Preparation method of glass shell, glass shell, etching liquid and electronic equipment
By wet etching the glass substrate using etching liquids of hydrofluoric acid, sulfuric acid, phosphoric acid and sulfamic acid, wet etching to form a gully three-dimensional texture, which solves the problem that it is difficult to prepare a three-dimensional texture structure in the prior art glass back cover. It achieves powerful texture designability and aesthetic effects.
Patent Information
- Application Number
- CN202310535060.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to prepare pre-designed three-dimensional texture structures for existing glass back covers, and the designability of microscopic 3D three-dimensional textures is weak and complex appearance effects cannot be achieved.
The glass substrate is wet etched by etching liquid of hydrofluoric acid, sulfuric acid, phosphoric acid and sulfamic acid, forming a mask layer gradually peels off from the edge of the hollow area, realizing the formation of a gully three-dimensional texture, and designing the hollow area The size, shape and arrangement enhance the designability of the texture.
It realizes the complex texture design of the surface of the glass shell, enhances the designability and appearance effect of the texture, and can customize the concave and convex textures as needed, suitable for decoration of electronic equipment.
Smart Images

Figure CN118930061A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electronics, and in particular to a method for preparing a glass shell, a glass shell, an etching solution and an electronic device. Background Art
[0002] With the fierce competition in the smartphone market, mobile phone types are becoming more diversified and novel. The appearance of a novel, beautiful and comfortable mobile phone back shell has become a hot spot of competition in the mobile phone industry. At present, the back cover glass of mobile phones is often decorated with acid etching technology, which can achieve a hazy appearance of the back cover glass substrate and enhance the visual effect of the back cover of the mobile phone. However, it is difficult to prepare a pre-designed three-dimensional texture structure in the preparation process of the glass back cover, and the designability of the microscopic 3D texture is weak. Summary of the invention
[0003] In view of the above problems, an embodiment of the present application provides a method for preparing a glass shell, wherein the prepared glass shell has a groove-shaped three-dimensional texture structure.
[0004] A first aspect of the present application provides a method for preparing a glass casing, which includes:
[0005] providing a glass substrate;
[0006] forming a mask layer on the surface of the glass substrate, wherein the mask layer has a hollow area; and
[0007] The glass substrate is wet-etched in an etching solution to obtain a glass shell, wherein the etching solution includes hydrofluoric acid, sulfuric acid, phosphoric acid and aminosulfonic acid, so that during the wet etching, the mask layer is gradually peeled off from the glass substrate from the edge portion adjacent to the hollow area toward a direction away from the hollow area.
[0008] A second aspect of the present application provides a glass housing, which is prepared by the preparation method described in the first aspect of the present application.
[0009] A third aspect of the present application provides a glass shell, comprising a main body and a plurality of protrusions, wherein the main body has a first surface, the plurality of protrusions are arranged on the first surface of the main body, the protrusions have a second surface connected to the first surface, an angle between the first surface and the second surface is greater than 90°, and the protrusions are formed by wet etching of a glass substrate; the roughness Ra of the surface of the glass shell having the protrusions is in the range of 1μm≤Ra≤3μm.
[0010] In a fourth aspect, an embodiment of the present application provides an etching solution, which is used for etching glass. The etching solution comprises, by mass fraction:
[0011] 20% to 30% hydrofluoric acid;
[0012] 15% to 25% sulfuric acid;
[0013] 10% to 20% phosphoric acid;
[0014] 3% to 10% sulfamic acid; and
[0015] 3% to 5% fluoride salt.
[0016] A fifth aspect of the present application provides an electronic device, comprising:
[0017] Display screen;
[0018] The glass shell prepared by the preparation method of the glass shell according to the first aspect of the present application, or the glass shell according to the second aspect of the present application, or the glass shell according to the third aspect of the present application, wherein the glass shell is arranged opposite to the display screen; and
[0019] A processor is located between the glass shell and the display screen, and the processor is electrically connected to the display screen to control the display screen to display.
[0020] The preparation method of the glass shell of the embodiment of the present application is to first form a mask layer on the surface of the glass substrate, and then use an etching solution including hydrofluoric acid, sulfuric acid, phosphoric acid and aminosulfonic acid to etch the glass substrate. During the etching, the hydrofluoric acid is mainly used to corrode the silicon dioxide network skeleton in the glass substrate, and the sulfuric acid, phosphoric acid and aminosulfonic acid are used to provide hydrogen ions so that the hydrogen ions in the etching solution are kept in a stable state with a relatively high concentration, providing basic conditions for fluorine ions to corrode the silicon dioxide network skeleton. In addition, sulfuric acid, phosphoric acid and aminosulfonic acid can also give full play to the mixed acid effect of the etching solution. The etching solution causes the mask layer to be gradually peeled off from the edge adjacent to the hollow area. The glass substrate is separated from the area originally covered by the mask layer, and the part close to the hollow area is gradually exposed, so that the area of the glass substrate not covered by the mask layer (i.e., the hollow area) is gradually etched along the thickness direction of the glass substrate. As the mask layer is gradually peeled off from the position close to the hollow area, the glass substrate adjacent to the hollow area is gradually etched from the side, so that the etching depth of the position corresponding to the hollow area of the obtained glass shell is the deepest, and the etching depth of the part corresponding to the area adjacent to the hollow area gradually becomes shallower. The etching surface of the glass substrate can be naturally transitioned and uniformly etched, thereby forming a gully-shaped three-dimensional texture pattern (or a mountain-shaped three-dimensional texture pattern). In addition, the preparation method of the glass shell of the present application can realize the design of the size, shape, arrangement mode, etc. of the concave-convex texture on the surface of the prepared glass shell by designing the size, shape, arrangement mode, etc. of the hollow area, and has strong designability, and the concave-convex texture can be customized according to the texture and appearance effect (such as flashing texture) actually required to be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 It is a schematic diagram of a process of preparing a glass shell according to an embodiment of the present application.
[0023] Figure 2 It is a structural schematic diagram of a preparation process of a glass shell according to an embodiment of the present application.
[0024] Figure 3 It is a schematic diagram of the process of preparing the mask layer of the present application.
[0025] Figure 4 It is a structural schematic diagram of the preparation process of the mask layer of the present application.
[0026] Figure 5Schematic diagram of the structure of a glass shell according to an embodiment of the present application.
[0027] Figure 6 The shell of one embodiment of the present application is along Figure 5 Schematic diagram of the cross-sectional structure in the AA direction.
[0028] Figure 7 yes Figure 6 Enlarged view of dashed box I.
[0029] Figure 8 This is a partial three-dimensional topography diagram of the glass shell of Example 1 of the present application.
[0030] Fig. 9 This is a three-dimensional topographical diagram of another part of the glass shell of Example 1 of the present application.
[0031] Fig.10 It is a schematic diagram of the structure of an electronic device according to an embodiment of the present application.
[0032] Fig.11 It is a circuit block diagram of an electronic device according to an embodiment of the present application.
[0033] Fig.12 It is a schematic diagram of a partial exploded structure of an electronic device according to an embodiment of the present application.
[0034] Fig.13 This is a circuit block diagram of an electronic device according to another embodiment of the present application.
[0035] Description of reference numerals:
[0036] 200-glass shell, 210-main body, 211-first surface, 230-protrusion, 231-second surface, 200a-glass substrate, 10a-mask layer, 11a-hollow area, 10b-photoresist layer, 10c-patterned layer, 300-electronic device, 310-display screen, 320-middle frame, 330-processor, 350-memory, 370-camera module, 201-light-transmitting part. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0038] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0039] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.
[0040] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.
[0041] The texture on the glass shell can be etched with frosting liquid, but the texture formed by etching with frosting liquid is a granular concave-convex texture, and the particle size is irregular. It is impossible to design the shape, size and arrangement of the texture. Only a matte or shiny sand glass shell can be obtained, and it is difficult to design the texture pattern.
[0042] In addition, the glass shell can also be etched by yellow light etching process. However, although the yellow light etching process can design the texture, the yellow light etching process (during etching, the surface of the photoresist layer away from the glass substrate is flat) can only prepare the texture of 2D structure (that is, the surface formed by etching is basically perpendicular to the glass surface of the substrate), and cannot prepare the texture of 3D structure, so that the pattern of the texture obtained by the yellow light etching process is limited, and only the texture of the characteristic pattern can be obtained.
[0043] The "2D structure" in the present application refers to a structure in which only vertical (also called Z-direction) etching occurs during etching, and the etched surface of the obtained etched texture is perpendicular to the surface.
[0044] The "3D structure" in the present application means that during etching, in addition to vertical etching, the glass also undergoes side (also known as X-direction) etching, thereby forming a 3D structural texture.
[0045] See also Figure 1 and Figure 2 , the embodiment of the present application provides a method for preparing a glass housing 200, which includes:
[0046] S101, providing a glass substrate 200a;
[0047] Optionally, the glass substrate 200a may be, but is not limited to, silicate glass, high alumina silicate glass (such as Corning high alumina silicate glass), quartz glass, soda lime glass, fluoride glass, etc.
[0048] Optionally, providing the glass substrate 200a further includes sequentially performing acid washing, alkali washing and water washing on the glass substrate 200a, or performing alkali washing, acid washing and water washing on the glass substrate 200a, and then drying the glass substrate 200a.
[0049] S102, forming a mask layer 10a on the surface of the glass substrate 200a, wherein the mask layer 10a has a hollow area 11a; and
[0050] Optionally, there may be one or more hollow areas 11a. When there are multiple hollow areas 11a, the multiple hollow areas 11a may be arranged at intervals, or may be arranged staggered according to a preset rule, or may be partially spaced, partially staggered, partially connected, etc. according to a preset rule. The shape of the hollow area 11a may be regular or irregular. The shape, number, and arrangement of the hollow areas 11a may be designed according to the actual appearance effect to be achieved, and this application does not make any specific limitation.
[0051] The term "plurality" in this application refers to more than two or at least two.
[0052] It can be understood that the plurality of hollow areas 11 a form a hollow pattern.
[0053] S103, wet-etching the glass substrate 200a in an etching solution to obtain a glass shell 200, wherein the etching solution includes hydrofluoric acid, sulfuric acid, phosphoric acid and aminosulfonic acid, so that during the wet etching, the mask layer 10a is gradually peeled off from the glass substrate 200a from the edge portion adjacent to the hollow area 11a toward a direction away from the hollow area 11a.
[0054] It can be understood that when etching is performed, the mask layer 10a is not etched by the etching solution, but the edge portion of the mask layer 10a adjacent to the hollow area 11a is gradually separated from the glass substrate 200a in the direction away from the hollow area 11a (in other words, gradually falls off), so that the area covered by the mask layer 10a is gradually etched from the side of the position adjacent to the hollow area 11a, so that the surface of the glass substrate 200a forms a three-dimensional texture pattern with a gully shape or a three-dimensional texture pattern with a convex vein-like peak shape, so that the glass shell 200 has a gully-like three-dimensional texture (3D) pattern.
[0055] In some embodiments, after the wet etching, the method for preparing the glass housing 200 of the embodiment of the present application further includes: removing the mask layer 10 a , and performing cleaning (eg, water washing) and drying to obtain the glass housing 200 .
[0056] The mixed acid is prepared using hydrofluoric acid, sulfuric acid, phosphoric acid, and aminosulfonic acid. The inherent properties of sulfuric acid, phosphoric acid, and aminosulfonic acid can be used to coordinate and influence the dissolution of the glass substrate 200a by hydrofluoric acid, thereby playing a compatibility role. The principle is that various silicates are formed by complex chemical reactions of sulfate ions, phosphate ions, aminosulfonic acid ions, etc. on the surface of the glass substrate 200a. Due to their inherent properties, they change the solubility of various silicates through hydrogen bonding to achieve a natural transition etching effect.
[0057] In the preparation method of the glass shell 200 of the embodiment of the present application, a mask layer 10a is first formed on the surface of the glass substrate 200a, and then an etching solution including hydrofluoric acid, sulfuric acid, phosphoric acid and aminosulfonic acid is used to etch the glass substrate 200a. During the etching, the hydrofluoric acid is mainly used to corrode the silicon dioxide network skeleton in the glass substrate 200a, and the sulfuric acid, phosphoric acid and aminosulfonic acid are used to provide hydrogen ions so that the hydrogen ions in the etching solution are kept in a stable state with a relatively high concentration, providing basic conditions for the fluorine ions to corrode the silicon dioxide network skeleton. In addition, the sulfuric acid, phosphoric acid and aminosulfonic acid can also give full play to the mixed acid effect of the etching solution. The etching solution causes the mask layer 10a to be gradually peeled off from the edge adjacent to the hollow area 11a, and the glass substrate 200a originally The portion of the area covered by the mask layer 10a close to the hollow area 11a is gradually exposed, so that the area of the glass substrate 200a not covered by the mask layer 10a (i.e., the hollow area 11a) is gradually etched along the thickness direction of the glass substrate 200a. As the mask layer 10a is gradually peeled off from the position close to the hollow area 11a, the glass substrate 200a adjacent to the hollow area 11a is gradually etched on the side, so that the etching depth of the obtained glass shell 200 corresponding to the hollow area 11a is the deepest, and the etching depth of the portion corresponding to the area adjacent to the hollow area 11a gradually becomes shallower. The etched surface of the glass substrate 200a can be naturally transitioned and uniformly etched, thereby forming a gully-shaped three-dimensional texture pattern (or a peak-shaped three-dimensional texture pattern). In addition, the preparation method of the glass shell 200 of the present application can achieve the design of the size, shape, arrangement, etc. of the concave-convex texture on the surface of the manufactured glass shell 200 by designing the size, shape, arrangement, etc. of the hollow area 11a. It has strong designability and can customize the concave-convex texture according to the texture and appearance effect (such as glittering texture) that are actually needed.
[0058] See also Figure 3 and Figure 4 In some embodiments, a mask layer 10a is formed on the surface of the glass substrate 200a, and the mask layer 10a has a hollow area 11a, including:
[0059] S1021, forming a photoresist layer 10b on the surface of the glass substrate 200a;
[0060] Optionally, a photoresist solution is coated or printed on the surface of the glass substrate 200 a and soft-baked to remove the solvent in the photoresist solution to obtain a photoresist layer 10 b with uniform thickness.
[0061] Optionally, the photoresist solution may be a positive photoresist solution or a negative photoresist solution, which is not specifically limited in the present application.
[0062] S1022, partially exposing the photoresist layer 10b, and developing it to obtain a patterned layer 10c; and
[0063] Optionally, a glass substrate 200a with a photoresist layer 10b is placed in a photolithography machine, a mask with a light hole is set on the surface of the photoresist layer 10b away from the glass substrate 200a, and exposure (for example, ultraviolet light exposure) is performed; then, it is placed in a developing device and developed in a developer to remove local photoresist on the photoresist layer 10b, thereby obtaining a patterned layer 10c, which has a patterned hollow area 11a. It can be understood that the hollow texture pattern can be transferred to the photoresist layer 10b through exposure and development.
[0064] Optionally, the softening point Ts of the patterned layer 10c is in the range of 140°C≤Ts≤160°C. Further, the softening point Ts of the patterned layer 10c is in the range of 145°C≤Ts≤155°C. Specifically, the softening point of the patterned layer 10c may be, but is not limited to, 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C, 160°C, etc. If the softening point of the patterned layer 10c is too low, the patterned layer 10c is prone to flow during hard baking, thereby deforming the patterned layer 10c, affecting the pattern of the hollow area 11a on the hardened layer, so that the protrusion on the surface of the manufactured glass shell 200 is different from the pre-designed shape, affecting the accuracy of the three-dimensional texture structure on the surface of the manufactured glass shell 200, and reducing the designability of the manufacturing method. If the softening point of the patterned layer 10c is too high, it is difficult to repair the defects left by the development during hard baking, which affects the accuracy of the hollow area 11a on the mask layer 10a, and further affects the accuracy of the three-dimensional texture structure on the manufactured glass shell 200, reducing the designability of the pattern on the glass shell 200. When the softening point of the patterned layer 10c is between 140°C and 160°C, the photoresist layer 10b with the hollow pattern can be well prevented from flowing during hard baking, and the defects left by the development can be well repaired, thereby improving the accuracy of the three-dimensional texture structure on the manufactured glass shell 200.
[0065] "Softening point" refers to the temperature at which an amorphous polymer begins to soften.
[0066] Optionally, the weight average molecular weight of the patterned layer 10c is in the range of 5000≤Mw≤8000. Specifically, the weight average molecular weight of the patterned layer 10c may be, but is not limited to, 5000, 5500, 6000, 6500, 7000, 7500, 8000, etc. If the weight average molecular weight of the patterned layer 10c is too low, the softening point of the patterned layer 10c is too low, and the patterned layer 10c is prone to flow during hard baking, thereby causing the patterned layer 10c to deform, affecting the pattern of the hollow area 11a on the hardened layer, so that the protrusions on the surface of the manufactured glass shell 200 are different from the pre-designed shape, affecting the accuracy of the three-dimensional texture structure on the surface of the manufactured glass shell 200, and reducing the designability of the preparation method. If the weight average molecular weight of the patterned layer 10c is too large, the softening point of the patterned layer 10c is too high, and it is difficult to repair the defects left by the development during hard baking, which affects the accuracy of the hollow area 11a on the hardened layer, and further affects the accuracy of the three-dimensional texture structure on the manufactured glass shell 200, reducing the designability of the pattern on the glass shell 200. When the weight average molecular weight of the patterned layer 10c is between 5000 and 8000, it can well prevent the photoresist layer 10b with the hollow pattern from flowing during hard baking, and can well repair the defects left by the development, thereby improving the accuracy of the three-dimensional texture structure on the manufactured glass shell 200.
[0067] S1023, hard-bake the patterned layer 10c to obtain a mask layer 10a, wherein the mask layer 10a has a hollow area 11a.
[0068] Optionally, the patterned layer 10c is heated (for example, heated to a temperature of 150° C. to 170° C.) to hard bake the patterned layer 10c so that the patterned layer 10c is cured to form a mask layer 10a (also called a photoresist hard film). In other words, a developing device is used to perform a developing operation so that the texture pattern is clearly presented on the photoresist film layer, and then a drying and curing process is performed to form a texture pattern photoresist hard film.
[0069] In the embodiments of the present application, when a value range from a to b is involved, unless otherwise specified, it means that the value can be any value between a and b, including the endpoint value a and the endpoint value b. For example, if the temperature is 80°C to 120°C, it means that the temperature can be any value between 80°C and 120°C, including 80°C and 120°C.
[0070] It can be understood that the exposure amount of the exposed portion of the photoresist layer 10b is equal, so after hard baking, the curing degree of the portion outside the hollow area 11a of the mask layer 10a is the same.
[0071] It can be understood that the pattern formed by the hollow areas 11 a of the mask layer 10 a is consistent with the pattern of the hollow areas 11 a on the patterned layer 10 c.
[0072] Optionally, the temperature T at which the patterned layer 10c is hard-baked is greater than the softening point Ts of the patterned layer 10c, that is, T>Ts.
[0073] Optionally, the range of the difference T-Ts between the temperature T of hard baking the patterned layer 10c and the softening point Ts of the patterned layer 10c is: 3°C ≤ T-Ts ≤ 20°C. Specifically, the difference T-Ts between the temperature T of hard baking the patterned layer 10c and the softening point Ts of the patterned layer 10c may be, but is not limited to, 3°C, 5°C, 7°C, 9°C, 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, etc. If the difference T-Ts between the hard-baking temperature T of the patterned layer 10c and the softening point Ts of the patterned layer 10c is too small, it is difficult to repair the defects left by the development during the hard-baking, which affects the accuracy of the hollow area 11a on the obtained mask layer 10a, and further affects the accuracy of the three-dimensional texture structure on the manufactured glass shell 200, reducing the designability of the pattern on the glass shell 200; if the difference T-Ts between the hard-baking temperature T of the patterned layer 10c and the softening point Ts of the patterned layer 10c is too large, the patterned layer 10c is easy to flow during the hard-baking, thereby causing the patterned layer 10c to deform, affecting the pattern of the hollow area 11a on the manufactured hardened layer, so that the protrusion on the surface of the manufactured glass shell 200 is different from the pre-designed shape, affecting the accuracy of the three-dimensional texture structure on the surface of the manufactured glass shell 200, and reducing the designability of the preparation method.
[0074] Optionally, the raw material components of the mask layer 10a include p-cresol and m-cresol, and the molar ratio of the m-cresol to the p-cresol ranges from 0.9 to 1.5. In other words, the photoresist glue includes p-cresol and m-cresol, and in the photoresist glue, the molar ratio of the m-cresol to the p-cresol ranges from 0.9 to 1.5. Specifically, the molar ratio of the m-cresol to the p-cresol can be, but is not limited to, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, etc. If the molar ratio of m-cresol to p-cresol is too high, the precision of the mask layer 10a obtained will be reduced. If the molar ratio of m-cresol to p-cresol is too low, the content of p-cresol is too high, which affects the molecular weight of the mask layer 10a obtained, and also affects the precision of the mask layer 10a obtained.
[0075] Optionally, the photoresist glue solution includes a phenolic resin monomer, a coupling agent, a photosensitizer and a solvent. The phenolic resin monomer may include p-cresol and m-cresol. The solvent may be, but is not limited to, propylene glycol methyl ether acetate (PMA). The coupling agent may be, but is not limited to, at least one of 3-glycidoxypropyltrimethoxysilane (such as the trade name KBM-403 manufactured by Shin-Etsu Chemical) and 3-glycidoxypropylmethyldiethoxysilane (such as the trade name KBM-402 manufactured by Shin-Etsu Chemical). The photosensitizer may be, but is not limited to, at least one of an ester compound of 4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]diphenol and (6-diazo-5,6-dihydroxy-5-oxy-1-naphthalenesulfonic acid), an ester of 2,3,4-trihydroxybenzophenone and 1,2-naphthoquinonediazide-5-sulfonic acid, and an ester of 2,3,4,4'-tetrahydroxybenzophenone and 1,2-naphthoquinonediazide-5-sulfonic acid.
[0076] In a specific embodiment, the photoresist solution includes the following components in parts by weight: 20 to 25 parts of phenolic resin, 70 to 75 parts of propylene glycol methyl ether acetate, 1 to 2 parts of coupling agent, and 4 to 5 parts of photosensitizer.
[0077] Optionally, when wet etching is performed, the etching depth of the glass substrate 200a per minute is s1 (i.e., the etching depth of the glass substrate 200a per minute along the thickness direction), and the stripping width of the mask layer 10a and the glass substrate 200a per minute is s2, wherein 4≤s2 / s1≤10. In other words, the ratio of the stripping rate v2 of the mask layer 10a and the glass substrate 200a to the etching rate v1 of the glass substrate 200a is in the range of 4≤v2 / v1≤10. Specifically, s2 / s1 may be, but is not limited to, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, etc. If the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is too small, the peeling speed of the mask layer 10a and the glass substrate 200a is too slow, which affects the side etching rate of the glass substrate 200a, thereby affecting the formation of the gully-like texture, or the inclination of the etching surface is not enough, which affects the morphology of the three-dimensional texture structure on the surface of the glass shell 200; if the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is too large, the peeling speed of the mask layer 10a and the glass substrate 200a is too fast, and the etching of the area covered by the mask layer 10a and the uncovered area on the glass substrate 200a is closer to synchronization, and the entire large surface of the glass substrate 200a is almost synchronously etched, and the texture morphology of the concave-convex structure cannot be formed. When the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is between 4 and 10, the vertical etching along the thickness direction and the side etching along the side of the glass substrate 200a can have a more reasonable rate ratio, thereby forming a gully-shaped three-dimensional texture with stronger designability and better appearance effect.
[0078] In some embodiments, the wet etching of the glass substrate 200a includes: immersing the glass substrate 200a provided with the mask layer 10a in an etching solution at a temperature of 15°C to 30°C, and swinging the glass substrate 200a provided with the mask layer 10a to perform wet etching. As the etching proceeds, glass slag will be generated on the surface of the glass substrate 200a. Swinging the glass substrate 200a can accelerate the falling of the glass slag from the glass substrate 200a, thereby making the transition of the etching surface of the glass substrate 200a more natural, avoiding the slowing down of the etching rate of the area on the glass substrate 200a blocked by the glass slag, affecting the etching accuracy, and in addition, the etching rate of the glass substrate 200a can be accelerated to improve the production efficiency of the glass shell 200.
[0079] Optionally, during etching, the temperature of the etching solution may be, but is not limited to, 15°C, 18°C, 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, etc. If the temperature of the etching solution is too high, the reaction rate between the glass substrate 200a and the etching solution is too fast, which may easily make the etching rate of the glass substrate 200a uneven, resulting in a reduction in the accuracy of the three-dimensional texture morphology on the glass shell 200. If the temperature of the etching solution is too low, the etching solution is likely to crystallize and precipitate crystals, thereby affecting the etching rate of the glass substrate 200a along the thickness direction and the side etching rate in the side direction (perpendicular to the thickness direction), affecting the accuracy of the gully-shaped three-dimensional texture on the surface of the manufactured glass shell 200, and also reducing the production efficiency of the glass shell 200. When the temperature of the etching solution is between 15°C and 30°C, the crystallization of the etching solution can be well prevented, and the etching rate of the glass substrate 200a can be controlled within a reasonable range, so that the transition of the etched surface of the glass substrate 200a is more natural, the etching is more uniform, and the obtained three-dimensional texture morphology has higher precision and better appearance.
[0080] Furthermore, the temperature of the etching solution may be 20° C. to 25° C. When the temperature of the etching solution is between 20° C. and 25° C., the crystallization of the etching solution can be well prevented, and the etching rate of the glass substrate 200a can be better controlled, so that the etching of each position of the glass substrate 200a is more uniform, the transition of the etched surface is more natural, the obtained three-dimensional texture morphology is more accurate, and the appearance effect is better.
[0081] In some embodiments, the swing amplitude of the swing is in the range of 400mm to 500mm. Specifically, the swing amplitude may be, but is not limited to, 400mm, 410mm, 420mm, 430mm, 440mm, 450mm, 455mm, 460mm, 465mm, 470mm, 475mm, 480mm, 485mm, 490mm, 495mm, 500mm, etc. If the swing amplitude is too small, it is difficult to remove the glass debris on the glass substrate 200a, and it is difficult to solve the problem of uneven etching caused by the residual glass debris on the glass substrate 200a; if the swing amplitude is too large, the removal rate of the glass debris is not significantly increased, but it is easy to cause the etching liquid to splash, or exceed the maximum swing amplitude of the etching equipment, which increases the requirements for the etching equipment.
[0082] In some embodiments, the swing frequency of the swing is 30 times / min to 60 times / min. Specifically, the swing frequency of the swing can be, but is not limited to, 30 times / min, 35 times / min, 40 times / min, 45 times / min, 50 times / min, 55 times / min, 60 times / min, etc. If the swing frequency is too small, it is difficult to make the glass slag on the glass substrate 200a fall off well, and it is difficult to solve the problem of uneven etching caused by the residual glass slag on the glass substrate 200a; if the swing frequency is too large, the removal rate of the glass slag is not significantly increased, but it is easy to cause the etching liquid to splash, and the requirements for the etching equipment are increased.
[0083] Optionally, when etching is performed, the etching time is 8 minutes to 20 minutes. In other words, the swing time is 8 minutes to 20 minutes. Further, when etching is performed, the etching time is 10 minutes to 15 minutes. Specifically, when etching is performed, the etching time can be but is not limited to 8 minutes, 10 minutes, 12 minutes, 15 minutes, 18 minutes, 20 minutes, etc. If the etching time is too short, the etching depth of the glass substrate 200a is not enough, and it is difficult to obtain a three-dimensional texture structure with a pre-designed depth; if the etching time is too long, the area of the mask layer 10a peeled off is too large, and the mask layer 10a may even fall off as a whole, affecting the morphology of the three-dimensional texture structure on the obtained glass shell 200.
[0084] The etching time is not only related to the depth of the desired groove-shaped or peak-shaped three-dimensional texture structure, but also to the line width and thickness of the mask layer 10a. The larger the line width and thickness of the mask layer 10a, the longer the time it takes for the mask layer 10a to peel off after being immersed in the etching solution, and the less likely it is to fall off, and the longer it can withstand etching. However, if the line width of the mask layer 10a is too long, it will affect the size of the obtained groove-shaped or peak-shaped three-dimensional texture structure, making it difficult to prepare a finer groove-shaped or peak-shaped three-dimensional texture structure.
[0085] In some embodiments, the etching solution includes, by mass fraction, 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid, and 3% to 5% fluoride salt, with the remainder being water.
[0086] During etching, the hydrofluoric acid in the etching solution plays a leading role in the erosion of the silicon dioxide network skeleton in the glass substrate 200a. Specifically, the hydrofluoric acid provides hydrogen ions to replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provides fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a to form a fluorosilicate etching particle layer, which plays a major etching role. Sulfuric acid, phosphoric acid, and aminosulfonic acid can provide hydrogen ions to ensure that the concentration of hydrogen ions in the etching solution is in a stable state of high concentration during the reaction process, replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provide basic conditions for fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a; at the same time, the mixed use of multiple acid solutions (i.e., the mixed use of sulfuric acid, phosphoric acid, and aminosulfonic acid) can give full play to the mixed acid effect of the etching solution, achieve the purpose of uniform etching, ensure the natural transition of the etching surface of the glass substrate 200a, and thus achieve a three-dimensional etching effect of a texture pattern with ravines and grooves. The fluoride salt in the etching solution can provide fluoride ions, timely replenish the consumption of fluoride ions in the etching solution during the etching process, and ensure that the efficacy of the etching solution is long-lasting and stable. In short, the etching solution of this embodiment is compounded by using hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid and fluoride salt, so that the etching solution etches the glass substrate 200a, and the etching depth of the glass substrate 200a along the depth direction and the ratio of the stripping width of the mask layer 10a to the glass substrate 200a are maintained in a more reasonable range, so that the etching of the glass substrate 200a by the etching solution is more balanced, and the etched surface obtained by etching can have a natural transition, and the gully-like texture of the three-dimensional structure is better formed.
[0087] Optionally, the fluoride salt may be, but is not limited to, at least one of sodium fluoride, ammonium fluoride, potassium fluoride, and the like.
[0088] Optionally, in the etching solution, the mass fraction of the hydrofluoric acid may be, but not limited to, 20%, 22%, 24%, 26%, 28%, 30%, etc. In the etching solution, the mass fraction of the sulfuric acid may be, but not limited to, 15%, 17%, 19%, 21%, 23%, 25%, etc. In the etching solution, the mass fraction of the phosphoric acid may be, but not limited to, 10%, 12%, 14%, 16%, 18%, 20%, etc. In the etching solution, the mass fraction of the aminosulfonic acid may be, but not limited to, 3%, 5%, 6%, 7%, 9%, 10%, etc. In the etching solution, the mass fraction of the fluoride salt may be, but not limited to, 3%, 3.5%, 4%, 4.5%, 5%, etc.
[0089] In some embodiments, the etching solution further comprises: 0.2% to 0.5% ferric chloride by mass fraction. It can be understood that in this embodiment, the etching solution comprises: 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid, 3% to 5% fluoride salt and 0.2% to 0.5% ferric chloride by mass fraction, and the balance is water. A large amount of micron-sized glass debris will be generated during the etching process. During swing etching, these fine glass debris are always suspended in the etching solution. When these glass debris reach a certain concentration, they will have a certain impact on the etching effect of the glass substrate 200a. Therefore, a certain proportion of ferric chloride is added to the etching solution. By utilizing the flocculation effect of ferric chloride, in the interval of stopping the etching operation (or when the glass substrate 200a stops swinging), these suspended glass debris are allowed to settle as soon as possible and are regularly removed to ensure the stability of the efficacy of the etching solution. Ferric chloride can avoid strong swinging and stirring during the etching process. These fine glass slag particles will impact the surface of the glass substrate 200a or even be adsorbed on the surface of the glass substrate 200a to cause etching defects, thereby reducing the surface defects of the manufactured glass shell 200, so that the groove-shaped texture structure of the obtained glass shell 200 has a better appearance effect.
[0090] Optionally, in the etching solution, the mass fraction of ferric chloride may be, but is not limited to, 0.2%, 0.3%, 0.4%, 0.5%, etc.
[0091] In some embodiments, the etching solution further comprises, by mass fraction: The etching solution further comprises, by mass fraction: 0.2% to 0.5% sodium dodecylbenzene sulfonate. It can be understood that in this embodiment, the etching solution comprises, by mass fraction: 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid, 3% to 5% fluoride salt, 0.2% to 0.5% ferric chloride and 0.2% to 0.5% sodium dodecylbenzene sulfonate, and the balance is water. Sodium dodecylbenzene sulfonate can increase the wettability (infiltration) of the etching solution and the glass substrate 200a, so that the etching solution can more evenly infiltrate the surface of the glass substrate 200a, and reduce the omission of etching reaction caused by poor wettability on the surface of the glass substrate 200a. Therefore, the etching of the surface of the glass substrate 200a can be more uniform, and the transition of the etched surface of the manufactured glass shell 200 can be more natural, and the groove-like three-dimensional texture structure on the surface of the glass shell 200 has a better feel.
[0092] Optionally, in the etching solution, the mass fraction of sodium dodecylbenzene sulfonate may be, but is not limited to, 0.2%, 0.3%, 0.4%, or 0.5%.
[0093] Optionally, the etching solution is prepared by the following steps: hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid, fluoride salt, ferric chloride, sodium dodecylbenzenesulfonate and water are weighed respectively according to weight ratio, mixed, stirred evenly, and left to stand for aging for 24 to 72 hours (e.g., 24h, 36h, 48h, 60h, 72h, etc.) for use.
[0094] See also Figure 5 The embodiment of the present application further provides a glass shell 200 , and the glass shell 200 is prepared by the preparation method of the glass shell 200 described in the embodiment of the present application.
[0095] See also Figure 6 and Figure 7 The embodiment of the present application further provides a glass shell 200, the glass shell 200 includes a main body 210 and a plurality of protrusions 230, the main body 210 has a first surface 211, the plurality of protrusions 230 are arranged on the first surface 211 of the main body 210, the protrusions 230 have a second surface 231 connected to the first surface 211, the angle α between the first surface 211 and the second surface 231 is greater than 90°, and the protrusions 230 are obtained by wet etching from a glass substrate 200a.
[0096] It can be understood that the main body 210 and the plurality of protrusions 230 form a concave-convex texture structure formed on the surface of the glass housing 200 , such as a gully-shaped or mountain-shaped three-dimensional texture structure.
[0097] It can be understood that the first surface 211 can be one surface or multiple surfaces of all surfaces of the main body 210, or a partial surface of a surface of the main body 210, or all surfaces. The selection of the first surface 211 is determined according to the decorative effect that the main body 210 needs to present. In the schematic diagram of this embodiment, the first surface 211 is taken as an example of a surface of the main body 210, which should not be understood as a limitation on the main body 210 provided in the embodiment of the present application.
[0098] The glass shell 200 of the present application can be applied to portable electronic devices such as mobile phones, tablet computers, laptop computers, desktop computers, smart bracelets, smart watches, e-readers, game consoles, etc. Optionally, the glass shell 200 of the present application can be a back cover (battery cover), a middle frame, a decorative piece, etc. of an electronic device. The glass shell 200 of the embodiment of the present application can be a 2D structure, a 2.5D structure, a 3D structure, etc.
[0099] The glass shell 200 of the embodiment of the present application includes a body 210 and a protrusion 230. The body 210 has a first surface 211. The protrusions 230 are arranged on the first surface 211 of the body 210. The protrusions 230 have a second surface 231 connected to the first surface 211. The angle between the first surface 211 and the second surface 231 is greater than 90°, so that the glass shell 200 has a three-dimensional texture pattern. By designing the three-dimensional texture pattern, the texture effect of the surface of the glass shell 200 can be changed. In addition, the glass shell 200 can also present a flashing texture effect by designing the protrusions 230. The glass shell 200 is obtained by setting a mask layer 10a and performing wet etching. The process is simple, and the size, shape and arrangement of the protrusions 230 on the glass shell 200 are highly designable.
[0100] Optionally, the plurality of protrusions 230 may be arranged randomly or according to a preset rule, such as a periodic arrangement. Optionally, the plurality of protrusions 230 may be arranged according to a pre-designed effect to be presented, such as a snowflake texture, a hexagonal pyramid texture, a flash sand texture, a Fresnel texture, a CD texture, etc. In addition, the plurality of protrusions 230 may be arranged according to a preset rule in such a way that at least one of the size or density of the plurality of protrusions 230 is arranged in a gradual manner, such as at least one of the size or density of the protrusions 230 gradually changes from one side to the other side, or at least one of the size or density of the protrusions 230 gradually changes along the radial direction.
[0101] Optionally, the protrusion 230 has a reflection or refraction effect on light (such as visible light), so that the protrusion 230 presents a glittering effect, thereby making the glass housing 200 present a glittering texture.
[0102] Optionally, the thickness of the glass shell 200 is 0.3 mm to 1 mm; specifically, the thickness of the glass shell 200 may be, but is not limited to, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, etc. When the glass shell 200 is too thin, it cannot play a good supporting and protective role, and the mechanical strength cannot meet the requirements of the electronic device shell. When the glass shell 200 is too thick, the weight of the electronic device is increased, affecting the feel of the electronic device and the user experience is not good.
[0103] Optionally, the range of the roughness Ra of the surface of the glass shell 200 with the protrusion 230 is 1μm≤Ra≤3μm. Specifically, the roughness of the glass shell 200 may be, but is not limited to, 1μm, 1.2μm, 1.4μm, 1.6μm, 1.8μm, 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 3μm, etc. If the roughness Ra of the surface of the glass shell 200 with the protrusion 230 is too small, the etching depth of the glass shell 200 is insufficient, the height of the protrusion 230 is too small, the texture effect is not obvious, and when a flashing texture is required, the flashing degree of the texture is insufficient; if the roughness Ra of the surface of the glass shell 200 with the protrusion 230 is too large, the scratching feeling of the glass shell 200 is increased, affecting the feel of the glass shell 200.
[0104] Furthermore, the roughness Ra of the surface of the glass shell 200 with the protrusion 230 is in the range of 1.8 μm≤Ra≤2.3 μm. When the roughness Ra of the surface of the glass shell 200 with the protrusion 230 is in this range, diffuse reflection can be better, so that the glass shell 200 can present a more shiny glittering texture.
[0105] Optionally, the light transmittance T of the glass shell 200 is in the range of 20%≤T≤40%. Optionally, the light transmittance of the glass shell 200 may be, but not limited to, 20%, 23%, 25%, 28%, 30%, 33%, 35%, 38%, 40%, etc. The lower the light transmittance of the glass shell 200, the stronger the reflection of the light by the protrusion 230, and the stronger the flash effect of the protrusion 230, but the height of the protrusion 230 (i.e., the etching depth of the glass shell 200) is, the deeper it is. Therefore, when the light transmittance of the glass shell 200 is too low, the scratching feel of the glass shell 200 is increased, the feel of the glass shell 200 is reduced, and the etching time during preparation is increased; when the light transmittance of the glass shell 200 is too large, the reflectivity is low, and the flash brightness of the protrusion 230 is reduced. The light transmittance of the present application refers to the transmittance of visible light.
[0106] Optionally, the haze H of the glass shell 200 is in the range of 60%≤H≤90%; specifically, the haze of the glass shell 200 may be, but is not limited to, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc. The higher the haze of the glass shell 200, the lower the light transmittance of the glass shell 200, the stronger the light reflection, and the stronger the scratching feeling of the protrusion 230; the lower the haze of the glass shell 200, the higher the light transmittance of the glass shell 200, and the lower the flash brightness of the protrusion 230. When the haze is too low, it will affect the formation of diffuse reflection, thereby affecting the flash brightness of the protrusion 230.
[0107] Optionally, the glossiness G of the glass shell 200 is in the range of 80Gu≤G≤100Gu. Specifically, the glossiness of the glass shell 200 may be, but is not limited to, 80Gu, 85Gu, 90Gu, 95Gu, 100Gu, etc. The higher the glossiness of the glass shell 200, the better the texture of the glass shell 200, and thus the better the appearance.
[0108] Optionally, the minimum width w of the orthographic projection of the protrusion 230 on the first surface 211 is in the range of 50 μm ≤ w ≤ 80 μm. Specifically, the minimum width w of the orthographic projection of the protrusion 230 on the first surface 211 may be, but is not limited to, 50 μm, 53 μm, 55 μm, 58 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, etc. If the minimum width w of the orthographic projection of the protrusion 230 on the first surface 211 is too small, the etching depth is too shallow during etching, and it is difficult to achieve the required haze, thereby affecting the diffuse reflection of the surface of the glass shell 200 and affecting the flash effect of the glass shell 200; if the minimum width w of the orthographic projection of the protrusion 230 on the first surface 211 is too large, it takes a long time to obtain a groove-shaped or mountain-shaped protrusion 230 by wet etching, so the height of the formed protrusion 230 is too large, and the depth between adjacent protrusions 230 is too deep, which affects the mechanical strength of the glass shell 200.
[0109] Optionally, along the direction perpendicular to the first surface 211, the maximum height h of the protrusion 230 is in the range of 9μm≤h≤13μm. Specifically, the maximum height h of the protrusion 230 may be, but is not limited to, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, etc. If the maximum height h of the protrusion 230 is too large, the depth between adjacent protrusions 230 is too deep, affecting the mechanical strength of the glass shell 200; if the maximum height h of the protrusion 230 is too small, it is difficult to achieve the required haze, thereby affecting the diffuse reflection of the surface of the glass shell 200 and affecting the flash effect of the glass shell 200.
[0110] Optionally, the minimum spacing d between any two adjacent protrusions 230 is in the range of 5μm≤d≤10μm. Specifically, the minimum spacing d between any two adjacent protrusions 230 may be, but is not limited to, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc. If the minimum spacing d between any two adjacent protrusions 230 is too small, the depth of etching will be affected, so that the maximum height and haze of the protrusions 230 cannot meet the requirements, affecting the diffuse reflection of the surface of the glass shell 200 and the flash effect of the glass shell 200; if the minimum spacing d between any two adjacent protrusions 230 is too large, the protrusions 230 in the shape of a gully or a peak will be obtained by wet etching, which requires a long etching time, and the height of the formed protrusions 230 is too large, and the depth between adjacent protrusions 230 is too deep, which affects the mechanical strength of the glass shell 200.
[0111] Optionally, the protrusion 230 is formed by wet etching of the glass substrate 200a, including: forming a mask layer 10a on the glass substrate 200a, the mask layer 10a having a hollow area 11a, performing wet etching to gradually peel off the mask layer 10a from the edge portion adjacent to the hollow area 11a toward a direction away from the hollow area 11a from the glass substrate 200a.
[0112] During etching, the mask layer 10a is not etched by the etching solution, but the edge portion of the mask layer 10a adjacent to the hollow area 11a is gradually separated from the glass substrate 200a in a direction away from the hollow area 11a (in other words, gradually peeled off), so that the area covered by the mask layer 10a is gradually etched from the side of the position adjacent to the hollow area 11a, so that the surface of the glass substrate 200a forms a gully-shaped three-dimensional texture pattern or a convex vein-shaped peak-shaped three-dimensional texture pattern, so that the glass shell 200 has a gully-shaped three-dimensional texture (3D) pattern.
[0113] Optionally, the etching depth of the glass substrate per minute is s1, and the stripping width of the mask layer 10a and the glass substrate per minute is s2, wherein 4≤s2 / s1≤10. In other words, the ratio of the stripping rate v2 of the mask layer 10a and the glass substrate 200a to the etching rate v1 of the glass substrate 200a is in the range of 4≤v2 / v1≤10. Specifically, s2 / s1 may be, but is not limited to, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, etc. If the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is too small, the peeling speed of the mask layer 10a and the glass substrate 200a is too slow, which affects the side etching rate of the glass substrate 200a, thereby affecting the formation of the gully-like texture, or the inclination of the etching surface is not enough, which affects the morphology of the three-dimensional texture structure on the surface of the glass shell 200; if the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is too large, the peeling speed of the mask layer 10a and the glass substrate 200a is too fast, and the etching of the area covered by the mask layer 10a and the uncovered area on the glass substrate 200a is closer to synchronization, and the entire large surface of the glass substrate 200a is almost synchronously etched, and the texture morphology of the concave-convex structure cannot be formed. When the ratio s2 / s1 of the peeling width s2 of the mask layer 10a and the glass substrate 200a per minute to the etching depth s1 of the glass substrate 200a per minute is between 4 and 10, the vertical etching along the thickness direction and the side etching along the side of the glass substrate 200a can have a more reasonable rate ratio, thereby forming a gully-shaped three-dimensional texture with stronger designability and better appearance effect.
[0114] Optionally, the wet etching is performed using an etching solution, and the etching solution includes hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid and fluoride salts.
[0115] During etching, the hydrofluoric acid in the etching solution plays a leading role in the erosion of the silicon dioxide network skeleton in the glass substrate 200a. Specifically, the hydrofluoric acid provides hydrogen ions to replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provides fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a to form a fluorosilicate etching particle layer, which plays a major etching role. Sulfuric acid, phosphoric acid, and aminosulfonic acid can provide hydrogen ions to ensure that the concentration of hydrogen ions in the etching solution is in a stable state of high concentration during the reaction process, replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provide basic conditions for fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a; at the same time, the mixed use of multiple acid solutions (i.e., the mixed use of sulfuric acid, phosphoric acid, and aminosulfonic acid) can give full play to the mixed acid effect of the etching solution, achieve the purpose of uniform etching, ensure the natural transition of the etching surface of the glass substrate 200a, and thus achieve a three-dimensional etching effect of a texture pattern with ravines and grooves. The fluoride salt in the etching solution can provide fluoride ions, timely replenish the consumption of fluoride ions in the etching solution during the etching process, and ensure that the efficacy of the etching solution is long-lasting and stable. In short, the etching solution of this embodiment is compounded by using hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid and fluoride salt, so that the etching solution etches the glass substrate 200a, and the etching depth of the glass substrate 200a along the depth direction and the ratio of the stripping width of the mask layer 10a to the glass substrate 200a are maintained in a more reasonable range, so that the etching of the glass substrate 200a by the etching solution is more balanced, and the etched surface obtained by etching can have a natural transition, and the gully-like texture of the three-dimensional structure is better formed.
[0116] An embodiment of the present application also provides an etching solution, which is used to etch glass. The etching solution includes, by mass fraction: 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid; and 3% to 5% fluoride salt, and the remainder is water.
[0117] Optionally, in the etching solution, the mass fraction of the hydrofluoric acid may be, but not limited to, 20%, 22%, 24%, 26%, 28%, 30%, etc. In the etching solution, the mass fraction of the sulfuric acid may be, but not limited to, 15%, 17%, 19%, 21%, 23%, 25%, etc. In the etching solution, the mass fraction of the phosphoric acid may be, but not limited to, 10%, 12%, 14%, 16%, 18%, 20%, etc. In the etching solution, the mass fraction of the aminosulfonic acid may be, but not limited to, 3%, 5%, 6%, 7%, 9%, 10%, etc. In the etching solution, the mass fraction of the fluoride salt may be, but not limited to, 3%, 3.5%, 4%, 4.5%, 5%, etc.
[0118] In this embodiment, hydrofluoric acid, sulfuric acid, phosphoric acid, and aminosulfonic acid are used to prepare a mixed acid. The inherent properties of sulfuric acid, phosphoric acid, and aminosulfonic acid can be used to coordinate and influence the dissolution of the glass substrate 200a by hydrofluoric acid, thereby playing a compatibility role. The principle is that various silicates are formed by complex chemical reactions of sulfate ions, phosphate ions, aminosulfonic acid ions, etc. on the surface of the glass substrate 200a. Due to their inherent properties, they change the solubility of various silicates through hydrogen bonding to achieve a natural transition etching effect.
[0119] During etching, the hydrofluoric acid in the etching solution plays a leading role in the erosion of the silicon dioxide network skeleton in the glass substrate 200a. Specifically, the hydrofluoric acid provides hydrogen ions to replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provides fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a to form a fluorosilicate etching particle layer, which plays a major etching role. Sulfuric acid, phosphoric acid, and aminosulfonic acid can provide hydrogen ions to ensure that the concentration of hydrogen ions in the etching solution is in a stable state of high concentration during the reaction process, replace the metal cations in the glass substrate 200a to generate a silica gel layer, and provide basic conditions for fluorine ions to erode the silicon dioxide skeleton in the glass substrate 200a; at the same time, the mixed use of multiple acid solutions (i.e., the mixed use of sulfuric acid, phosphoric acid, and aminosulfonic acid) can give full play to the mixed acid effect of the etching solution, achieve the purpose of uniform etching, ensure the natural transition of the etching surface of the glass substrate 200a, and thus achieve a three-dimensional etching effect of a texture pattern with ravines and grooves. The fluoride salt in the etching solution can provide fluoride ions, timely replenish the consumption of fluoride ions in the etching solution during the etching process, and ensure that the efficacy of the etching solution is long-lasting and stable. In short, the etching solution of this embodiment is compounded by using hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid and fluoride salt, so that the etching solution etches the glass substrate 200a, and the etching depth of the glass substrate 200a along the depth direction and the ratio of the stripping width of the mask layer 10a to the glass substrate 200a are maintained in a more reasonable range (for example, between 4 and 10), so that the etching solution etches the glass substrate 200a more evenly, and the etched surface obtained by etching can have a natural transition, and the gully-like texture of the three-dimensional structure is better formed.
[0120] Optionally, the fluoride salt may be, but is not limited to, at least one of sodium fluoride, ammonium fluoride, potassium fluoride, and the like.
[0121] In some embodiments, the etching solution includes, by mass fraction, 24% to 26% hydrofluoric acid, 18% to 22% sulfuric acid, 13% to 16% phosphoric acid, 5% to 8% aminosulfonic acid, and 3.5% to 4.5% fluoride salt. When the etching solution includes substances with these components and contents, when used to etch the glass substrate 200a, the etching depth of the glass substrate 200a along the depth direction and the ratio of the stripping width of the mask layer 10a to the glass substrate 200a can be kept in a more reasonable range, the etching solution etches the glass substrate 200a more evenly, and the etched surface obtained by etching can have a natural transition, so as to better form a gully-like texture of a three-dimensional structure.
[0122] In some embodiments, the etching solution further comprises: 0.2% to 0.5% ferric chloride by mass fraction. It can be understood that in this embodiment, the etching solution comprises: 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid, 3% to 5% fluoride salt and 0.2% to 0.5% ferric chloride by mass fraction, and the balance is water. A large amount of micron-sized glass debris will be generated during the etching process. During swing etching, these fine glass debris are always suspended in the etching solution. When these glass debris reach a certain concentration, they will have a certain impact on the etching effect of the glass substrate 200a. Therefore, a certain proportion of ferric chloride is added to the etching solution. By utilizing the flocculation effect of ferric chloride, in the interval of stopping the etching operation (or when the glass substrate 200a stops swinging), these suspended glass debris are allowed to settle as soon as possible and are regularly removed to ensure the stability of the efficacy of the etching solution.
[0123] In some embodiments, the etching solution further comprises, by mass fraction: the etching solution further comprises, by mass fraction: 0.2% to 0.5% sodium dodecylbenzene sulfonate. It can be understood that in this embodiment, the etching solution comprises, by mass fraction: 20% to 30% hydrofluoric acid, 15% to 25% sulfuric acid, 10% to 20% phosphoric acid, 3% to 10% aminosulfonic acid, 3% to 5% fluoride salt, 0.2% to 0.5% ferric chloride and 0.2% to 0.5% sodium dodecylbenzene sulfonate, and the balance is water. Sodium dodecylbenzene sulfonate can increase the wettability (wetting property) of the etching solution and the glass substrate 200a, so that the etching solution can more evenly infiltrate the surface of the glass substrate 200a, thereby making the etching of the surface of the glass substrate 200a more uniform, improving the transition of the etched surface of the manufactured glass shell 200 to be more natural, and the groove-like three-dimensional texture structure on the surface of the glass shell 200 has a better feel.
[0124] The following further describes the method for preparing the glass housing 200 according to the embodiment of the present application through specific examples.
[0125] Example 1
[0126] The glass housing 200 of this embodiment is prepared by the following steps:
[0127] 1) preparing an etching solution (mass fraction wt%): weighing hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid, fluoride salt, ferric chloride, sodium dodecylbenzene sulfonate and water according to the weight ratio of each component in the pre-designed etching solution, stirring and mixing them evenly, and standing and aging for 48 hours for use; the prepared etching solution includes 30% hydrofluoric acid, 15% sulfuric acid, 10% phosphoric acid, 6.5% aminosulfonic acid, 3.5% sodium fluoride, 0.2% ferric chloride, 0.3% sodium dodecylbenzene sulfonate, and 34.5% water;
[0128] 2) providing a glass substrate 200a (such as a mobile phone rear cover glass original sheet), cleaning and drying the glass substrate 200a, coating a photoresist solution on the surface of the glass substrate 200a, and removing the solvent to obtain a photoresist layer 10b;
[0129] 3) performing exposure operation using a photolithography machine to obtain a photoresist layer 10b having a hollow pattern;
[0130] 4) performing a developing operation using a developing device to form the mask layer 10a on the surface of the glass substrate 200a, wherein the mask layer 10a has a hollow area 11a;
[0131] 5) placing the glass substrate 200a with the mask layer 10a into an etching solution for swinging, wherein the temperature of the etching solution is controlled at 25°C, the swing amplitude is 450mm, the swing frequency is 35 times / minute, and the swing etching time is 11 minutes; and
[0132] 6) After the set etching time is reached, the glass substrate 200a with the mask layer 10a is taken out and cleaned with flowing pure water. After air drying, the desired three-dimensional etched glass shell 200 (such as a mobile phone glass back cover) with a similar texture pattern can be obtained.
[0133] The surface morphology of the glass housing 200 prepared in this embodiment is shown in FIG. Figure 8 and Fig. 9 As shown, Figure 8 and Fig. 9 The topography image was taken using a 3D laser microscope (160 times).
[0134] Example 2
[0135] 1) preparing an etching solution (mass fraction wt%): weighing hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid, fluoride salt, ferric chloride, sodium dodecylbenzene sulfonate and water according to the weight ratio of each component in the pre-designed etching solution, stirring and mixing them evenly, and standing and maturing for 48 hours for use; the prepared etching solution includes 25% hydrofluoric acid, 20% sulfuric acid, 12% phosphoric acid, 5% aminosulfonic acid, 5% sodium fluoride, 0.3% ferric chloride, 0.2% sodium dodecylbenzene sulfonate, and 32.5% water;
[0136] 2) providing a glass substrate 200a (such as a mobile phone rear cover glass original sheet), cleaning and drying the glass substrate 200a, coating a photoresist solution on the surface of the glass substrate 200a, and removing the solvent to obtain a photoresist layer 10b;
[0137] 3) performing exposure operation using a photolithography machine to obtain a photoresist layer 10b having a hollow pattern;
[0138] 4) performing a developing operation using a developing device to form the mask layer 10a on the surface of the glass substrate 200a, wherein the mask layer 10a has a hollow area 11a;
[0139] 5) placing the glass substrate 200a with the mask layer 10a into an etching solution for swinging, wherein the temperature of the etching solution is controlled at 20°C, the swing amplitude is 400mm, the swing frequency is 50 times / minute, and the swing etching time is 8 minutes; and
[0140] 6) After the set etching time is reached, the glass substrate 200a with the mask layer 10a is taken out and cleaned with flowing pure water. After air drying, the desired three-dimensional etched glass shell 200 (such as a mobile phone glass back cover) with a similar texture pattern can be obtained.
[0141] Example 3
[0142] 1) preparing an etching solution (mass fraction wt%): weighing hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid, fluoride salt, ferric chloride, sodium dodecylbenzene sulfonate and water according to the weight ratio of each component in the pre-designed etching solution, stirring and mixing them evenly, and standing and aging for 48 hours for use; the prepared etching solution includes 20% hydrofluoric acid, 25% sulfuric acid, 15% phosphoric acid, 3% aminosulfonic acid, 3.5% sodium fluoride, 0.3% ferric chloride, 0.3% sodium dodecylbenzene sulfonate, and 32.9% water;
[0143] 2) providing a glass substrate 200a (such as a mobile phone rear cover glass original sheet), cleaning and drying the glass substrate 200a, coating a photoresist solution on the surface of the glass substrate 200a, and removing the solvent to obtain a photoresist layer 10b;
[0144] 3) performing exposure operation using a photolithography machine to obtain a photoresist layer 10b having a hollow pattern;
[0145] 4) performing a developing operation using a developing device to form the mask layer 10a on the surface of the glass substrate 200a, wherein the mask layer 10a has a hollow area 11a;
[0146] 5) placing the glass substrate 200a with the mask layer 10a into an etching solution for swinging, wherein the temperature of the etching solution is controlled at 20°C, the swing amplitude is 500mm, the swing frequency is 60 times / minute, and the swing etching time is 15 minutes; and
[0147] 6) After the set etching time is reached, the glass substrate 200a with the mask layer 10a is taken out and cleaned with flowing pure water. After air drying, the desired three-dimensional etched glass shell 200 (such as a mobile phone glass back cover) with a similar texture pattern can be obtained.
[0148] The light transmittance, roughness, glossiness and haze of the glass substrate 200 a and the glass housing 200 obtained in Examples 1 to 3 were measured. The measurement results are shown in Table 1 below.
[0149] Table 1 Parameters of the glass housing 200 of each embodiment
[0150] Example Glass substrate Example 1 Example 2 Example 3 Light transmittance (%) 99.8 36.5 38.3 37.8 Roughness(μm) 0.00 2.05 1.95 1.98 Glossiness(Gu) 145 90.5 88.6 89.5 Haze(%) 0.00 69.2 68.5 68.8
[0151] From the test results of Examples 1 to 3, it can be seen that after the mask layer 10a is disposed on the glass substrate 200a, etching is performed using the etching solution of the present application to obtain a glass shell 200 with a clear groove-like three-dimensional texture pattern, and the obtained glass shell 200 has good glossiness and sparkle.
[0152] See also Figures 10 to 12 The embodiment of the present application further provides an electronic device 300, which includes a display screen 310, a glass shell 200 manufactured by the preparation method described in the embodiment of the present application or the glass shell 200 described in the embodiment of the present application, the glass shell 200 and the display screen 310 are arranged back to back, the processor 330 is located between the glass shell 200 and the display screen 310, and the processor 330 is electrically connected to the display screen 310 for controlling the display screen 310 to display.
[0153] The electronic device 300 of the embodiment of the present application may be, but is not limited to, a portable electronic device such as a mobile phone, a tablet computer, a laptop computer, a desktop computer, a smart bracelet, a smart watch, an e-reader, a game console, etc.
[0154] For a detailed description of the glass housing 200 , please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.
[0155] Optionally, the display screen 310 may be, but is not limited to, one or more of a liquid crystal display screen, a light emitting diode display screen (LED display screen), a micro light emitting diode display screen (Micro LED display screen), a sub-millimeter light emitting diode display screen (Mini LED display screen), an organic light emitting diode display screen (OLED display screen), etc.
[0156] Optionally, the processor 330 includes one or more general-purpose processors, wherein the general-purpose processor can be any type of device capable of processing electronic instructions, including a central processing unit (CPU), a microprocessor, a microcontroller, a main processor, a controller, and an ASIC, etc. The processor 330 is used to execute various types of digital storage instructions, such as software or firmware programs stored in a memory, which enables the computing device to provide a wide variety of services.
[0157] Optionally, the electronic device 300 of the present application further includes a memory 350. The memory 350 is electrically connected to the processor 330 and is used to store program codes required for the processor 330 to run, program codes required for controlling the display screen 310, display content of the display screen 310, and the like.
[0158] Optionally, the memory 350 may include a volatile memory (Volatile Memory), such as a random access memory (Random Access Memory, RAM); the memory 350 may also include a non-volatile memory (NVM), such as a read-only memory (Read-Only Memory, ROM), a flash memory (Flash Memory, FM), a hard disk drive (Hard Disk Drive, HDD) or a solid-state drive (SSD). The memory 350 may also include a combination of the above-mentioned types of memory.
[0159] See also Fig.13 In some embodiments, the electronic device 300 of the embodiment of the present application further includes a middle frame 320 and a camera module 370, wherein the middle frame 320 is disposed between the display screen 310 and the glass shell 200, and the side of the middle frame 320 is exposed to the glass shell 200 and the display screen 310. The middle frame 320 and the glass shell 200 enclose a housing space (not shown), and the housing space is used to accommodate the processor 330, the memory 350 and the camera module 370. The camera module 370 is electrically connected to the processor 330, and is used to shoot under the control of the processor 330.
[0160] Optionally, the glass housing 200 has a light-transmitting portion 201, and the camera module 370 can shoot through the light-transmitting portion 201 on the glass housing 200, that is, the camera module 370 in this embodiment is a rear camera module 370. It can be understood that in other embodiments, the light-transmitting portion 201 can be set on the display screen 310, that is, the camera module 370 is a front camera module 370. In the schematic diagram of this embodiment, the light-transmitting portion 201 is illustrated as an opening. In other embodiments, the light-transmitting portion 201 may not be an opening, but a light-transmitting material, such as plastic, glass, etc.
[0161] It can be understood that the electronic device 300 described in this embodiment is only one form of the electronic device 300 used by the glass shell 200, and should not be understood as a limitation on the electronic device 300 provided in this application, nor should it be understood as a limitation on the glass shell 200 provided in each embodiment of this application.
[0162] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, provided that there is no contradiction between them.
[0163] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A method for preparing a glass shell, characterized in that: include: providing a glass substrate; forming a mask layer on the surface of the glass substrate, wherein the mask layer has a hollow area; as well as The glass substrate is wet-etched in an etching solution to obtain a glass shell, wherein the etching solution includes hydrofluoric acid, sulfuric acid, phosphoric acid and aminosulfonic acid, so that during the wet etching, the mask layer is gradually peeled off from the glass substrate from the edge portion adjacent to the hollow area toward a direction away from the hollow area.
2. The method for preparing a glass casing according to claim 1, characterized in that: When wet etching is performed, the etching depth of the glass substrate per minute is s1, and the peeling width of the mask layer and the glass substrate per minute is s2, wherein 4≤s2 / s1≤10.
3. The method for preparing a glass casing according to claim 1, characterized in that: The mask layer is formed on the surface of the glass substrate, comprising: forming a photoresist layer on a surface of a glass substrate; Partially exposing the photoresist layer and developing it to obtain a patterned layer, wherein the softening point Ts of the patterned layer is in the range of 140° C. ≤ Ts ≤ 160° C.; and The patterned layer is hard-baked to obtain a mask layer, wherein the mask layer has a hollow area.
4. The method for preparing a glass casing according to claim 3, characterized in that: The weight average molecular weight of the patterned layer is in the range of 5000≤Mw≤8000.
5. The method for preparing a glass casing according to claim 1, characterized in that: The raw material components of the mask layer include p-cresol and m-cresol, and the molar ratio of the m-cresol to the p-cresol is in a range of 0.9 to 1.
5.
6. The method for preparing a glass casing according to claim 1, characterized in that: The etching solution comprises, by mass fraction: 20% to 30% hydrofluoric acid; 15% to 25% sulfuric acid; 10% to 20% phosphoric acid; 3% to 10% sulfamic acid; and 3% to 5% fluoride salt.
7. The method for preparing a glass casing according to claim 6, characterized in that: The etching solution further comprises, by mass fraction, 0.2% to 0.5% of ferric chloride.
8. The method for preparing a glass casing according to claim 6 or 7, characterized in that: The etching solution further comprises, by mass fraction, 0.2% to 0.5% of sodium dodecylbenzene sulfonate.
9. The method for preparing a glass casing according to claim 1, characterized in that: The step of wet etching the glass substrate in an etching solution comprises: The glass substrate provided with the mask layer is immersed in an etching solution with a temperature of 15° C. to 30° C., and the glass substrate provided with the mask layer is swung to perform wet etching.
10. The method for preparing a glass casing according to claim 9, characterized in that: The swing amplitude of the swinging is in the range of 400 mm to 500 mm; the swing frequency of the swinging is in the range of 30 times / min to 60 times / min.
11. A glass housing, characterized in that: The method is prepared by any one of claims 1 to 10.
12. A glass housing, characterized in that: The glass shell includes a main body and a plurality of protrusions, the main body having a first surface, the plurality of protrusions being arranged on the first surface of the main body, the protrusion having a second surface connected to the first surface, an angle between the first surface and the second surface being greater than 90°, and the protrusion being formed by wet etching of a glass substrate; the roughness Ra of the surface of the glass shell having the protrusion is in the range of 1 μm≤Ra≤3 μm.
13. The glass housing according to claim 12, characterized in that: The minimum width w of the orthographic projection of the protrusion on the first surface is in the range of 50 μm≤w≤80 μm.
14. The glass housing according to claim 12, characterized in that: Along a direction perpendicular to the first surface, a maximum height h of the protrusion is in a range of 9 μm≤h≤13 μm.
15. The glass housing according to claim 12, characterized in that: The range of the minimum distance d between any two adjacent protrusions is 5 μm≤d≤10 μm.
16. The glass housing according to claim 12, characterized in that: The light transmittance T of the glass shell is in the range of 20%≤T≤40%.
17. The glass housing according to claim 12, characterized in that: The haze H of the glass shell is in the range of 60%≤H≤90%.
18. The glass housing according to any one of claims 12 to 17, characterized in that: The protrusion is formed by wet etching of a glass substrate, comprising: forming a mask layer on the glass substrate, the mask layer having a hollow area, performing wet etching to gradually peel the mask layer from an edge portion adjacent to the hollow area toward a direction away from the hollow area and the glass substrate.
19. The glass housing according to claim 18, characterized in that: During the wet etching, the etching depth of the glass substrate per minute is s1, and the peeling width of the mask layer and the glass substrate per minute is s2, wherein 4≤s2 / s1≤10.
20. The glass housing according to claim 12, wherein: The wet etching is performed using an etching solution, and the etching solution includes hydrofluoric acid, sulfuric acid, phosphoric acid, aminosulfonic acid and fluoride salt.
21. An etching solution, characterized in that: The etching solution is used for etching glass, and the etching solution comprises, by mass fraction: 20% to 30% hydrofluoric acid; 15% to 25% sulfuric acid; 10% to 20% phosphoric acid; 3% to 10% sulfamic acid; and 3% to 5% fluoride salt.
22. The etching solution according to claim 21, characterized in that: The etching solution comprises, by mass fraction: 24% to 26% hydrofluoric acid; 18% to 22% sulfuric acid; 13% to 16% phosphoric acid; 5% to 8% sulfamic acid; and 3.5% to 4.5% fluoride salt.
23. The etching solution according to claim 21, characterized in that: The etching solution further comprises, by mass fraction, 0.2% to 0.5% of ferric chloride.
24. The etching solution according to any one of claims 21 to 23, characterized in that: The etching solution further comprises, by mass fraction: 0.2% to 0.5% sodium dodecylbenzene sulfonate.
25. An electronic device, characterized in that: include: Display screen; A glass shell made by the method for making a glass shell according to any one of claims 1 to 10 or a glass shell according to any one of claims 11 to 20, wherein the glass shell is arranged opposite to the display screen; as well as A processor is located between the glass shell and the display screen, and the processor is electrically connected to the display screen to control the display screen to display.