ , Ga 3+ Cr 3+ Ions that can substitute in the tetrahedral and octahedral sites of gadolinium aluminum garnet, and 0≤x≤1, 0≤y≤1.
[0026] In an optional embodiment, a certain amount of Al2O3 is additionally added to the stoichiometric ratio of the gadolinium aluminum garnet glass component to improve the glass forming ability of the material. x G 1-x )3(Al y N 1-y )5O 12 -zAl2O3, the addition amount is z=0~150mol%, preferably z=100mol%.
[0027] In an optional embodiment, the selection of M and N ions is based on the size of the ionic radius and the balance of the valence state. The ionic radius of the substituted dodecahedron ranges from 0.083 to 0.129 nm. The ionic radius of the substituted octahedron ranges from 0.053 to 0.098 nm; the ionic radius of the substituted tetrahedron ranges from 0.028 to 0.059 nm.
[0028] In an optional embodiment, the ions that can be stimulated to emit light can occupy the M or N positions respectively or simultaneously according to the ion radius and valence state. When the luminescent ions occupy the M or N positions, the preferred concentration range is 0<x≤10%, 0<y≤10%.
[0029] In the present invention, the component has the characteristics of being compatible with non-stoichiometric ratios and having a wide adjustable luminescence spectrum; in the process of glass growth, a pneumatic suspension laser heating technology is used, and the airflow size is controlled by an airflow controller, so that the sample is supported by the spiral airflow in the conical nozzle and maintains a non-contact state with the container; a laser is used to heat the sample and control the temperature; a CCD camera (Charge Coupled Device) is used to observe the sample suspension, heating, melting and cooling process in real time, and an infrared thermometer is used to record temperature data in real time. The glass transition temperature and crystallization temperature are characterized by DSC-DTA thermal analysis; the crystallization temperature range is determined according to the thermal analysis results, and transparent ceramic preparation is achieved by amorphous crystallization, which has the characteristics of short cycle and simple process.
[0030] The present invention adopts containerless technology to prepare gadolinium aluminum garnet glass. The technology of preventing the material from contacting the container during the preparation process of gadolinium aluminum garnet glass material can solve several problems that always exist in the traditional material processing process: (1) chemical reaction between the material and the container wall; (2) auxiliary nucleation effect of the container wall on the material (3) the influence of the container on the supercooling degree of the material. Therefore, this technology can provide a high-purity and interference-free deep supercooling process for the material. Since deep supercooling is crucial to the formation of glass, this means that using containerless technology, some materials that are difficult to amorphize by conventional contact methods can be prepared into glass. Pneumatic suspension technology is a type of containerless technology, which refers to the use of gas as an external force to offset gravity so that the object reaches a suspended state without contact with the container wall. The following is an exemplary description of the preparation method of gadolinium aluminum garnet glass.
[0031] Weigh. Press (M x G 1-x )3(Al y N 1-y )5O 12 Weigh the component compound powders according to the stoichiometric ratio, including but not limited to oxides, nitrates, etc.; or directly use (M x G 1-x )3(Al y N1-y )5O 12 Phase compound powder.
[0032] Mixing. The raw materials are mixed evenly; the mixing methods include but are not limited to dry grinding, wet grinding and a combination thereof to obtain a mixed powder.
[0033] Forming. Dry and sieve the mixed powder, weigh appropriate powder and form it to obtain a green blank. The forming technology includes but is not limited to the dry pressing method using a tablet press.
[0034] Pre-sintering. The purpose of pre-sintering the formed green blank is to make the green blank have a certain mechanical strength to avoid the generation of flying powder during the suspension firing process. The pre-sintering atmosphere includes air, oxidizing atmosphere, reducing atmosphere, inert atmosphere, heating temperature range 500 ℃ ~ 1500 ℃; preferably 1000 ℃; insulation time range 1 ~ 10 hours, preferably 2-4 hours.
[0035] Glass growth uses a pneumatic suspension laser heating technology. The airflow size is controlled by an airflow controller, so that the sample is supported by the spiral airflow in the conical nozzle and maintained in a container-free state; a laser is used to heat the sample and control the temperature; a CCD camera (Charge Coupled Device) is used to observe the sample suspension, heating, melting and cooling process in real time, and an infrared thermometer is used to record temperature data in real time. When the material is fully melted, the laser is turned off or the laser power is reduced to quickly cool the melt to solidify into glass. Subsequently, the glass transition temperature (Tg) and crystallization temperature (Tp) are obtained according to DSC and / or DTA thermal analysis technology to determine its heat treatment temperature.
[0036] The glass is crystallized by heat treatment, and transparent ceramics are prepared by crystallization. The heat treatment method is one or a combination of pressureless firing, hot pressing firing, hot isostatic pressing firing, discharge plasma firing, etc. The grain size of the transparent ceramic obtained is submicron (0.1-0.35μm) or nanometer (1-100nm). When the obtained ceramic sample is double-sided polished with a thickness of 1mm, its total transmittance in the visible light region is greater than 50%; preferably, the linear transmittance is greater than 50%.
[0037] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0038] Example 1 Preparation of GdAG-Al2O3 glass by gas suspension and amorphous crystallization: (1) High-purity (purity 99.99%) commercial raw materials Al2O3 and Gd2O3 oxide powders were prepared according to (M x G 1-x )3(Al y N 1-y )5O 12 The ratio of , where x = 0 mol%, y = 1, that is, the component is undoped Gd3Al5O 12 , and then add 100 mol% Al2O3 powder, namely Gd3Al5O 12 The molar ratio of Al2O3 is 1:1; after mixing for 1 hour using an automatic agate mortar machine, a mixed powder is obtained; (2) Weigh the mixed powder in portions of 0.6 g / portion, fill them in a dry pressing mold, and press them into A cylindrical blank; (3) sintering the green body in an air atmosphere muffle furnace at 1000° C. for 1 hour to obtain a ceramic with a certain density; (4) Place the fired ceramic into the nozzle of the pneumatic levitation furnace, ensure that the laser spot evenly covers the sample, turn on the laser, slowly increase the output power, and observe the material melting in real time through the video in situ, rotate the airflow knob to control the airflow, and keep the sample in a suspended state; after the sample is stably suspended and completely melted into a uniform and symmetrical sphere (such as Figure 2 Turn off the laser and take out the fired spherical glass sample, as shown in Figure 3 , Figure 6 , Figure 7 Shown (5) DTA analysis was used to characterize its glass transition temperature (Tg) and crystallization temperature (Tp), and the measured Tg = 870 ° C; Tp = 951 ° C; ΔT = Tp-Tg = 81. In an air atmosphere, the silicon molybdenum rod furnace was annealed and crystallized at 900 ° C / 4 h to form a transparent ceramic. Its phase and microstructure are as follows Figure 6-Figure 7 shown.
[0039] Table 1 shows the composition and properties of the GdAG glass prepared in Example 1 with different amounts of Al2O3 powder added: z Tg(℃) Tp(℃) ΔT(k) 150mol% 866 959 93 125mol% 869 960 91 100mol% 877 966 89 50mol% 871 955 84 0mol% 876 950 74 .
[0040] Table 2 shows the composition and properties of the GdAG transparent ceramics prepared in Example 1 with the addition of Al2O3 powder: z Total transmittance in the visible light region / % Linear transmittance / % 100mol% 75 10 .
[0041] Embodiment 2: (1) High-purity (purity 99.99%) commercial raw materials Al2O3, Ga2O3, Gd2O3 oxide powders were prepared according to (RE x G 1-x )3Ga2Al3O 12 The ratio of (x = 0.01 to 0.09, for example 0.05), where RE 3+ For rare earth luminescent ions, Ce is selected independently. 3+ , Pr 3+ 、Nd 3+ 、Sm 3+ and introduced in the form of oxide powder. After mixing for 1 hour using an automatic agate mortar machine, a mixed powder was obtained; (2) Weigh the mixed powder in portions of 0.6 g / portion, fill them in a dry pressing mold, and press them into A cylindrical blank; (3) sintering the green blank in a tubular furnace at 1000° C. for 1 hour in a flowing oxygen atmosphere to obtain a ceramic with a certain density; (4) Place the fired ceramic into the nozzle of the pneumatic levitation furnace, ensure that the laser spot evenly covers the sample, turn on the laser, slowly increase the output power, and observe the material melting in real time through the video in situ, rotate the airflow knob to control the airflow, and keep the sample in a suspended state; after the sample is stably suspended and completely melted into a uniform and symmetrical sphere (such as Figure 2 Turn off the laser and take out the fired spherical glass sample, as shown in Figure 8 As shown; (5) DTA analysis was used to characterize its glass transition temperature (Tg) and crystallization temperature (Tp), and Ce 3+ The ion-doped glass has Tg=865°C, Tp=952°C, ΔT=87; after annealing and crystallization, a transparent ceramic is formed.
[0042] Table 3 shows the composition and properties of the GdAG glass doped with different rare earth ions prepared in Example 2: x Components Tg(℃) Tp(℃) ΔT(k) 0.05 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ce <h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> )3Al3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> - 952 - 0.05 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Pr <h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> )3Al3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> - 952 - 0.05 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Nd <h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> )3Al3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> - 953 - 0.05 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Sm <h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> )3Al3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> - 953 - 0 <![CDATA[Gd3Al3O 12 ]]> 876 950 74 .
[0043] Example 3 Different Ga / Al ratios (Ce, Gd)3(Ga , Al)5O 12 Air suspension preparation and amorphous crystallization of glass: High purity (purity 99.99%) commercial raw materials Al2O3, Ga2O3, Gd2O3 oxide powders were prepared according to Gd3Ga x Al 5-5y O 12The proportion of (5y = 0, 1, 2, 2.5, 3) was weighed. After mixing for 1 hour using an automatic agate mortar machine, a mixed powder was obtained; (2) Weigh the mixed powder in portions of 0.6 g / portion, fill them in a dry pressing mold, and press them into A cylindrical blank; (3) sintering the green blank in a tubular furnace at 1000° C. for 1 hour in a flowing oxygen atmosphere to obtain a ceramic with a certain density; (4) Place the fired ceramic into the nozzle of the pneumatic levitation furnace, ensure that the laser spot evenly covers the sample, turn on the laser, slowly increase the output power, and observe the material melting in real time through the video in situ, rotate the airflow knob to control the airflow, and keep the sample in a suspended state; after the sample is stably suspended and completely melted into a uniform and symmetrical sphere (such as Figure 2 Turn off the laser and take out the fired spherical glass sample, as shown in Figure 3 As shown; (5) The glass transition temperature (Tg) and crystallization temperature (Tp) of the obtained glass were characterized by DTA analysis, as shown in the following table; the obtained glass was then annealed and crystallized at 900°C / 4h to form a transparent ceramic.
[0044] Example 4 (Ce, Gd)3Ga2Al3O with different Ce doping concentrations 12 Air suspension preparation and amorphous crystallization of glass: (1) High-purity (purity 99.99%) commercial raw materials Al2O3, Ga2O3, Gd2O3 oxide powders were prepared according to (Ce x G 1-x )3Ga2Al3O 12 (x=0.1%, 0.3%, 0.5%, 0.7%, 0.9%, y=0.6) were weighed. After mixing for 1 hour using an automatic agate mortar machine, a mixed powder was obtained; (2) Weigh the mixed powder in portions of 0.6 g / portion, fill them in a dry pressing mold, and press them into A cylindrical blank; (3) sintering the green blank in a tubular furnace at 1000° C. for 1 hour in a flowing oxygen atmosphere to obtain a ceramic with a certain density; (4) Place the fired ceramic into the nozzle of the pneumatic levitation furnace, ensure that the laser spot evenly covers the sample, turn on the laser, slowly increase the output power, and observe the material melting in real time through the video in situ, rotate the airflow knob to control the airflow, and keep the sample in a suspended state; after the sample is stably suspended and completely melted into a uniform and symmetrical sphere (such as Figure 2 Turn off the laser and take out the fired spherical glass sample, as shown in Fig. 9As shown (from left to right, x = 0.1%, 0.3%, 0.5%, 0.7%, 0.9%); (5) After polishing the sample on both sides by 1.0 mm, the fluorescence performance was tested. Fig.10 , under 450nm blue light excitation, there is a broad band of light emission at 580nm, which is considered to be Ce 3+ The luminescence performance of the material indicates that it is expected to be used in the fields of fluorescent lighting and scintillation detection. (6) Prepare three components (Ce 0.009 G 0.991 )3Ga2Al3O 12 The samples (x = 1%) were treated at different annealing temperatures (821°C, 835°C, 850°C) for 40 min. Fig.11 As can be seen from the figure, as the annealing temperature increases, the sample annealed at 850℃ emits fluorescence under X-ray excitation, indicating that the relaxation of the amorphous structure inside the material to high-energy X-ray excitation decreases with the increase of annealing temperature, and the material has a higher degree of crystallinity after high-temperature annealing;
[0045] Table 6 shows the Ce doping concentration of 0.9% prepared in Example 4 (Ce x G 1-x )3(Al y Ga 1-y )5O 12 Composition and properties of glass: x y Tg(℃) Tp(℃) ΔT(k) 0.9% 0.6 870 951 81 .
Claims
1. A gadolinium aluminum garnet glass, It is characterized in that The chemical formula of the gadolinium aluminum garnet glass is (M x G 1-x ) 3 (Al y N 1-y ) 5 O 12 -zAl 2 O 3 , wherein M is an ion replacing a dodecahedron, N is an ion replacing an octahedron or / and an ion replacing a tetrahedron; and 0≤x≤1, 0≤y≤1, z=0~150mol%.
2. The gadolinium aluminum garnet glass according to claim 1, It is characterized in that z=100 mol%.
3. The gadolinium aluminum garnet glass according to claim 1, It is characterized in that The ionic radius of the substituted dodecahedron ranges from 0.083 to 0.129 nm; the ionic radius of the substituted octahedron ranges from 0.053 to 0.098 nm; and the ionic radius of the substituted tetrahedron ranges from 0.028 to 0.059 nm.
4. The gadolinium aluminum garnet glass according to any one of claims 1 to 3, It is characterized in that M includes Y 3+ 、Lu 3+ 、Ce 3 + , Pr 3+ 、Eu 3+ At least one of; N includes Sc 3+ , Ga 3+ Cr 3+ At least one of them.
5. The gadolinium aluminum garnet glass according to claim 4, It is characterized in that When the luminescent ion Ce 3+ , Pr 3+ 、Eu 3+ When at least one of them occupies the M position or / and the N position, 0<x≤10%, 0<y≤10%.
6. A method for preparing the gadolinium aluminum garnet glass according to any one of claims 1 to 5, It is characterized in that include: (1) Press (M x G 1-x ) 3 (Al y N 1-y ) 5 O 12 -zAl 2 O 3 Weigh the raw materials in a stoichiometric ratio and mix them to obtain a mixed powder; (2) Mix the powder or (M x G 1-x ) 3 (Al y N 1-y ) 5 O 12 -zAl 2 O 3 The powder is pressed into a shape to obtain a green body; (3) pre-sintering the obtained green billet to obtain a sample block; (4) The sample block is heated to fully melt by using pneumatic levitation laser heating technology, and then the melt is rapidly cooled to solidify, finally obtaining gadolinium aluminum garnet glass.
7. The preparation method according to claim 6, It is characterized in that In step (1), the raw materials include oxides of M, oxides of Gd, oxides of N, Al 2 O 3 , at least one of the nitrates of M, Gd, and N; the mixing method includes dry grinding and / or wet grinding.
8. The preparation method according to claim 6, It is characterized in that In step (2), the pressing method is dry pressing or / cold isostatic pressing; Preferably, the pressure of the dry pressing is 15-20 MPa; the pressure of the cold isostatic pressing is 10-200 MPa.
9. The preparation method according to claim 6, It is characterized in that In step (3), the parameters of the pre-sintering include: the atmosphere of the pre-sintering is selected from at least one of an oxidizing atmosphere, a reducing atmosphere, and an inert atmosphere, and the oxidizing atmosphere is an air atmosphere or a pure oxygen atmosphere; The pre-sintering temperature is 500-1500°C, preferably 1000°C; The pre-sintering heat preservation time ranges from 1 to 10 hours, preferably from 2 to 4 hours.
10. The preparation method according to any one of claims 6 to 9, It is characterized in that In step (4), the parameters of the pneumatic suspension laser heating technology include: the heating power of the solid laser is 180-200W, the heating temperature is above 1000-1900°C, and the stable melting suspension time is maintained for 20-30s; The rapid cooling rate is 100-170°C / second.
11. A gadolinium aluminum garnet transparent ceramic, It is characterized in that The gadolinium aluminum garnet glass according to any one of claims 1 to 5 is subjected to heat treatment to achieve crystallization, thereby obtaining a crystallized gadolinium aluminum garnet transparent ceramic.
12. The gadolinium aluminum garnet transparent ceramic according to claim 11, It is characterized in that The heat treatment method is one or a combination of pressureless firing, hot pressing firing, hot isostatic pressing firing, and discharge plasma firing; Preferably, the parameters of the pressureless firing include: a holding temperature of 900 to 1000° C. and a holding time of 100 to 240 min; Preferably, the parameters of the hot pressing sintering include: pressure 10-200 MPa, insulation temperature 900-1000° C., insulation time 100-240 min; Preferably, the parameters of the hot isostatic pressing include: pressure 10-200 MPa, holding temperature 900-1000° C., holding time 100-240 min; Preferably, the parameters of the spark plasma sintering include: a pressure of 1 to 100 MPa, a holding temperature of 900 to 1000° C., and a sintering time of 0 to 10 min and not 0.
13. The gadolinium aluminum garnet transparent ceramic according to claim 11 or 12, It is characterized in that When the thickness of the gadolinium aluminum garnet transparent ceramic is 1 mm, its total transmittance in the visible light region is greater than 50%; preferably, the linear transmittance is greater than 50%.
14. The gadolinium aluminum garnet transparent ceramic according to any one of claims 11 to 13, It is characterized in that The grain size of the gadolinium aluminum garnet transparent ceramic is submicron or / and nanometer.
Citation Information
Patent Citations
Scintillation crystallized glass embedded with GYAGG: Ce microcrystalline phase and preparation method thereof
CN108264234A
Warm-white high-color-rendering-index fluorescent ceramic for high-power LED / LD illumination, as well as preparation method and application thereof
CN109592978A
GGAG fluorescent glass ball and preparation method thereof
CN111423128A
Green fluorescent composite ceramic as well as preparation method and application thereof
CN112552038A
Method for growing gadolinium gallium garnet crystal by moving flux floating zone method
CN115386956A