Preparation method and application of high-strength fiber composite material
By introducing highly conjugated benzooxazole and phosphorus nitrogen elements into the polyester fiber, high-strength flame retardant polyester copolymer is prepared, which solves the problem of insufficient flame retardant properties and strength of polyester fibers, and achieves high strength and good resistance Fibre composite material with flameability and heat resistance.
Patent Information
- Application Number
- CN202411229326.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polyester fiber has poor flame retardant performance and is easy to decompose at high temperatures, which cannot meet the fire resistance needs. At the same time, its strength is insufficient, which affects the application effect.
By introducing highly conjugated benzoxazole into the polyester and combining it with phosphorus and nitrogen elements, a high-strength flame retardant polyester copolymer is prepared. Through esterification reaction and melt spinning technology, high-strength and good flame retardant properties are formed. Fiber composite material.
The flame retardant properties and strength of fiber composite materials are improved, the flame retardant elements are not easy to migrate, have good durability, and the thermal stability and mechanical properties of the fiber are significantly improved.
Smart Images

Figure BDA0005025615010000031 
Figure BDA0005025615010000032 
Figure BDA0005025615010000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber materials, and in particular to a preparation method of a high-strength fiber composite material and application thereof. Background Art
[0002] Polyester fiber, also known as terylene, is a synthetic fiber obtained by spinning polyester formed by the condensation of organic dibasic acids and diols. It is currently the largest variety of synthetic fibers and is widely used in interior decoration, transportation, sportswear, personal protection, etc. Polyester fiber has many excellent properties, such as large fiber fineness, easy dispersion, moderate resilience, excellent heat setting, etc., and is widely used in clothing fabrics. However, when the tension is too large, the polyester fiber can be easily broken due to its poor strength, thus affecting the practicality of the polyester fiber. At the same time, the large molecular straight chain of polyester fiber is easily decomposed at high temperature to produce flammable molten products, which cannot meet the fire protection needs in daily life. Therefore, the modification of polyester fiber has also received more and more attention from researchers.
[0003] When polyester fiber is used in rubber reinforcing materials such as tires and cords, the strength of the polyester fiber is required to be as high as possible to meet the needs of the application. In the prior art, the high strength of polyester fiber is improved by adjusting the spinning process parameters and increasing the stretching multiple, but the disadvantage of this method is that the improvement of fiber strength is very limited. There is also a method of increasing the molecular weight of polyester, but polyester is prepared by polycondensation reaction. For polycondensation, to increase the molecular weight of the product, extremely harsh polymerization process conditions need to be adopted, such as strict water removal in the system, process The process repeatability is poor; for the flame retardant modification of polyester fibers, invention patent CN110923841B discloses flame retardant polyester fibers and a preparation method thereof, in which polyester, melamine cyanurate, graphite-like carbon nitride, zinc compounds and DOPO derivatives are melt-blended to obtain flame retardant polyester slices, which are then melt-spun and drawn to obtain flame retardant polyester fibers. However, the small molecule flame retardant in this technology has poor thermal stability and is easily migrated and precipitated after being blended with polyester, resulting in poor flame retardancy. In addition, the blended flame retardant will also affect the spinnability of polyester, and the fibers are easily broken and floating during spinning.
[0004] The invention introduces highly conjugated benzoxazole into polyester to improve the order of polyester molecular chains and enhance the breaking strength of polyester fibers; at the same time, phosphorus and nitrogen elements are introduced into the polyester molecular chains to produce a synergistic flame retardant effect; a polyester copolymer is obtained by catalytic polycondensation of the prepared functional monomer and terephthalic acid, and then melt-spinning is performed to obtain a high-strength fiber composite material, thereby avoiding the problem of migration and precipitation of flame retardant elements, and having good spinnability, good flame retardancy and high strength. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a high-strength fiber composite material and its application, which solves the problem of poor flame retardant performance of existing polyester fibers and further improves the strength of the fiber composite material.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a high-strength fiber composite material comprises the following steps:
[0008] (1) Under nitrogen atmosphere, terephthalic acid and a structural formula of The diphenol-based benzoxazole phosphorus nitrogen flame retardant intermediate is stirred evenly, and a catalyst, dihydrogen trioxide, and a heat stabilizer, triphenyl phosphate, are added. The esterification reaction is carried out at 220-260°C, and the top temperature of the fractionation column is controlled to be 120-140°C. When the amount of esterified water received is 80-90% of the theoretical value, vacuum is drawn to carry out a condensation reaction, and the vacuum degree in the kettle is reduced to 0.2-0.3kPa. Nitrogen is used to break the vacuum and discharge the material to obtain a high-strength flame retardant polyester copolymer.
[0009] (2) 100 parts by weight of vacuum-dried PET polyester chips and 5-25 parts of high-strength flame-retardant polyester copolymer are added to a high-speed disperser and mixed evenly, and then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 600-800 m / min and a spinning machine temperature of 260-280°C. After the primary fibers are balanced for 8-12 hours, they are stretched and wound on a parallel drawing machine to obtain a high-strength fiber composite material.
[0010] Furthermore, in step (1), by weight, terephthalic acid is 100 parts, diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate is 360-390 parts, antimony trioxide is 0.05-0.1 parts, and triphenyl phosphate is 0.03-0.06 parts.
[0011] Furthermore, in step (1), the polycondensation reaction temperature is 250-280° C., and the polycondensation reaction time is 24-48 hours.
[0012] Furthermore, in step (2), the drawing speed is 400-500 m / min, and the drawing multiple is 5-7.
[0013] Furthermore, the preparation method of the diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate in step (1) comprises the following steps:
[0014] Step S1, add 2-amino-4-methoxyphenol, p-aminobenzoic acid and polyphosphoric acid to a reaction flask equipped with a reflux condenser, stir to react, cool to room temperature after the reaction, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline. The preparation reaction formula is as follows:
[0015]
[0016] Step S2: Add phenyl dichloride phosphate and acetonitrile to a reaction flask under a nitrogen atmosphere, stir evenly, add triethylamine and 4-methoxybenzoxazolylaniline, stir to react, filter after the reaction, wash with ethanol, and dry to obtain a dimethoxybenzoxazolyl phosphorus nitrogen flame retardant intermediate. The preparation reaction formula is as follows:
[0017]
[0018] Step S3, under a nitrogen atmosphere, add 100 parts by weight of dimethoxybenzoxazole phosphine nitrogen flame retardant intermediate and dichloromethane to the reaction flask, stir evenly, cool to -78 ° C, drop 90-110 parts of boron tribromide, stir to react, after the reaction is completed, cool to 0 ° C, pour into deionized water, add ethyl acetate to extract, concentrate the organic phase, and dry to obtain a diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate. The preparation reaction formula is as follows:
[0019]
[0020] Furthermore, in step S1, by weight, 2-amino-4-methoxyphenol is 100 parts, p-aminobenzoic acid is 120-150 parts, and polyphosphoric acid is 1000-1500 parts.
[0021] Furthermore, in step S1, the reaction temperature is 170-190° C., and the reaction time is 8-16 h.
[0022] Furthermore, in step S2, by weight, phenyl dichloride phosphate is 100 parts, triethylamine is 110-130 parts, and 4-methoxybenzoxazolyl aniline is 230-255 parts.
[0023] Furthermore, in step S2, the reaction temperature is 60-80° C., and the reaction time is 5-10 h.
[0024] Furthermore, in step S3, the reaction temperature is 20-35° C., and the reaction time is 16-24 h.
[0025] By adopting the above technical solution, the beneficial effects of the present invention are:
[0026] The invention firstly reacts 2-amino-4-methoxyphenol with p-aminobenzoic acid under the action of polyphosphoric acid to obtain 4-methoxybenzoxazolyl aniline, which is then reacted with phenyl dichlorophosphate to obtain a dimethoxybenzoxazolyl phosphine nitrogen flame retardant intermediate, and then under the action of boron tribromide, the methoxy group is removed to obtain a diphenol-based benzoxazolyl phosphine nitrogen flame retardant intermediate, which is then subjected to an esterification polycondensation reaction with terephthalic acid to obtain a high-strength flame retardant polyester copolymer, and finally the high-strength fiber composite material is obtained after being blended with PET polyester chips and melt-spun.
[0027] The high-strength flame-retardant polyester copolymer contains phosphorus and nitrogen synergistic flame-retardant elements. During the combustion process, phosphoric acid and metaphosphoric acid compounds produced by the phosphorus element catalyze into carbon to form a solid phase covering layer; the nitrogen element generates non-flammable nitrogen oxides during thermal decomposition, which dilutes the oxygen concentration and takes away the combustion heat. At the same time, it can produce an obvious carbon layer to inhibit the transmission of oxygen and heat; in addition, the hydroxyl group of the high-strength flame-retardant polyester copolymer and the carboxyl group of terephthalic acid produce condensation, so that the flame retardant elements are embedded in the polyester molecular chain, which is not easy to migrate and precipitate, and the flame retardant durability is improved.
[0028] The high-strength flame-retardant polyester copolymer contains a planar rigid heterocyclic structure of dibenzoxazole, which has high regularity and orientation, thereby improving the rigidity of the polyester fiber, and the hydrogen bonding of the heterocyclic ring can effectively improve the mechanical properties of the polyester fiber; at the same time, oxazole has a highly conjugated rigid planar structure and a high charge density, which can effectively improve the order of the molecular chains in the system, regulate the aggregation structure of the polyester fiber, slow down the coagulation rate during the fiber forming process, avoid the formation of a porous structure, reduce the pores inside the fiber, and is conducive to the formation of denser primary fibers and orderly stacking of macromolecular chains, thereby improving the crystallinity and crystal orientation of the polyester fiber, and thus improving the mechanical properties of the polyester fiber.
[0029] The structure of high-strength flame-retardant polyester copolymer is a rigid planar structure, which improves the rigidity of the macromolecular chain and has high thermal stability, thereby increasing the activation energy of chain segment movement. On the other hand, high-strength flame-retardant polyester copolymer improves the crystallinity of the fiber by improving the orderly stacking of the molecular chains, restricts the movement of the amorphous chain segments, and at the same time, the thermal decomposition activation energy of the benzoxazole structure is high, which significantly improves the heat resistance of the polyester fiber composite material. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.
[0031] Example 1
[0032] (1) Add 12 g of 2-amino-4-methoxyphenol, 16.2 g of p-aminobenzoic acid and 160 g of polyphosphoric acid to a reaction flask equipped with a reflux condenser, react at 180° C. for 12 h, cool to room temperature, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline.
[0033] (2) Under nitrogen atmosphere, 25 g of phenyl dichlorophosphate and 300 mL of acetonitrile were added to a reaction flask, and after stirring, 30 g of triethylamine and 60 g of 4-methoxybenzoxazolylaniline were added, and the mixture was reacted at 70° C. for 8 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazolylphosphine flame retardant intermediate.
[0034] (3) Under a nitrogen atmosphere, 18 g of dimethoxybenzoxazole phosphonium nitrogen flame retardant intermediate and 450 mL of dichloromethane were added to a reaction flask, stirred evenly, cooled to -78 ° C, 18.9 g of boron tribromide was added dropwise, reacted at 25 ° C for 20 h, cooled to 0 ° C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a diphenol-based benzoxazole phosphonium nitrogen flame retardant intermediate.
[0035] (4) Under nitrogen atmosphere, 100 g of terephthalic acid and 380 g of diphenolylbenzoxazole phosphine nitrogen flame retardant intermediate were added to a stainless steel reactor, the mixture was stirred evenly, 0.06 g of catalyst tritium trioxide and 0.5 g of thermal stabilizer triphenyl phosphate were added, and the esterification reaction was carried out at 240° C. The top temperature of the fractionation column was controlled at 130° C. When the amount of esterification water received was 85% of the theoretical value, polycondensation was carried out at 260° C. for 36 h, the vacuum degree in the reactor was reduced to 0.25 kPa, and the vacuum was broken by nitrogen to obtain a high-strength flame retardant polyester copolymer.
[0036] (5) 100 g of vacuum-dried PET polyester chips and 5 g of high-strength flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 700 m / min and a spinning machine temperature of 265 °C. After the primary fibers were balanced for 10 h, they were stretched on a parallel stretching machine at a stretching speed of 450 m / min and a stretching multiple of 5.5. The fibers were then wound to obtain a high-strength fiber composite material.
[0037] Example 2
[0038] (1) Add 25 g of 2-amino-4-methoxyphenol, 30 g of p-aminobenzoic acid and 250 g of polyphosphoric acid to a reaction flask equipped with a reflux condenser, react at 190° C. for 8 h, cool to room temperature, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline.
[0039] (2) Under a nitrogen atmosphere, 40 g of phenyl dichlorophosphate and 400 mL of acetonitrile were added to a reaction flask, and after stirring, 44 g of triethylamine and 92 g of 4-methoxybenzoxazolylaniline were added, and the mixture was reacted at 80° C. for 5 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazolylphosphine flame retardant intermediate.
[0040] (3) Under a nitrogen atmosphere, 32 g of dimethoxybenzoxazole phosphonium nitrogen flame retardant intermediate and 960 mL of dichloromethane were added to a reaction flask, stirred evenly, cooled to -78 ° C, 28.8 g of boron tribromide was added dropwise, reacted at 35 ° C for 16 h, cooled to 0 ° C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a diphenol-based benzoxazole phosphonium nitrogen flame retardant intermediate.
[0041] (4) Under nitrogen atmosphere, 100 g of terephthalic acid and 360 g of diphenolylbenzoxazole phosphonium nitrogen flame retardant intermediate were added to a stainless steel reactor, the mixture was stirred evenly, 0.05 g of catalyst tritium trioxide and 0.03 g of thermal stabilizer triphenyl phosphate were added, and the esterification reaction was carried out at 260° C. The top temperature of the distillation column was controlled at 140° C. When the amount of esterification water received was 80% of the theoretical value, polycondensation was carried out at 280° C. for 24 h, the vacuum degree in the reactor was reduced to 0.3 kPa, and the vacuum was broken by nitrogen to obtain a high-strength flame retardant polyester copolymer.
[0042] (5) 100 g of vacuum-dried PET polyester chips and 10 g of high-strength flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 800 m / min and a spinning machine temperature of 280 °C. After the primary fibers were balanced for 8 h, they were stretched on a parallel stretching machine at a stretching speed of 500 m / min and a stretching multiple of 7. The fibers were then wound to obtain a high-strength fiber composite material.
[0043] Example 3
[0044] (1) Add 15 g of 2-amino-4-methoxyphenol, 22.5 g of p-aminobenzoic acid and 225 g of polyphosphoric acid to a reaction flask equipped with a reflux condenser, react at 170° C. for 16 h, cool to room temperature, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline.
[0045] (2) Under nitrogen atmosphere, 8 g of phenyl dichlorophosphate and 120 mL of acetonitrile were added to a reaction flask, and after stirring, 10.4 g of triethylamine and 20.4 g of 4-methoxybenzoxazolylaniline were added, and the mixture was reacted at 60 ° C for 10 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazolyl phosphine nitrogen flame retardant intermediate.
[0046] (3) Under a nitrogen atmosphere, 5 g of dimethoxybenzoxazole phosphonium nitrogen flame retardant intermediate and 150 mL of dichloromethane were added to a reaction flask, stirred evenly, cooled to -78°C, 5.5 g of boron tribromide was added dropwise, reacted at 20°C for 24 h, cooled to 0°C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a diphenol-based benzoxazole phosphonium nitrogen flame retardant intermediate.
[0047] (4) Under nitrogen atmosphere, 100 g of terephthalic acid and 390 g of diphenolylbenzoxazole phosphonium nitrogen flame retardant intermediate were added to a stainless steel reactor, the mixture was stirred evenly, 0.1 g of catalyst tritium trioxide and 0.06 g of thermal stabilizer triphenyl phosphate were added, and the esterification reaction was carried out at 220° C. The top temperature of the fractionation column was controlled at 120° C. When the amount of esterification water received was 90% of the theoretical value, polycondensation was carried out at 250° C. for 48 h, the vacuum degree in the reactor was reduced to 0.2 kPa, and the vacuum was broken by nitrogen to obtain a high-strength flame retardant polyester copolymer.
[0048] (5) 100 g of vacuum-dried PET polyester chips and 15 g of high-strength flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 600 m / min and a spinning machine temperature of 260 °C. After the primary fibers were balanced for 12 h, they were stretched on a parallel stretching machine at a stretching speed of 400 m / min and a stretching multiple of 5. The fibers were then wound to obtain a high-strength fiber composite material.
[0049] Example 4
[0050] (1) Add 35 g of 2-amino-4-methoxyphenol, 43.4 g of p-aminobenzoic acid and 420 g of polyphosphoric acid to a reaction flask equipped with a reflux condenser, react at 185° C. for 15 h, cool to room temperature, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline.
[0051] (2) Under nitrogen atmosphere, 28 g of phenyl dichlorophosphate and 320 mL of acetonitrile were added to a reaction flask, and after stirring, 32.2 g of triethylamine and 68.6 g of 4-methoxybenzoxazolylaniline were added, and the mixture was reacted at 75 ° C. for 8 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazolylphosphine flame retardant intermediate.
[0052] (3) Under a nitrogen atmosphere, 15 g of dimethoxybenzoxazole phosphonium nitrogen flame retardant intermediate and 390 mL of dichloromethane were added to a reaction flask, stirred evenly, cooled to -78 ° C, 15.9 g of boron tribromide was added dropwise, reacted at 30 ° C for 24 h, cooled to 0 ° C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a diphenol-based benzoxazole phosphonium nitrogen flame retardant intermediate.
[0053] (4) Under nitrogen atmosphere, 100 g of terephthalic acid and 375 g of diphenolylbenzoxazole phosphonium nitrogen flame retardant intermediate were added to a stainless steel reactor, the mixture was stirred evenly, 0.08 g of catalyst tritium trioxide and 0.06 g of thermal stabilizer triphenyl phosphate were added, and the esterification reaction was carried out at 245° C. The top temperature of the distillation column was controlled at 130° C. When the amount of esterification water received was 90% of the theoretical value, polycondensation was carried out at 265° C. for 24 h, the vacuum degree in the reactor was reduced to 0.3 kPa, and the vacuum was broken by nitrogen to obtain a high-strength flame retardant polyester copolymer.
[0054] (5) 100 g of vacuum-dried PET polyester chips and 20 g of high-strength flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 750 m / min and a spinning machine temperature of 270 °C. After the primary fibers were balanced for 10 h, they were stretched on a parallel stretching machine at a stretching speed of 460 m / min and a stretching multiple of 6. The fibers were then wound to obtain a high-strength fiber composite material.
[0055] Example 5
[0056] (1) Add 10 g of 2-amino-4-methoxyphenol, 13 g of p-aminobenzoic acid and 125 g of polyphosphoric acid to a reaction flask equipped with a reflux condenser, react at 185° C. for 16 h, cool to room temperature, pour into an ice water bath with stirring, add saturated sodium bicarbonate to neutralize, filter, wash the filter cake with deionized water, and dry to obtain 4-methoxybenzoxazolylaniline.
[0057] (2) Under nitrogen atmosphere, 6 g of phenyl dichlorophosphate and 80 mL of acetonitrile were added to a reaction flask, and after stirring, 7.5 g of triethylamine and 14.7 g of 4-methoxybenzoxazolylaniline were added, and the mixture was reacted at 75 ° C. for 9 h, filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazolyl phosphine nitrogen flame retardant intermediate.
[0058] (3) Under a nitrogen atmosphere, 3 g of dimethoxybenzoxazole phosphine nitrogen flame retardant intermediate and 75 mL of dichloromethane were added to a reaction flask, stirred evenly, cooled to -78°C, 3 g of boron tribromide was added dropwise, reacted at 20°C for 20 h, cooled to 0°C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate.
[0059] (4) Under nitrogen atmosphere, 100 g of terephthalic acid and 365 g of diphenolylbenzoxazole phosphine nitrogen flame retardant intermediate were added to a stainless steel reactor, the mixture was stirred evenly, 0.1 g of catalyst tritium trioxide and 0.05 g of thermal stabilizer triphenyl phosphate were added, and the esterification reaction was carried out at 255° C. The top temperature of the fractionation column was controlled at 135° C. When the amount of esterification water received was 90% of the theoretical value, polycondensation was carried out at 260° C. for 36 h, the vacuum degree in the reactor was reduced to 0.25 kPa, and the vacuum was broken by nitrogen to obtain a high-strength flame retardant polyester copolymer.
[0060] (5) 100 g of vacuum-dried PET polyester chips and 25 g of high-strength flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 720 m / min and a spinning machine temperature of 270 °C. After the primary fibers were balanced for 12 h, they were stretched on a parallel stretching machine at a stretching speed of 500 m / min and a stretching multiple of 6.5. The fibers were then wound to obtain a high-strength fiber composite material.
[0061] Comparative Example 1
[0062] (1) Under a nitrogen atmosphere, 25 g of phenyl dichlorophosphate and 300 mL of acetonitrile were added to a reaction flask, and after stirring, 30 g of triethylamine and 60 g of 4-methoxyaniline (CAS No. 104-94-9) were added, and the mixture was reacted at 70° C. for 8 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxyphosphorus nitrogen flame retardant intermediate.
[0063] (2) Under nitrogen atmosphere, 18 g of dimethoxyphosphorus nitrogen flame retardant intermediate and 450 mL of dichloromethane were added to the reaction flask, stirred evenly, cooled to -78 ° C, 18.9 g of boron tribromide was added dropwise, reacted at 25 ° C for 20 h, cooled to 0 ° C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a structure of Diphenol-based phosphorus-nitrogen flame retardant intermediate.
[0064] (3) Under nitrogen atmosphere, 100 g of terephthalic acid and 380 g of diphenol-based phosphorus nitrogen flame retardant intermediate were added to a stainless steel reactor, and the mixture was stirred evenly. 0.06 g of catalyst tritium trioxide and 0.5 g of thermal stabilizer triphenyl phosphate were added, and an esterification reaction was carried out at 240° C. The top temperature of the distillation column was controlled at 130° C. When the amount of esterified water received was 85% of the theoretical value, polycondensation was carried out at 260° C. for 36 h, the vacuum degree in the reactor was reduced to 0.25 kPa, and nitrogen was used to break the vacuum and discharge the material to obtain a flame retardant polyester copolymer.
[0065] (4) 100 g of vacuum-dried PET polyester chips and 5 g of flame-retardant polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 700 m / min and a spinning machine temperature of 265°C. After the nascent fibers were balanced for 10 h, they were stretched on a parallel stretching machine at a stretching speed of 450 m / min and a stretching multiple of 5.5. The fibers were then wound to obtain a fiber composite material.
[0066] Comparative Example 2
[0067] (1) Under a nitrogen atmosphere, 25 g of 1,4-dichlorobenzene (CAS No. 106-46-7) and 300 mL of acetonitrile were added to a reaction flask, and after stirring, 30 g of triethylamine and 60 g of 4-methoxybenzoxazolylaniline (prepared in Example 1) were added, and the mixture was reacted at 70° C. for 8 h. The mixture was filtered, washed with ethanol, and dried to obtain a dimethoxybenzoxazole intermediate.
[0068] (2) Under nitrogen atmosphere, 18 g of dimethoxybenzoxazole intermediate and 450 mL of dichloromethane were added to the reaction flask, stirred evenly, cooled to -78°C, 18.9 g of boron tribromide was added dropwise, reacted at 25°C for 20 h, cooled to 0°C, poured into deionized water, extracted with ethyl acetate, concentrated the organic phase, and dried to obtain a structure of
[0069] Diphenolylbenzoxazole intermediate.
[0070] (3) Under nitrogen atmosphere, 100 g of terephthalic acid and 380 g of diphenolylbenzoxazole intermediate were added to a stainless steel reactor, stirred evenly, 0.06 g of catalyst tritium trioxide and 0.5 g of thermal stabilizer triphenyl phosphate were added, and esterification reaction was carried out at 240° C. The top temperature of the fractionation column was controlled at 130° C. When the amount of esterification water received was 85% of the theoretical value, polycondensation was carried out at 260° C. for 36 h, the vacuum degree in the reactor was reduced to 0.25 kPa, and nitrogen was used to break the vacuum and discharge the material to obtain a high-strength polyester copolymer.
[0071] (4) 100 g of vacuum-dried PET polyester chips and 5 g of high-strength polyester copolymer were added to a high-speed disperser and mixed evenly. The mixture was then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 700 m / min and a spinning machine temperature of 265°C. After the primary fibers were balanced for 10 h, they were stretched on a parallel stretching machine at a stretching speed of 450 m / min and a stretching multiple of 5.5. The fibers were then wound to obtain a fiber composite material.
[0072] Comparative Example 3
[0073] 100g of vacuum-dried PET polyester chips were placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 700m / min and a spinning machine temperature of 265°C. After the primary fibers were balanced for 10 hours, they were stretched on a parallel stretching machine at a stretching speed of 450m / min and a stretching multiple of 5.5, and then wound to obtain a fiber material.
[0074] Limiting oxygen index (LOI): The limiting oxygen index of fabric is measured according to GB / T 5454-1997 "Textile combustion performance test oxygen index method".
[0075] Vertical burning performance test: The vertical burning performance of the fabric is measured according to GB / T 5455-1997 "Vertical method for testing burning performance of textiles".
[0076] Table 1 Flame retardant performance test
[0077]
[0078] It can be seen from the test results in the above table that with the increase in the amount of high-strength flame-retardant polyester copolymer, the limiting oxygen index in Example 5 reaches 31.2%, and the vertical combustion grade is V-0, which belongs to a flame-retardant material, and the flame retardant performance has been greatly improved. This is because the high-strength flame-retardant polyester copolymer contains phosphorus and nitrogen synergistic flame retardant elements. During the combustion process, phosphoric acid and metaphosphoric acid compounds produced by the phosphorus element are catalyzed into carbon to form a solid phase covering layer; nitrogen elements generate non-flammable nitrogen oxides during thermal decomposition, which dilute the oxygen concentration and take away the combustion heat. At the same time, an obvious carbon layer can be produced to inhibit the transmission of oxygen and heat; in addition, the hydroxyl group of the high-strength flame-retardant polyester copolymer and the carboxyl group of terephthalic acid produce condensation, so that the flame retardant element is embedded in the polyester molecular chain, which is not easy to migrate and precipitate, and the flame retardant durability is improved.
[0079] Comparative Example 1 contains phosphorus and nitrogen flame retardant elements, and its flame retardant performance is good, with a limiting oxygen index of 25.2%; Comparative Example 2 does not contain phosphorus elements, and no phosphorus and nitrogen synergistic flame retardant system is formed, the vertical combustion grade is V-2, and the flame retardant performance is poor; Comparative Example 3 is pure polyester fiber, and its limiting oxygen index is only 20.8, which is a flammable material and has no flame retardant effect.
[0080] Mechanical properties test: The fiber strength was tested using an electronic single yarn strength tester with a clamping length of 500 mm and a tensile rate of 500 mm / min.
[0081] Table 2 Mechanical properties test
[0082] Breaking strength (cN / dtex) Initial modulus (cN / dtex) Example 1 2.12 6.25 Example 2 2.37 6.58 Example 3 2.45 7.21 Example 4 2.66 7.64 Example 5 2.53 7.72 Comparative Example 1 1.35 5.01 Comparative Example 2 2.05 6.23 Comparative Example 3 1.24 4.82
[0083] It can be seen from the test results in the above table that with the increase in the amount of high-strength flame-retardant polyester copolymer, the breaking strength and initial modulus of the prepared fiber composite material gradually increase. The breaking strength of Example 4 is 2.66 cN / dtex, the initial modulus is 7.64 cN / dtex, and the mechanical properties are relatively excellent. This is because the high-strength flame-retardant polyester copolymer structure contains a planar rigid heterocyclic structure of dibenzoxazole, which has high regularity and orientation, so that the rigidity of the polyester fiber is improved, and the hydrogen bonding effect of the heterocyclic ring can effectively improve the mechanical properties of the polyester fiber; at the same time, oxazole has a highly conjugated rigid planar structure and a high charge density, which can effectively improve the order of the molecular chain in the system, regulate the aggregated structure of the polyester fiber, slow down the coagulation rate in the fiber forming process, avoid the formation of a porous structure, reduce the pores inside the fiber, and is conducive to the formation of a denser primary fiber, which is conducive to the orderly stacking of macromolecular chains, improves the crystallinity and crystal orientation of the polyester fiber, and thus improves the mechanical properties of the polyester fiber.
[0084] Thermal performance test: Pyrolysis was performed using a thermal analyzer, nitrogen was introduced as a protective gas, and the temperature was increased from 25°C to 600°C at a heating rate of 10°C / min.
[0085] Table 3 Thermal performance test
[0086]
[0087] It can be seen from the test results in the above table that with the increase in the amount of high-strength flame-retardant polyester copolymer, the heat resistance of the prepared fiber composite material is improved. The initial thermal decomposition temperature in Example 4 is 425.5°C, which is 30.3°C higher than the pure polyester fiber in Comparative Example 3. This is because, on the one hand, the structure of the high-strength flame-retardant polyester copolymer is a rigid planar structure with high thermal stability, which improves the rigidity of the macromolecular chain and increases the activation energy of the chain segment movement; on the other hand, the high-strength flame-retardant polyester copolymer improves the crystallinity of the fiber by improving the orderly stacking of the molecular chains, restricts the movement of the amorphous region segments, and at the same time, the thermal decomposition activation energy of the benzoxazole structure is high, which significantly improves the heat resistance of the polyester fiber composite material.
[0088] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength fiber composite material, It is characterized in that The preparation method comprises the following steps: (1) Under nitrogen atmosphere, terephthalic acid and a structural formula of The diphenol-based benzoxazole phosphonitrile flame retardant intermediate is stirred evenly, and a catalyst, dihydrogen trioxide, and a heat stabilizer, triphenyl phosphate, are added to carry out an esterification reaction at 220-260°C, and the top temperature of the fractionation column is controlled to be 120-140°C. When the amount of esterified water received is 80-90% of the theoretical value, vacuum is drawn to carry out a polycondensation reaction, and the vacuum degree in the kettle is reduced to 0.2-0.3 kPa, and nitrogen is used to break the vacuum and discharge the material to obtain a high-strength flame retardant polyester copolymer; (2) 100 parts by weight of vacuum-dried PET polyester chips and 5-25 parts of high-strength flame-retardant polyester copolymer are added to a high-speed disperser and mixed evenly, and then placed on a twin-screw high-speed composite spinning machine for melt spinning at a spinning speed of 600-800 m / min and a spinning machine temperature of 260-280°C. After the primary fibers are balanced for 8-12 hours, they are stretched and wound on a parallel drawing machine to obtain a high-strength fiber composite material.
2. The method for preparing the high-strength fiber composite material according to claim 1, It is characterized in that In the step (1), by weight, terephthalic acid is 100 parts, diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate is 360-390 parts, antimony trioxide is 0.05-0.1 parts, and triphenyl phosphate is 0.03-0.06 parts.
3. The method for preparing the high-strength fiber composite material according to claim 1, It is characterized in that In the step (1), the polycondensation reaction temperature is 250-280° C., and the polycondensation reaction time is 24-48 hours.
4. The method for preparing the high-strength fiber composite material according to claim 1, It is characterized in that In the step (2), the drawing speed is 400-500 m / min, and the drawing multiple is 5-7.
5. The method for preparing the high-strength fiber composite material according to claim 1, It is characterized in that The method for preparing the diphenol-based benzoxazole phosphonium nitrogen flame retardant intermediate in step (1) comprises the following steps: Step S1, adding 2-amino-4-methoxyphenol, p-aminobenzoic acid and polyphosphoric acid to a reaction flask equipped with a reflux condenser, stirring for reaction, cooling to room temperature after the reaction, pouring into an ice water bath under stirring, adding saturated sodium bicarbonate for neutralization, filtering, washing the filter cake with deionized water, and drying to obtain 4-methoxybenzoxazolylaniline; Step S2, under a nitrogen atmosphere, add phenyl dichloride phosphate and acetonitrile to a reaction flask, stir evenly, add triethylamine and 4-methoxybenzoxazolylaniline, stir to react, filter after the reaction is completed, wash with ethanol, and dry to obtain a dimethoxybenzoxazolyl phosphorus nitrogen flame retardant intermediate; Step S3, under a nitrogen atmosphere, add 100 parts by weight of a dimethoxybenzoxazole phosphine nitrogen flame retardant intermediate and dichloromethane to a reaction flask, stir evenly, cool to -78°C, dropwise add 90-110 parts of boron tribromide, stir to react, and after the reaction is completed, cool to 0°C, pour into deionized water, add ethyl acetate for extraction, concentrate the organic phase, and dry to obtain a diphenol-based benzoxazole phosphine nitrogen flame retardant intermediate.
6. The method for preparing the high-strength fiber composite material according to claim 5, It is characterized in that In the step S1, by weight, 2-amino-4-methoxyphenol is 100 parts, p-aminobenzoic acid is 120-150 parts, and polyphosphoric acid is 1000-1500 parts.
7. The method for preparing the high-strength fiber composite material according to claim 5, It is characterized in that In step S1, the reaction temperature is 170-190° C. and the reaction time is 8-16 hours.
8. The method for preparing the high-strength fiber composite material according to claim 5, It is characterized in that In the step S2, by weight, 100 parts of phenyl dichloride phosphate, 110-130 parts of triethylamine, and 230-255 parts of 4-methoxybenzoxazolylaniline are used.
9. The method for preparing the high-strength fiber composite material according to claim 5, It is characterized in that In step S2, the reaction temperature is 60-80° C. and the reaction time is 5-10 h.
10. The method for preparing the high-strength fiber composite material according to claim 5, It is characterized in that In step S3, the reaction temperature is 20-35° C. and the reaction time is 16-24 h.