Preparation method of aerogel fiber felt

The preparation of hydrophobic aerogel slurry and composite with fiber felt by reacting inorganic silicone source and catalyst, solving the problems of complex and high cost of preparation of aerogel fiber felt in the prior art, and achieving uniform distribution and low thermal conductivity of the aerogel , significantly improves the thermal insulation performance.

CN118930130AActive Publication Date: 2024-11-12CNCEC HUALU NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411167906.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The preparation process of existing aerogel fiber felts is complex and costly. The produced aerogels are unevenly distributed and have high thermal conductivity, resulting in poor thermal insulation performance.

Method used

The sol is prepared by dissolving the inorganic silicone source in desalinated water, adding an acid catalyst and an alkaline catalyst to react to obtain the sol. After frozen desalination and aging of the water bath, it is subjected to hydrophobic modification to obtain a hydrophobic aerogel slurry and a preliminary molded fiber felt. A uniformly distributed aerogel fiber felt is formed by injection and secondary needle puncture.

Benefits of technology

The preparation process is simplified, the cost is reduced, the uniform distribution and thermal insulation performance of the aerogel are improved, the thermal conductivity coefficient of the room temperature is reduced by 20%, and the production efficiency and thermal insulation performance are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930130A_ABST
    Figure CN118930130A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aerogel fiber felt, which is characterized in that aerogel slurry and a fiber felt are directly compounded to prepare the aerogel felt, and the aerogel slurry does not need to be dried into aerogel powder, re-dissolved into the aerogel slurry and compounded with the aerogel fiber felt, so that the preparation process is simplified, and the cost is saved. Compared with the method for preparing the aerogel slurry by using finished aerogel powder, the method for preparing the aerogel fiber felt by directly using the aerogel slurry prepared at present can avoid using an aqueous solvent to dissolve the aerogel powder, thereby avoiding damage to the structure of the aerogel and influence on the heat insulation performance of the aerogel fiber felt. The normal-temperature heat conductivity coefficient of the aerogel fiber felt is 0.0201 W / (m.k), and compared with an aerogel fiber felt prepared from finished aerogel powder, the heat conductivity coefficient is reduced by 20%, and the heat insulation performance is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of aerogel fiber felt, and in particular to a method for preparing aerogel fiber felt. Background Art

[0002] Aerogel fiber felt is a high-performance thermal insulation material, which is widely used in thermal insulation in industrial production, transportation, household appliances and other fields.

[0003] At present, most companies producing aerogel fiber felts purchase finished aerogel powder to prepare aerogel fiber felts. During the preparation, the aerogel powder is first made into aerogel slurry and then compounded with various already formed needle-punched felts, and finally dried. In this way, first, the purchase of finished aerogel powder to prepare aerogel fiber felts is costly and not conducive to industrial production; second, most of the finished aerogel powders are actually made by drying aerogel slurry, but when using it to prepare aerogel fiber felts, the aerogel powder needs to be dissolved into slurry again. Such a preparation process is relatively complicated and costly. In addition, aerogel powders are mostly dissolved in water as a solvent during the dissolution process to make aqueous aerogel slurry, which is then compounded with fiber felt. The aqueous system will cause certain damage to the structure of the aerogel powder, and the thermal conductivity of the fiber felt produced will be higher. The slurry of the aqueous system will dry more slowly, the production efficiency will be lower, and the product will turn yellow if the drying temperature is not well controlled. For example, CN112522949A discloses a method for manufacturing aerogel felt, which includes the following steps: S10, adding aerogel powder to water containing a wetting agent and stirring to form aerogel slurry; S20, using an injection gun head to inject the aerogel slurry into the glass fiber felt; S30, drying the glass fiber felt in a dryer; S40, mixing water, acrylic emulsion, talcum powder, VAE emulsion, and water-based curing agent and stirring evenly to prepare a soaking liquid; S50, pouring the soaking liquid into a soaking tank, soaking the dried glass fiber felt in the soaking tank, and when the soaking liquid is attached to the surface of the glass fiber felt, drying the glass fiber felt through a dryer to form an aerogel felt. This technical solution uses finished aerogel powder to prepare aerogel fiber felt, and its room temperature thermal conductivity is 0.02436W / (m·k), the thermal conductivity is high, and the thermal insulation performance is poor.

[0004] In addition, when compounding aerogel slurry and fiber felt, the existing technology mostly uses immersion or spraying to compound aerogel. This compounding method will cause uneven impregnation of aerogel and affect the thermal insulation performance of aerogel felt. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing an aerogel fiber felt, so as to solve the problems that the preparation process of the aerogel fiber felt in the prior art is relatively complicated, the cost is high, and the aerogel fiber felt prepared has uneven aerogel distribution and high thermal conductivity.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an aerogel fiber felt comprises the following steps:

[0008] (1) dissolving an inorganic silicon source in desalted water, slowly adding an acid catalyst thereto, and reacting the mixture to obtain sol A, and then freezing and desalting sol A to obtain sol B;

[0009] (2) adding an alkaline catalyst and desalted water to sol B to allow sufficient reaction to obtain an aqueous gel;

[0010] (3) subjecting the aqueous gel obtained in step (2) to water bath aging, water washing and crushing in sequence;

[0011] (4) adding a solvent and a surface modifier to the aqueous gel crushed in step (3), performing a hydrophobic modification on the aqueous gel, standing the aqueous gel for stratification, and collecting the supernatant to obtain a hydrophobic aerogel slurry;

[0012] (5) After the chopped fibers are opened, combed, and laid in sequence, the laid fiber web is pre-needled to obtain a preliminarily formed fiber mat;

[0013] (6) after the hydrophobic aerogel slurry obtained in step (4) and the adhesive are uniformly mixed, the mixed slurry is quantitatively injected into the preliminarily formed fiber felt, and the preliminarily formed fiber felt is subjected to secondary needle punching to obtain a formed fiber felt;

[0014] (7) spraying the mixed slurry obtained in step (6) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the hydrophobic aerogel slurry;

[0015] (8) After the fiber felt obtained in step (7) is dried, an aerogel fiber felt is obtained.

[0016] Furthermore, the freezing desalination in step (1) is as follows: cooling the sol A to 0-10° C. until no more crystals are precipitated, filtering to remove the solid, and obtaining the sol B.

[0017] Furthermore, in step (6), the hydrophobic aerogel slurry and the adhesive are mixed at a mass ratio of the inorganic silicon source to the adhesive of 100:1 to 10.

[0018] Furthermore, the mass ratio of the inorganic silicon source, the acid catalyst and the alkaline catalyst is 100:100-250:0.5-2.

[0019] Furthermore, in the step (4), the mass ratio of the solvent to the surface modifier is 100:1-10.

[0020] Furthermore, in step (4), the solvent includes hexamethyldisiloxane, methanol, ethanol, n-hexane or n-heptane.

[0021] Furthermore, in step (4), the surface modifier includes trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane or propyltrichlorosilane.

[0022] Furthermore, in step (8), the drying method is to transfer the fiber felt obtained in step (7) to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

[0023] Furthermore, the water bath aging in step (3) is performed by standing in a water bath at 40 to 60° C. for 6 to 20 hours.

[0024] Furthermore, the adhesive in step (6) includes epoxy resin, acrylic resin, white latex, phenolic resin or polyurethane.

[0025] The aerogel slurry prepared by the present invention uses water glass as a silicon source, and the silicon source is low in price and the cost is controllable. The gelation speed is controlled by an acid-base two-step method, and freezing desalination and water washing desalination are combined to improve the quality of the product. The undried hydrophobic aerogel slurry is directly injection-compounded with an incompletely needled fiber felt, and finally the aerogel is evenly distributed in the fiber felt, so as to prepare an aerogel felt with good thermal conductivity and low production cost.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The method for preparing aerogel fiber felt of the present invention adopts aerogel slurry and fiber felt to directly compound to prepare aerogel felt. There is no need to dry the aerogel slurry into aerogel powder, dissolve it into aerogel slurry, and then compound it with aerogel fiber felt, which simplifies the preparation process and saves costs. Compared with using finished aerogel powder to prepare aerogel slurry, directly using ready-made aerogel slurry to prepare aerogel fiber felt can avoid using aqueous solvents to dissolve aerogel powder, thereby avoiding damage to the structure of the aerogel and affecting the thermal insulation performance of the aerogel fiber felt. The room temperature thermal conductivity of the aerogel fiber felt of the present invention is 0.0201W / (mk). Compared with the aerogel fiber felt prepared using finished aerogel powder, the thermal conductivity is reduced by 20%, and the thermal insulation performance is significantly improved.

[0028] 2. The composite method of the aerogel slurry and the fiber felt of the present invention is to first inject the aerogel slurry into the preliminarily formed fiber felt by injection, and then perform a secondary needle punch on the fiber felt. In this way, firstly, the composite is performed by injection, so that the aerogel in the fiber felt can be distributed more evenly. Secondly, the present invention does not directly inject the aerogel slurry into the finished fiber felt (the finished fiber felt that has been needled has been formed and has a certain density and strength, and direct immersion or injection cannot evenly distribute the hydrophobic aerogel slurry inside the fiber felt), but first injects the aerogel slurry into the preliminarily formed fiber felt, and then performs a secondary needle punch. This composite method can make the aerogel distribution more even, and further improve the thermal insulation performance of the aerogel fiber felt.

[0029] 3. The present invention combines the production process of aerogel slurry with the preparation process of fiber felt, thereby realizing the continuous production of aerogel fiber felt. This continuous production process reduces manufacturing costs and increases production efficiency. The composite fiber felt is directly transferred to the tunnel drying line for drying, which can realize an assembly line production line, greatly improve production efficiency, reduce costs and increase efficiency.

[0030] 4. The investment cost of production line equipment is much lower than that of supercritical process, which solves the problem of large investment in CO2 supercritical process equipment and high risk factor of high-temperature supercritical process, and lowers the investment threshold for investors. Compared with CO2 supercritical drying process, the product after drying will have some organic solvents. The product of the present invention is dried in tunnel furnaces in different temperature zones, and the product has better fire resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention is a flow chart of the process for preparing aerogel slurry used in aerogel fiber felt;

[0032] Figure 2 The present invention is a flow chart of the preparation process of aerogel fiber felt. DETAILED DESCRIPTION

[0033] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.

[0034] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.

[0035] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.

[0036] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.

[0037] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods.

[0038] The quantitative tests in the present invention were repeated three times and the results were averaged.

[0039] The present invention provides a method for preparing an aerogel fiber felt. The preparation process is as follows: Figure 1 , Figure 2 As shown, the following steps are included:

[0040] (1) dissolving an inorganic silicon source in desalted water, slowly adding an acid catalyst thereto, and reacting the mixture to obtain sol A, and then freezing and desalting sol A to obtain sol B;

[0041] (2) adding an alkaline catalyst and desalted water to sol B to allow sufficient reaction to obtain an aqueous gel;

[0042] (3) The aqueous gel obtained in step (2) is subjected to water bath aging, water washing and crushing in sequence; water bath aging can strengthen the internal structure of the gel, thereby improving product quality and reducing product thermal conductivity. After aging, water washing can remove residual salt substances in the aqueous gel, thereby avoiding an increase in the thermal conductivity of the aerogel product, thereby improving product quality.

[0043] (4) adding a solvent and a surface modifier to the aqueous gel crushed in step (3), performing a hydrophobic modification on the aqueous gel, standing the aqueous gel for stratification, and collecting the supernatant to obtain a hydrophobic aerogel slurry;

[0044] (5) After the chopped fibers are opened, combed, and laid in sequence, the laid fiber web is pre-needled to obtain a preliminarily formed fiber mat;

[0045] (6) after uniformly mixing the aerogel slurry obtained in step (4) and the adhesive, quantitatively injecting the mixed slurry into the preliminarily formed fiber felt, and performing secondary needle punching on the preliminarily formed fiber felt to obtain a formed fiber felt;

[0046] (7) spraying the mixed slurry obtained in step (6) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the aerogel slurry;

[0047] (8) The fiber felt obtained in step (7) is transferred to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

[0048] In specific implementation, the freezing desalination in step (1) is as follows: cooling the sol A to 0-10°C until no more crystals are precipitated, filtering to remove the solids, and obtaining the purified sol B. Cooling the sol A can cause most of the salts to precipitate, thereby obtaining a sol containing only a very small amount of salt, thereby achieving separation and purification of the sol. The obtained solid precipitate can be collected and purified for secondary sale or directly treated as solid waste.

[0049] In a specific implementation, the inorganic silicon source includes water glass, potassium silicate or lithium silicate. The acid catalyst includes one or more of nitric acid, hydrochloric acid, phosphoric acid or sulfuric acid. The mass concentration of the acid catalyst is 15-20%. The alkaline catalyst includes one or more of sodium hydroxide, potassium hydroxide, ammonia water with a mass concentration of 15-20% or sodium carbonate.

[0050] In a specific implementation, the mass ratio of the inorganic silicon source, the acid catalyst and the alkaline catalyst is 100:100-250:0.5-2. Controlling the mass ratio of the inorganic silicon source to the acid-base catalyst within this range can ensure a certain silicon content, avoid too low silicon content, resulting in increased thermal conductivity; and avoid too high silicon content, increased costs, and hardening of the product.

[0051] In a specific implementation, the water bath aging in step (3) is to stand in a water bath at 40 to 60° C. for 6 to 20 hours.

[0052] In a specific implementation, the solvent used in step (4) includes hexamethyldisiloxane, methanol, ethanol, n-hexane or n-heptane.

[0053] In a specific implementation, the surface modifier used in step (4) includes trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane or propyltrichlorosilane.

[0054] In a specific implementation, the mass ratio of the solvent to the surface modifier is 100:1 to 10. If the modifier is too little, the modification will be insufficient. After the modification is completed and the surface is left to stand for stratification, a portion of the aqueous gel will remain in the lower wastewater, resulting in a low yield of the aerogel slurry and a waste of cost. If the modifier is too much, the cost will be high.

[0055] In a specific implementation, the mass ratio of the inorganic silicon source to the adhesive is 100:1 to 10. If the adhesive is too little, the bonding effect between the hydrophobic aerogel and the fiber felt will be poor, resulting in serious powder loss; and if the adhesive is too much, the product will become hard, which is not conducive to the application of the product, and the thermal conductivity will increase, resulting in a decrease in the thermal insulation performance of the product, so the mass ratio of the inorganic silicon source to the adhesive is controlled to be 100:1 to 10.

[0056] In a specific implementation, the adhesive includes epoxy resin, acrylic resin, white latex, phenolic resin or polyurethane.

[0057] In a specific implementation, the chopped fibers include one or more of glass fibers, ceramic fibers, mullite fibers, carbon fibers, basalt fibers, and high-silica fibers.

[0058] During specific implementation, product sampling, winding and packaging are carried out at the end of the tunnel drying line, and the packaged finished products are transferred to the warehouse for storage.

[0059] Example 1

[0060] This embodiment provides a method for preparing an aerogel fiber felt, comprising the following steps:

[0061] (1) 100 kg of water glass and 100 kg of desalted water are stirred and mixed uniformly, and then 100 kg of sulfuric acid with a mass fraction of 20% is slowly added thereto, and the pH is adjusted to below 2, and the reaction is fully carried out to obtain a sol; wherein the purchase specifications of the water glass are: modulus 3.1-3.4, Baume degree 39.0-40.0, and silicon dioxide content ≥26%.

[0062] (2) cooling the obtained sol to 5° C. until no more crystals are precipitated, filtering out the solids, and obtaining a purified sol;

[0063] (3) adding 1 kg of 20% concentrated ammonia water and 19 kg of desalted water to the purified sol, adjusting the pH to 5, and reacting to obtain an aqueous gel;

[0064] (4) placing the aqueous gel obtained in step (3) in a 60° C. water bath for aging for 6 h, crushing the aged gel, washing it with water to remove salt, and then mechanically crushing the desalted colloid after washing;

[0065] (5) Adding a mixed solution of 500 kg of hexamethyldisiloxane and 20 kg of trimethylchlorosilane to the crushed gel in step (4), stirring continuously, and performing hydrophobic modification on the crushed aqueous gel. After the modification is completed, the separated upper liquid is the hydrophobic aerogel slurry.

[0066] (6) The short-cut inorganic glass fibers are weighed according to the process conditions, and then added to the opening machine for opening; the opened glass fibers are automatically transferred to the carding machine for fiber combing to fully comb the glass fibers; the combed glass fibers are automatically transferred to the web laying machine to lay the glass fibers into a continuous glass fiber web; the number of layers of the glass fiber web is adjusted according to the thickness of the needle felt, and then pre-needling is performed to obtain a pre-needled fiber felt. The main purpose of pre-needling is to make the fiber webs between the layers have a certain weaving and interlacing in the longitudinal direction, initially forming the contour of the needle felt, and having a certain strength.

[0067] (7) After the hydrophobic aerogel slurry obtained in step (5) and 10 kg of white latex are stirred and mixed evenly, the mixed slurry is quantitatively injected into the preliminarily formed fiber felt, and the preliminarily formed fiber felt is subjected to secondary needle punching to obtain a formed fiber felt; the process of injecting the slurry is carried out in a sealed cover filled with nitrogen to prevent the risk of explosion, combustion, etc.

[0068] (8) spraying the mixed slurry obtained in step (7) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the aerogel slurry;

[0069] (9) The fiber felt obtained in step (8) is transferred to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

[0070] Example 2

[0071] This embodiment provides a method for preparing an aerogel fiber felt, comprising the following steps:

[0072] (1) After 100 kg of water glass and 100 kg of water are stirred and mixed uniformly, 250 kg of nitric acid with a mass fraction of 20% is slowly added thereto, the pH is adjusted to below 2, and the reaction is fully carried out to obtain a sol; wherein the purchase specifications of the water glass are: modulus 3.1-3.4, Baume degree 39.0-40.0, and silicon dioxide content ≥26%.

[0073] (2) cooling the obtained sol to 0° C. until no more crystals are precipitated, filtering out the solids, and obtaining a purified sol;

[0074] (3) adding 0.8 kg of sodium hydroxide and 19.2 kg of desalted water to the purified sol, adjusting the pH to 5, and reacting to obtain an aqueous gel;

[0075] (4) placing the aqueous gel obtained in step (3) in a 50° C. water bath for aging for 12 h, crushing the aged aqueous gel, washing it with water to remove salt, and mechanically crushing the desalted colloid after washing;

[0076] (5) Adding a mixed solution of 500 kg of n-heptane and 15 kg of dimethyldichlorosilane to the pulverized aqueous gel in step (4) to hydrophobically modify the aqueous gel. After the modification is completed, the separated supernatant is the hydrophobic aerogel slurry.

[0077] (6) The chopped ceramic fibers are weighed according to the process conditions, and then added to the opening machine for opening; the opened ceramic fibers are automatically transferred to the carding machine for fiber combing to fully comb the ceramic fibers; the combed ceramic fibers are automatically transferred to the web laying machine to lay the ceramic fibers into a continuous ceramic fiber web; the number of layers of the ceramic fiber web is adjusted according to the thickness of the needle felt, and then pre-needling is performed to obtain a pre-needled fiber felt. The main purpose of pre-needling is to make the fiber webs between layers have a certain weaving and interlacing in the longitudinal direction, initially forming the contour of the needle felt, and having a certain strength.

[0078] (7) After the aerogel slurry obtained in step (5) and 10 kg of epoxy resin are stirred and mixed evenly, the mixed slurry is quantitatively injected into the preliminarily formed fiber felt, and the preliminarily formed fiber felt is subjected to secondary needle punching to obtain a formed fiber felt; the process of injecting the slurry is carried out in a sealed cover filled with nitrogen to prevent the risk of explosion, combustion, etc.

[0079] (8) spraying the mixed slurry obtained in step (7) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the aerogel slurry;

[0080] (9) The fiber felt obtained in step (8) is transferred to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

[0081] Example 3

[0082] This embodiment provides a method for preparing an aerogel fiber felt, comprising the following steps:

[0083] (1) After 100 kg of water glass and 100 kg of water are stirred and mixed uniformly, 150 kg of nitric acid with a mass fraction of 20% is slowly added thereto, the pH is adjusted to below 2, and the reaction is fully carried out to obtain a sol; wherein the purchase specifications of the water glass are: modulus 3.1-3.4, Baume degree 39.0-40.0, and silicon dioxide content ≥26%.

[0084] (2) cooling the obtained sol to 10° C. until no more crystals are precipitated, filtering to remove the solid, and obtaining a purified sol;

[0085] (3) adding 1 kg of sodium hydroxide and 24 kg of deionized water to the purified sol, adjusting the pH to 6, and reacting to obtain an aqueous gel;

[0086] (4) placing the aqueous gel obtained in step (3) in a 40° C. water bath for aging for 20 h, crushing the aged aqueous gel, washing it with water to remove salt, and mechanically crushing the desalted colloid after washing;

[0087] (5) Adding a mixed solution of 500 kg of n-hexane and 5 kg of methyltrichlorosilane to the pulverized aqueous gel in step (4) to hydrophobically modify the aqueous gel. After the modification is completed, the separated supernatant is the hydrophobic aerogel slurry.

[0088] (6) Weigh the chopped carbon fibers according to the process conditions, and then add them to the opener for opening; the opened carbon fibers are automatically transferred to the carding machine for fiber combing to fully comb the carbon fibers; the combed carbon fibers are automatically transferred to the web laying machine to lay the carbon fibers into a continuous carbon fiber web; the number of layers of the carbon fiber web is adjusted according to the thickness of the needle felt, and then pre-needling is performed to obtain a pre-needled fiber felt. The main purpose of pre-needling is to make the fiber webs between the layers have a certain weaving and interlacing in the longitudinal direction, initially forming the contour of the needle felt, and having a certain strength.

[0089] (7) After the aerogel slurry obtained in step (5) and 10 kg of phenolic resin are stirred and mixed evenly, the mixed slurry is quantitatively injected into the preliminarily formed fiber felt, and the preliminarily formed fiber felt is subjected to secondary needle punching to obtain a formed fiber felt; the process of injecting the slurry is carried out in a sealed cover filled with nitrogen to prevent the risk of explosion, combustion, etc.

[0090] (8) spraying the mixed slurry obtained in step (7) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the aerogel slurry;

[0091] (9) The fiber felt obtained in step (8) is transferred to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

[0092] A comparison table of room temperature thermal conductivity of aerogel fiber felts of this embodiment and prior art is shown in Table 1.

[0093] Table 1 Fiber felt performance comparison table

[0094] sample Thermal conductivity / W / (m·K) Glass fiber needle felt 0.032 CN112522949A-Example 1 0.02418 Example 1 0.0201 Example 2 0.0211 Example 3 0.0217

[0095] It can be seen from Table 1 that the thermal conductivity of the aerogel fiber felt prepared by the present invention is as low as 0.0201 W / (m·K) at room temperature, and the thermal insulation performance is relatively high. Compared with the aerogel fiber felt prepared using the finished aerogel powder, the thermal conductivity is reduced by 20%, and the thermal insulation performance is significantly improved.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an aerogel fiber felt, characterized in that: The following steps are involved: (1) dissolving an inorganic silicon source in desalted water, slowly adding an acid catalyst thereto, and reacting the mixture to obtain sol A, and then freezing and desalting sol A to obtain sol B; (2) adding an alkaline catalyst and desalted water to sol B to allow sufficient reaction to obtain an aqueous gel; (3) subjecting the aqueous gel obtained in step (2) to water bath aging, water washing and crushing in sequence; (4) adding a solvent and a surface modifier to the aqueous gel crushed in step (3), performing a hydrophobic modification on the aqueous gel, standing the aqueous gel for stratification, and collecting the supernatant to obtain a hydrophobic aerogel slurry; (5) After the chopped fibers are opened, combed, and laid in sequence, the laid fiber web is pre-needled to obtain a preliminarily formed fiber mat; (6) after the hydrophobic aerogel slurry obtained in step (4) and the adhesive are uniformly mixed, the mixed slurry is quantitatively injected into the preliminarily formed fiber felt, and the preliminarily formed fiber felt is subjected to secondary needle punching to obtain a formed fiber felt; (7) spraying the mixed slurry obtained in step (6) onto the formed fiber felt so that the surface of the formed fiber felt is evenly covered with the hydrophobic aerogel slurry; (8) After the fiber felt obtained in step (7) is dried, an aerogel fiber felt is obtained.

2. The method for preparing aerogel fiber felt according to claim 1, characterized in that: The freezing desalination in step (1) is as follows: cooling the sol A to 0-10° C. until no more crystals are precipitated, filtering to remove the solids, and obtaining the sol B.

3. The method for preparing aerogel fiber felt according to claim 1, characterized in that: In the step (6), the hydrophobic aerogel slurry and the adhesive are mixed at a mass ratio of the inorganic silicon source to the adhesive of 100:1 to 10.

4. The method for preparing aerogel fiber felt according to claim 1, characterized in that: The mass ratio of the inorganic silicon source, the acid catalyst and the alkaline catalyst is 100:100-250:0.5-2.

5. The method for preparing aerogel fiber felt according to claim 1, characterized in that: In the step (4), the mass ratio of the solvent to the surface modifier is 100:1-10.

6. The method for preparing aerogel fiber felt according to claim 1, characterized in that: In the step (4), the solvent includes hexamethyldisiloxane, methanol, ethanol, n-hexane or n-heptane.

7. The method for preparing aerogel fiber felt according to claim 1, characterized in that: In the step (4), the surface modifier includes trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane or propyltrichlorosilane.

8. The method for preparing aerogel fiber felt according to claim 1, characterized in that: In the step (8), the drying method is to transfer the fiber felt obtained in the step (7) to a tunnel drying line for continuous drying to obtain an aerogel fiber felt.

9. The method for preparing aerogel fiber felt according to claim 1, characterized in that: The water bath aging in step (3) is performed by standing at 40 to 60° C. in a water bath for 6 to 20 hours.

10. The method for preparing aerogel fiber felt according to claim 1, characterized in that: The adhesive in step (6) includes epoxy resin, acrylic resin, white latex, phenolic resin or polyurethane.

Citation Information

Patent Citations

  • Manufacturing method of aerogel felt

    CN112522949A

  • Fiber-reinforced heat-insulating silicone aerogel composite material and preparation method thereof

    CN108641361A

  • Equipment and method for recycling aerogel waste felt

    CN114986943A

  • Method for rapidly preparing silicon dioxide aerogel and composite product thereof at low cost

    CN115093197A

  • Low-heat-conductivity-coefficient fiber composite aerogel wet felt and preparation method thereof

    CN115583829A