Admixture for inhibiting alkali-silicic acid reaction of aggregate and preparation method thereof
By using a blend of tuff powder, anhydrous lithium bromide, carbon fiber and calcium carbonate, the problem of inhibiting the alkali silicate reaction of aggregates is solved, which significantly reduces the expansion and damage of concrete, improves durability, and realizes the active aggregate effective inhibition.
Patent Information
- Application Number
- CN202411117880.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively inhibit the alkali-silicic acid reaction of aggregates, especially in the absence of inactive aggregates and difficult to control concrete humidity, resulting in cracking and deformation of concrete structures.
Using a blend composed of tuff powder, anhydrous lithium bromide, carbon fiber and calcium carbonate, prepared by drying and stirring, the resulting blend can significantly inhibit the alkali-silicic acid reaction of aggregates, and utilize the active silicon dioxide in tuff powder. The combination of anhydrous lithium bromide and calcium carbonate limits expansion and the formation of stable lithium silicate gels, and carbon fiber increases the support force of the specimen.
It effectively inhibits the alkali-silicic acid reaction of aggregate, reduces the expansion and damage of concrete, significantly improves the durability of concrete, and does not exceed 30% of the cement consumption, significantly inhibiting the hazards of alkali-active reaction of aggregate.
Smart Images

Figure CN118930111A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material performance detection, and in particular relates to an admixture for inhibiting aggregate alkali-silica reaction. The invention also relates to a preparation method of the admixture for inhibiting aggregate alkali-silica reaction. Background Art
[0002] Aggregate alkali-reactive reaction can generally be divided into aggregate alkali-silica reaction and alkali-carbonic acid reaction. It is a chemical reaction that usually occurs in concrete structures such as bridges and dams, and is one of the factors that affect the durability of concrete. Aggregate alkali-reactive reaction is the reaction of active components in aggregate with cement, admixtures, additives and soluble alkali (sodium, potassium) in the composition of concrete to generate silicate gel that can expand. When the silicate gel expands, it causes cracking and deformation of the concrete structure, which has a destructive effect on the concrete.
[0003] At present, scholars at home and abroad have proposed different measures to effectively inhibit the alkali-silica reaction of aggregates, mainly including: 1) using inactive aggregates, 2) limiting the alkali content in cement and concrete, 3) using low-alkalinity chemical admixtures or mixed materials, and 4) controlling humidity. Using inactive aggregates is the most reliable measure to prevent the alkali-silica reaction of aggregates, but inactive aggregates are lacking in many places. When active aggregates are used, limiting the alkali content in concrete and cement may not be enough to effectively inhibit the alkali-silica reaction of aggregates. Studies by Stark et al. in the United States have shown that most concretes contain humidity that causes the alkali-active reaction of aggregates. Structures in desert climates will still be damaged by the alkali-active reaction of aggregates, and the humidity in concrete is difficult to control artificially. Studies have shown that adding fly ash has a certain inhibitory effect on the expansion of aggregate alkali-silica reaction, but fly ash is a waste produced by coal-fired power plants. Closing coal-fired power plants and using cleaner energy will greatly reduce the supply of fly ash, and the heterogeneity of fly ash and the variability of its composition make different fly ashes have different effects on inhibiting the alkali-silica reaction of aggregates. Summary of the invention
[0004] The purpose of the present invention is to provide an admixture for inhibiting the alkali-silica reaction of aggregates, which has the characteristic of being able to significantly inhibit the alkali-silica reaction of aggregates.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned admixture for inhibiting the alkali-silica reaction of aggregate, so as to prepare the admixture for inhibiting the alkali activity of aggregate.
[0006] The technical solution adopted by the present invention is that the admixture for inhibiting the alkali-silica reaction of aggregate is composed of the following components in mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, and the total mass percentage of the above components is 100%.
[0007] The present invention is also characterized in that:
[0008] The fineness of tuff powder is not more than 25%.
[0009] The carbon fiber is chopped into a flat shape, and the width of the carbon fiber is 1mm to 2mm and the length is 3mm to 6mm.
[0010] Another technical solution adopted by the present invention is a method for preparing an admixture for inhibiting the alkali-silica reaction of aggregates, which is specifically implemented according to the following steps:
[0011] Step 1: Weigh the following components by mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, the total mass percentage of the above components being 100%;
[0012] Step 2: Dry the tuff powder taken symmetrically;
[0013] Step 3: Put the dried tuff powder, anhydrous lithium bromide and calcium carbonate into a mixer for the first stirring, and then add carbon fiber for the second stirring to obtain an admixture for inhibiting the alkali-silica reaction of aggregate.
[0014] Another technical solution adopted by the present invention is also characterized in that:
[0015] In step 3, the time for the first stirring and the second stirring are both 5 min to 10 min, and the speeds for the first stirring and the second stirring are both 25 r / min to 35 r / min.
[0016] The specific process of the drying treatment in step 1 is to dry the tuff powder at 105°C ± 5°C for 24 hours, and then naturally cool it to 20°C ~ 25°C.
[0017] The beneficial effects of the present invention are as follows: active silicon dioxide components exist in the tuff powder, which are distributed in various parts of the mortar rod system, dissolving the limited local expansion into an infinite number of active centers, inhibiting the alkali-silicic acid reaction of the aggregate; the Li + Limiting Na + , K + Reacts with silicates in aggregates containing active silicon to form stable lithium silicate gel, which inhibits the alkali activity of aggregates; Ca in calcium carbonate 2+ The presence of increases the activation energy of active silica dissolution, stabilizes the active silica, and effectively limits the expansion of the mortar rod; carbon fiber belongs to stable fiber. Adding fiber to the specimen can fill the specimen, increase the supporting force of the specimen, and reduce the expansion of the specimen during the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a scanning electron microscope photograph of the active aggregate added to the admixture for inhibiting the alkali-silica reaction of the aggregate according to the present invention. DETAILED DESCRIPTION
[0019] The present invention is described in detail below in conjunction with specific implementation modes.
[0020] The first technical solution of the present invention is to provide an admixture for inhibiting the alkali-silica reaction of aggregate, which is composed of the following components in mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, and the total mass percentage of the above components is 100%.
[0021] The fineness of tuff powder is not more than 25%.
[0022] The carbon fiber is in a chopped flat shape, with a width of 1 mm to 2 mm and a length of 3 mm to 6 mm.
[0023] The second technical solution of the present invention is to provide a method for preparing an admixture for inhibiting the alkali-silica reaction of aggregates, which is specifically implemented according to the following steps:
[0024] Step 1: Weigh the following components by mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, the total mass percentage of the above components being 100%;
[0025] Step 2: Dry the tuff powder taken symmetrically;
[0026] Step 3: Put the dried tuff powder, anhydrous lithium bromide and calcium carbonate into a mixer for the first stirring, and then add carbon fiber for the second stirring to obtain an admixture for inhibiting the alkali-silica reaction of aggregate.
[0027] In step 3, the time for the first stirring and the second stirring are both 5 min to 10 min, and the speeds for the first stirring and the second stirring are both 25 r / min to 35 r / min.
[0028] The specific process of the drying treatment in step 1 is to dry the tuff powder at 105°C ± 5°C for 24 hours, and then naturally cool it to 20°C ~ 25°C.
[0029] The selected tuff powder has a fineness (45 μm square hole sieve) of ≤25.0%, a water requirement ratio of ≤115%, a loss on ignition of ≤10.0%, a water content of ≤1.0%, and an activity index of ≥60.0%.
[0030] Table 1 Main chemical composition of cement and tuff powder
[0031] Components <![CDATA[SiO 2 ]]> CaO MgO <![CDATA[Fe 2 THE 3 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[SO 3 ]]> <![CDATA[NaO 2 ]]> <![CDATA[K 2 The]]> P·O 42.5 cement 22.79 57.20 0.77 4.24 6.71 2.74 0.08 0.40 tuff powder 64.18 3.39 1.65 5.24 12.49 0.20 2.51 2.17
[0032] Table 2 Main chemical composition of aggregates
[0033] Components <![CDATA[SiO 2 ]]> CaO MgO <![CDATA[Fe 2 THE 3 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[SO 3 ]]> <![CDATA[NaO 2 ]]> <![CDATA[K 2 The]]> wt / % 61.58 5.98 2.23 7.11 15.86 0.12 3.96 1.99
[0034] The density of tuff powder is 2.73g / cm 3 .
[0035] The active silica particles in the tuff powder are scattered in various parts of the mortar rod system, dissolving the limited local expansion into an infinite number of active centers. Each center participates in the reaction and consumes alkali. The energy can only be dispersed and cannot be concentrated locally, dissolving the energy and inhibiting the alkali-silica reaction of the aggregate. The addition of anhydrous lithium bromide makes Li + Limiting Na + , K + It reacts with silicates in aggregates containing active silicon to form lithium silicate gel, which is less likely to expand. In addition, crystalline lithium silicate forms a barrier on the surface of active silica, which is very effective against Na + , K + It acts as a protective barrier to prevent the formation of alkali silicate gel and effectively inhibit expansion. 2+ The presence of increases the activation energy of active silica dissolution, making it stable and not easily eroded and dissolved, thus effectively limiting the expansion of mortar bars and inhibiting the dissolution rate and amount of silicates. Carbon fibers redistribute the local strain caused by the expansion of aggregate alkali silicate reaction to the entire specimen, helping to reduce the overall expansion of the specimen.
[0036] Figure 1 Scanning electron microscope photo of active aggregate added to the admixture to inhibit the alkali-silica reaction of aggregate.
[0037] The aggregate alkali-silica reaction inhibiting admixture prepared by the above scheme is applied to concrete using alkali-active aggregate, and its admixture amount does not exceed 30% of the cement amount.
[0038] Example 1
[0039] Preparation method of aggregate alkali silicate reaction inhibiting admixture, according to mass percentage weighed the following components: tuff powder 64.1%, anhydrous lithium bromide 15.4%, carbon fiber 5.1%, calcium carbonate 15.4%, the sum of the mass percentages of the above components is 100%; firstly, the weighed tuff powder is dried at 105 ℃ for 24 hours, and naturally cooled to 20 ℃, then the dried tuff powder, anhydrous lithium bromide and calcium carbonate are put into a mixer for the first stirring, the first stirring time is 5 minutes, the first stirring rate is 25r / min, then the carbon fiber is added for the second stirring, the second stirring time is 10 minutes, the second stirring mixing rate is 35r / min, and the aggregate alkali silicate reaction inhibiting admixture A is obtained. The aggregate alkali silicate reaction inhibiting admixture A is added to the active aggregate to carry out the aggregate alkali silicate reaction inhibition experiment, the amount of the aggregate alkali silicate reaction inhibiting admixture A is 30% of the cement mass, and the experimental results are shown in Table 3.
[0040] Example 2
[0041] Preparation method of aggregate alkali silicate reaction inhibiting admixture, according to mass percentage weighed the following components: tuff powder 69.7%, anhydrous lithium bromide 9.1%, carbon fiber 6.1%, calcium carbonate 15.1%, the sum of the mass percentages of the above components is 100%; firstly, the weighed tuff powder is dried at 100 ℃ for 24h, and naturally cooled to 25 ℃, then the dried tuff powder, anhydrous lithium bromide and calcium carbonate are put into a mixer for the first stirring, the first stirring and mixing time is 7min, the first stirring rate is 30r / min, then the carbon fiber is added for the second stirring, the second stirring time is 9min, the second stirring rate is 32r / min, and the aggregate alkali silicate reaction inhibiting admixture B is obtained, the aggregate alkali silicate reaction inhibiting admixture B is added to the active aggregate to carry out the aggregate alkali silicate reaction inhibition experiment, the amount of the aggregate alkali silicate reaction inhibiting admixture B is 30% of the cement mass, the experimental results are shown in Table 3.
[0042] Example 3
[0043] Preparation method of aggregate alkali silicate reaction inhibiting admixture, according to mass percentage weighed the following components: tuff powder 76.9%, anhydrous lithium bromide 11.5%, carbon fiber 3.8%, calcium carbonate 7.8%, the sum of the mass percentages of the above components is 100%; firstly, the weighed tuff powder is dried at 105 ℃ for 24 hours, and naturally cooled to 23 ℃, then the dried tuff powder, anhydrous lithium bromide and calcium carbonate are put into a mixer for the first stirring, the first stirring time is 10 minutes, the first stirring mixing rate is 25r / min, then the carbon fiber is added for the second stirring, the second stirring time is 8 minutes, the second stirring rate is 33r / min, the aggregate alkali silicate reaction inhibiting admixture C can be obtained, the aggregate alkali silicate reaction inhibiting admixture C is added to the active aggregate to carry out the aggregate alkali silicate reaction inhibition experiment, the amount of the aggregate alkali silicate reaction inhibiting admixture C is 30% of the cement mass, the experimental results are shown in Table 3.
[0044] Example 4
[0045] Preparation method of aggregate alkali silicate reaction inhibiting admixture, according to mass percentage weighed the following components: tuff powder 65.6%, anhydrous lithium bromide 15.6%, carbon fiber 4.7%, calcium carbonate 14.1%, the sum of the mass percentages of the above components is 100%; firstly, the weighed tuff powder is dried at 110 ° C for 24 hours, and naturally cooled to 21 ° C, then the dried tuff powder, anhydrous lithium bromide and calcium carbonate are put into a mixer for the first stirring, the first stirring time is 8 minutes, the first stirring rate is 35r / min, then the carbon fiber is added for the second stirring, the second stirring time is 5 minutes, the second stirring rate is 25r / min, the aggregate alkali silicate reaction inhibiting admixture D can be obtained, the aggregate alkali silicate reaction inhibiting admixture D is added to the active aggregate to carry out the aggregate alkali silicate reaction inhibition experiment, the amount of the aggregate alkali silicate reaction inhibiting admixture D is 30% of the cement mass, the experimental results are shown in Table 3.
[0046] The alkali-aggregate reaction test method refers to DL / T5151-2014 "Test Procedure for Hydraulic Concrete Sand and Stone Aggregates" Aggregate Alkali Reactivity Test-Mortar Bar Quick Method (AMBT). The specific parameters of sample molding are: sample size is 25.4mm×25.4mm×285mm, three samples are in a group, the mass ratio of cement to sand is 1:2.25, and the water-cement ratio of mortar is 0.47. The crushed and sieved aggregates are washed and dried, and the materials used are placed in a constant temperature chamber at 20℃ 24h before molding. Use a nail-embedded test mold with stainless metal at both ends to shape the weighed material. The sample is cured in a curing box at a temperature of 20°C and a relative humidity of more than 95% for 24 hours before demoulding. The demoulded sample is completely immersed in a sealed box filled with tap water for curing. The sealed box is placed in a constant temperature water bath at a temperature of 80°C for 24 hours, and then the sample is placed in a curing cylinder filled with 1mol / L NaOH solution, and then the curing cylinder is placed in a constant temperature water bath at a temperature of 80°C. If the 14d expansion rate is less than 0.10%, it is an inactive aggregate; if the 14d expansion rate is greater than 0.20%, it is an active aggregate with potential harmful reactions; if the 14d expansion rate is between 0.10 and 0.20%, the test observation time is extended to 28d; the specific test steps are as follows:
[0047] The experimental process is as follows:
[0048] Specimen preparation: 24 hours before molding, the raw materials used in the test were placed in a constant temperature room with a temperature of 20°C and a relative humidity greater than 50%;
[0049] The specimens are cured at a temperature of 20°C and a relative humidity of more than 95%. After 24 hours of curing, they are demoulded and the initial length of the specimens is immediately measured in a standard curing room as a reference value for measuring the reference length.
[0050] After the measurement is completed, the specimen is completely immersed in a sealed curing tube filled with tap water, and the curing tube is placed in a constant temperature water bath at 80°C for 24 hours, and then the length of the specimen is measured as the reference length. The test time should be completed within 15 seconds;
[0051] The specimen is placed in a curing cylinder containing 1 mol / L NaOH solution. The specimen should be completely immersed in the solution. Cover the curing cylinder lid to make it airtight, and then place the curing barrel in a constant temperature water bath at 80°C.
[0052] The test ages of the specimens are 3d, 7d, 14d and 28d respectively.
[0053] Test results and analysis:
[0054] Table 3 Experimental results of inhibiting the alkali activity of aggregate alkali-silica reaction admixtures
[0055]
[0056] Comparing Examples 1 to 4 with the reference example, the results of the aggregate alkali-silica reaction inhibition test were analyzed. From Table 3, it can be seen that the reference example is the active aggregate performance measured without adding any admixtures. The expansion rate of the aggregate changes with time, and the expansion rate reaches 0.297% at 28 days.
[0057] When 30% of the composite admixture is added to the concrete mortar, the expansion rate of the aggregate of the test piece at 28 days is less than 0.1%. When the expansion rate of the aggregate is less than 0.1%, it is proved that the composite admixture has a significant effect on the alkali-silica reaction of the aggregate at this dosage. The inhibition effect of Examples 1 to 4 is significant compared with the benchmark example. When the composite materials of Examples 1 to 4 are added to the aggregate, the alkali-silica reaction of the aggregate can be effectively inhibited.
Claims
1. An admixture for inhibiting alkali-silica reaction of aggregate, characterized in that: The invention is composed of the following components in terms of mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, and the total mass percentage of the above components is 100%.
2. The aggregate alkali-silica reaction inhibiting admixture according to claim 1, characterized in that: The fineness of the tuff powder is not more than 25%.
3. The aggregate alkali-silica reaction inhibiting admixture according to claim 1, characterized in that: The carbon fibers are in a chopped flat shape, and have a width of 1 mm to 2 mm and a length of 3 mm to 6 mm.
4. A method for preparing an admixture for inhibiting aggregate alkali-silica reaction, characterized in that: Follow the steps below to implement it: Step 1: Weigh the following components by mass percentage: 64.1% to 76.9% of tuff powder, 9.1% to 15.6% of anhydrous lithium bromide, 3.8% to 6.1% of carbon fiber, and 7.8% to 15.4% of calcium carbonate, the total mass percentage of the above components being 100%; Step 2: Dry the tuff powder taken symmetrically; Step 3: Put the dried tuff powder, anhydrous lithium bromide and calcium carbonate into a mixer for the first stirring, and then add carbon fiber for the second stirring to obtain an admixture for inhibiting the alkali-silica reaction of aggregate.
5. The method for preparing an aggregate alkali-silica reaction inhibiting admixture according to claim 4, characterized in that: The specific process of the drying treatment in step 1 is to dry the tuff powder at 105°C ± 5°C for 24 hours, and then naturally cool it to 20°C ~ 25°C.
6. The method for preparing an aggregate alkali-silica reaction inhibiting admixture according to claim 4, characterized in that: The time of the first stirring and the second stirring in step 3 are both 5 min to 10 min, and the speed of the first stirring and the second stirring are both 25 r / min to 35 r / min.