Alkali-activated cementing material for improving low-carbon durability and preparation method

By combining functionalized silicon carbide nanofibers and calcined kaolin, alkali-excited gelling materials with high durability and mechanical properties were prepared, which solved the problem of insufficient stability and durability of gelling materials in the prior art, and was suitable for marine engineering and building materials in high-altitude areas.

CN118930205APending Publication Date: 2024-11-12CHONGQING JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984965.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing alkali-excited granulated blast furnace slag gelling materials are insufficient in stability and durability, which is difficult to meet the practical needs of engineering, especially in applications in marine concrete and high-altitude areas, which are susceptible to freeze-thawing and sulfate corrosion.

Method used

Functional silicon carbide nanofibers and calcined kaolin as the main raw materials, and gelled materials are prepared by mixing magnetic stirring and ultrasonic shock to form a three-dimensional spatial network structure, increasing the density of hydration products and structures, and preventing microcracks and micropores. form.

Benefits of technology

It significantly improves the mechanical properties and durability of gelled materials, reduces cement usage and carbon emissions, realizes the utilization of industrial solid waste, and shows a lower mass loss rate and strength in freeze-thaw and sulfate corrosion tests. Loss rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930205A_ABST
    Figure CN118930205A_ABST
Patent Text Reader

Abstract

The invention discloses an alkali-activated cementing material for improving low-carbon durability. The alkali-activated cementing material comprises the following raw materials in parts by weight: 70-100 parts of inorganic powder, 0.05-0.10 part of functionalized silicon carbide nanofibers, 8-16 parts of an alkali activator, 11-15 parts of water and 13-15 parts of quartz sand, and the functionalized silicon carbide nanofibers are formed by adhering silicon hydroxyl groups to the surfaces of the silicon carbide nanofibers; the cementitious material has a three-dimensional space net structure, the mechanical property can be effectively improved, aluminum is introduced into the calcined kaolin in the inorganic powder, and hydration products of a reaction system can be increased; the functionalized silicon carbide nanofibers are combined with the inorganic powder, so that microcracks and micropores caused by freeze-thaw damage and sulfate corrosion damage can be effectively prevented, and the purpose of improving the durability is achieved. According to the alkali-activated cementing material, the use of cement can be greatly reduced, carbon emission is reduced, the purpose of utilizing industrial solid waste is achieved, and the preparation process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, and in particular to an alkali-activated gelling material with improved low-carbon durability and a preparation method thereof. Background Art

[0002] Ordinary Portland cement is the most commonly used and indispensable civil engineering material. However, the excessive carbon dioxide emissions and energy consumption caused by cement production are receiving more and more attention. According to the two documents of the Ministry of Ecology and Environment of my country in 2024, "Guidelines for the Accounting and Reporting of Greenhouse Gas Emissions of Enterprises - Cement Clinker Production" and "Technical Guidelines for the Verification of Greenhouse Gas Emissions of Enterprises - Cement Clinker Production", the cement industry, as the main supplier of bulk building materials, accounts for 13.5% of the total emissions. Therefore, under the background of "double carbon", it is urgent to promote sustainable ecological development and adopt low-carbon cementitious materials. As a by-product of blast furnace ironmaking, industrial granulated blast furnace slag is bound to cause environmental pollution and ecological damage if it is piled up for a long time. Therefore, preparing cementitious materials with granulated blast furnace slag through alkali activation technology is a feasible solution to turn solid waste into treasure and replace cement to reduce carbon emissions. However, the single use of granulated blast furnace slag to prepare cementitious materials has poor stability and is not enough to meet engineering practicality, thus affecting durability. Durability is crucial to the long-term stable development of materials in the construction and transportation industries, especially marine concrete. Some harmful ions penetrate into the matrix through the pores of the material, form stress through the expansion products, produce microcracks, destroy the matrix structure, and cause indelible harm over time; at the same time, in the extremely cold regions of my country, freeze-thaw cycles are also very common in damaging the concrete matrix. It is generally believed that under repeated expansion pressure and penetration pressure, the microcracks and pores inside the material will gradually increase and expand, causing loss of structural quality and strength. At present, there are mainly the following methods to solve the stability of alkali-activated granulated blast furnace slag cementitious materials: (1) adjust the mix ratio to reduce the alkali content; (2) add highly active silicon and aluminum raw materials; (3) add chemical admixtures; (4) other methods. Among them, adjusting the alkali content of the alkali activator in method (1) can moderately reduce the cracking phenomenon of granulated blast furnace slag cementitious materials, but the later strength improvement is not obvious; for method (2), adding high-activity silicon aluminum raw materials, although it can appropriately improve the stability of the system, it does not effectively solve the microcracks and micropores caused by durability damage; for method (3), the additional use of chemical admixtures can improve the early hydration degree of granulated blast furnace slag cementitious materials to a certain extent, thereby slightly improving the later stability, and the addition of new chemical admixtures may bring harmful ions, and the impact on durability is still unknown.

[0003] Therefore, the stability and durability of alkali-activated cementitious materials remain a technical problem that needs to be solved urgently. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide an alkali-activated cementitious material and a preparation method with improved low-carbon durability, which can improve mechanical strength while improving durability, can adapt to sulfate corrosion and freeze-thaw damage in high-cold areas, and can be widely used in the field of road and bridge concrete structures in marine and high-cold areas.

[0005] The alkali-activated gelling material for improving low-carbon durability of the present invention comprises 70-100 parts of inorganic powder, 0.05-0.10 parts of functionalized silicon carbide nanofibers, 8-16 parts of alkaline activator, 11-15 parts of water, and 13-15 parts of quartz sand in parts by weight, wherein the functionalized silicon carbide nanofibers are formed by silanol groups attached to the surface of the silicon carbide nanofibers;

[0006] Furthermore, the functionalized silicon carbide nanofiber is prepared by: generating an amorphous oxide thin layer on the surface of the silicon carbide nanofiber, and then converting the amorphous oxide into silanol groups attached to the surface of the silicon carbide nanofiber under acid and alkali conditions;

[0007] Furthermore, the functionalized silicon carbide nanofibers are prepared by: placing the silicon carbide nanofibers in an acid for ultrasonic treatment, washing and drying, then placing the dried silicon carbide nanofibers in an alkaline solution for stirring, and finally washing and drying to obtain the functionalized silicon carbide nanofibers;

[0008] Further, the acid is hydrochloric acid, and the alkali is caustic soda;

[0009] Furthermore, the alkaline activator is water glass and sodium hydroxide, and by weight, the water glass is 6-12 parts and the sodium hydroxide is 2-4 parts;

[0010] Furthermore, the inorganic powder is a mixture of calcined kaolin and granulated blast furnace slag, wherein the granulated blast furnace slag is 60-80 parts by weight and the calcined kaolin is 10-20 parts by weight;

[0011] Further, the raw materials include, by mass, 70 parts of granulated blast furnace slag, 15 parts of calcined kaolin, 0.075 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand;

[0012] Furthermore, the mesh number of the quartz sand is 150-250 mesh; the mesh number of the calcined kaolin is 1200-1300 mesh.

[0013] The present invention also discloses a method for preparing an alkali-activated gelling material with improved low-carbon durability, comprising the following steps:

[0014] S1, mixing the functionalized silicon carbide nanofibers with an alkaline activator by magnetic stirring and ultrasonic oscillation to prepare a functionalized silicon carbide nanofiber mixed solution;

[0015] S2, mixing quartz sand, water, functionalized silicon carbide nanofiber mixed liquid and inorganic powder to prepare an alkali-activated cementitious material with improved low carbon durability.

[0016] Beneficial effects of the invention: The alkali-activated cementitious material and preparation method for improving low-carbon durability of the invention have a three-dimensional spatial network structure, which can effectively improve mechanical properties. The calcined kaolin in the inorganic powder introduces aluminum elements, which can increase the hydration products of the reaction system; the functionalized silicon carbide nanofibers are combined with the inorganic powder to effectively prevent microcracks and micropores caused by freeze-thaw damage and sulfate corrosion damage, thereby achieving the purpose of improving durability. The alkali-activated cementitious material can not only greatly reduce the use of cement and reduce carbon emissions, but also achieve the purpose of industrial solid waste utilization, and the preparation process is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0018] Figure 1 This is the SEM image of the alkali-activated gelling material prepared in Example 3 after curing for 28 days;

[0019] Figure 2 This is a SEM image of the alkali-activated gelling material prepared in Example 3 after 50 freeze-thaw cycles;

[0020] Figure 3 This is the SEM image of the alkali-activated cementitious material prepared in Example 3 after 56 days of sulfate corrosion;

[0021] Figure 4 This is a sample diagram of alkali-activated gelling material prepared in Example 3. DETAILED DESCRIPTION

[0022] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0023] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0024] The alkali-activated cementitious material for improving low-carbon durability of this embodiment comprises 70-100 parts of inorganic powder, 0.05-0.10 parts of functionalized silicon carbide nanofibers, 8-16 parts of alkaline activator, 11-15 parts of water, and 13-15 parts of quartz sand as raw materials by weight, wherein the functionalized silicon carbide nanofibers are formed by the attachment of silanol groups to the surface of silicon carbide nanofibers; the calcined kaolin in the inorganic powder introduces aluminum elements, which can increase the hydration products of the reaction system; the functionalized silicon carbide nanofibers are combined with the inorganic powder, the inorganic powder can effectively improve the structural density and reduce the porosity, and the functionalized silicon carbide nanofibers undergo a dehydration condensation reaction with the matrix, which can effectively play a bridging role and a filling effect, and can effectively prevent microcracks and micropores caused by freeze-thaw damage and sulfate corrosion damage, thereby achieving the purpose of improving durability.

[0025] In this embodiment, the functionalized silicon carbide nanofiber is prepared by the following method: a thin layer of amorphous oxide is generated on the surface of the silicon carbide nanofiber, and then the amorphous oxide is converted into silanol groups attached to the surface of the silicon carbide nanofiber under acid and alkaline conditions; a thin layer of amorphous oxide is generated on the surface of the silicon carbide nanofiber, and under acidic conditions, the amorphous oxide is converted into a small number of silanol groups; under alkaline conditions, the amorphous oxide is converted into a large number of silanol groups attached to the surface of the silicon carbide nanofiber. Since the surface of the silicon carbide nanofiber has silanol groups, it can undergo a dehydration condensation reaction with the matrix, which can effectively play a bridging role and a filling effect, and can effectively prevent microcracks and micropores caused by freeze-thaw damage and sulfate corrosion damage.

[0026] In this embodiment, the functionalized silicon carbide nanofibers are prepared by the following method: the silicon carbide nanofibers are ultrasonically treated in an acid, washed and dried, and then the dried silicon carbide nanofibers are placed in an alkaline solution and stirred, and finally washed and dried to obtain the functionalized silicon carbide nanofibers; preferably, the acid is hydrochloric acid and the alkali is caustic soda; when treated in the acid, the ultrasound is performed at a temperature of 35-45°C for 25-35 minutes; when treated in the alkali, the stirring is performed at a temperature of 75-85°C for at least 24 hours.

[0027] In this embodiment, the alkaline activator is water glass and sodium hydroxide, and by weight, the water glass is 6-12 parts and the sodium hydroxide is 2-4 parts; the inorganic powder is a mixture of calcined kaolin and granulated blast furnace slag, and by weight, the granulated blast furnace slag is 60-80 parts and the calcined kaolin is 10-20 parts; the addition of calcined kaolin effectively improves the structural density and reduces the porosity; and an appropriate amount of functionalized silicon carbide nanofibers undergo a dehydration condensation reaction with the matrix, effectively playing a bridging role and a filling effect, preventing freeze-thaw damage and sulfate corrosion from affecting the performance of the system.

[0028] In a preferred embodiment, the raw materials include 70 parts of granulated blast furnace slag, 15 parts of calcined kaolin, 0.075 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand in parts by mass.

[0029] In this embodiment, the mesh number of the quartz sand is 150-250 meshes, and the mesh number of the calcined kaolin is 1200-1300 meshes. The calcined kaolin is calcined kaolin, the calcination temperature is generally 700° C., and the calcination time is generally not less than 2 hours.

[0030] This embodiment also discloses a method for preparing an alkali-activated gelling material with improved low-carbon durability, comprising the following steps:

[0031] S1, mixing the functionalized silicon carbide nanofibers with an alkaline activator by magnetic stirring and ultrasonic oscillation to obtain a functionalized silicon carbide nanofiber mixed solution; the magnetic stirring time is controlled to be 15-25 minutes, and then the ultrasonic oscillation is performed at a power of 200 W for at least 10 minutes;

[0032] S2, mixing quartz sand, water, functionalized silicon carbide nanofiber mixed liquid and inorganic powder to prepare an alkali-activated cementitious material with improved low carbon durability.

[0033] Embodiment 1

[0034] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 80 parts of industrial granulated blast furnace slag, 10 parts of calcined kaolin, 0.05 parts of functionalized silicon carbide nanofibers, 6 parts of water glass, 2 parts of sodium hydroxide, 11 parts of water, and 13 parts of quartz sand.

[0035] The preparation method comprises the following steps:

[0036] 1) First, the weighted silicon carbide nanofibers were placed in 0.2M hydrochloric acid and ultrasonicated at 40°C for 30min, washed with a large amount of deionized water, and then dried. The dried silicon carbide nanofibers were then placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers.

[0037] 2) uniformly stirring and mixing industrial granulated blast furnace slag and calcined kaolin for 60 seconds to obtain an inorganic powder mixture; stirring and cooling water glass and sodium hydroxide to room temperature to obtain an alkaline activator, and then adding the functionalized silicon carbide nanofibers to the prepared alkaline activator solution, magnetically stirring and ultrasonically shaking to obtain a functionalized silicon carbide nanofiber mixed solution;

[0038] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0039]

[0040]

[0041] Embodiment 2

[0042] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 80 parts of industrial granulated blast furnace slag, 10 parts of calcined kaolin, 0.10 parts of functionalized silicon carbide nanofibers, 7 parts of water glass, 2 parts of sodium hydroxide, 12 parts of water, and 12 parts of quartz sand.

[0043] The preparation method comprises the following steps:

[0044] 1) The original silicon carbide nanofibers are treated with hydrochloric acid and caustic soda aqueous solution successively to obtain functionalized silicon carbide nanofibers. First, the weighted silicon carbide nanofibers are placed in 0.2M hydrochloric acid, ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried; then the dried portion of silicon carbide nanofibers are placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0045] 2) industrial granulated blast furnace slag and calcined kaolin are uniformly stirred and mixed in proportion for 60 seconds to obtain an inorganic powder mixture; water glass and sodium hydroxide are stirred and cooled to room temperature to obtain an alkaline activator, and then the functionalized silicon carbide nanofibers are added to the prepared alkaline activator solution, and magnetic stirring and ultrasonic vibration are used to mix to obtain a functionalized silicon carbide nanofiber mixed solution;

[0046] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0047]

[0048] Embodiment 3

[0049] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 70 parts of industrial granulated blast furnace slag, 15 parts of calcined kaolin, 0.075 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand.

[0050] The preparation method comprises the following steps:

[0051] 1) The original silicon carbide nanofibers were treated with hydrochloric acid and caustic soda aqueous solution successively to obtain functionalized silicon carbide nanofibers. First, the weighted silicon carbide nanofibers were placed in 0.2M hydrochloric acid, ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried; then the dried silicon carbide nanofibers were placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0052] 2) industrial granulated blast furnace slag and calcined kaolin are uniformly stirred and mixed in proportion for 60 seconds to obtain an inorganic powder mixture; water glass and sodium hydroxide are stirred and cooled to room temperature to obtain an alkaline activator, and then the functionalized silicon carbide nanofibers are added to the prepared alkaline activator solution, and magnetic stirring and ultrasonic vibration are used to mix to obtain a functionalized silicon carbide nanofiber mixed solution;

[0053] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0054]

[0055] Embodiment 4

[0056] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 70 parts of industrial granulated blast furnace slag, 15 parts of calcined kaolin, 0.10 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand.

[0057] The preparation method comprises the following steps:

[0058] 1) The original silicon carbide nanofibers were treated with hydrochloric acid and caustic soda aqueous solution successively to obtain functionalized silicon carbide nanofibers. First, the weighted silicon carbide nanofibers were placed in 0.2M hydrochloric acid, ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried; then the dried silicon carbide nanofibers were placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0059] 2) industrial granulated blast furnace slag and calcined kaolin are uniformly stirred and mixed in proportion for 60 seconds to obtain an inorganic powder mixture; water glass and sodium hydroxide are stirred and cooled to room temperature to obtain an alkaline activator, and then the functionalized silicon carbide nanofibers are added to the prepared alkaline activator solution, and magnetic stirring and ultrasonic vibration are used to mix to obtain a functionalized silicon carbide nanofiber mixed solution;

[0060] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0061]

[0062] Embodiment 5

[0063] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 60 parts of industrial granulated blast furnace slag, 20 parts of calcined kaolin, 0.075 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand.

[0064] The preparation method comprises the following steps:

[0065] 1) The original silicon carbide nanofibers are treated with hydrochloric acid and caustic soda aqueous solution successively to obtain functionalized silicon carbide nanofibers. First, the weighted silicon carbide nanofibers are placed in 0.2M hydrochloric acid, ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried. The dried silicon carbide nanofibers are then placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0066] 2) uniformly stirring and mixing industrial granulated blast furnace slag and calcined kaolin for 60 seconds to obtain an inorganic powder mixture; stirring and cooling water glass and sodium hydroxide to room temperature to obtain an alkaline activator, and then adding the functionalized silicon carbide nanofibers to the prepared alkaline activator solution, magnetically stirring and ultrasonically shaking to obtain a functionalized silicon carbide nanofiber mixed solution;

[0067] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0068]

[0069] Embodiment 6

[0070] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 60 parts of industrial granulated blast furnace slag, 20 parts of calcined kaolin, 0.05 parts of functionalized silicon carbide nanofibers, 11 parts of water glass, 4 parts of sodium hydroxide, 13 parts of water, and 12 parts of quartz sand.

[0071] The preparation method comprises the following steps:

[0072] 1) The weighted silicon carbide nanofibers were placed in 0.2M hydrochloric acid and ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried, and then the dried silicon carbide nanofibers were placed in a 5M caustic soda solution. After stirring at 80°C for 24 hours, they were rinsed with a sufficient amount of deionized water and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0073] 2) uniformly stirring and mixing industrial granulated blast furnace slag and calcined kaolin for 60 seconds to obtain an inorganic powder mixture; stirring and cooling water glass and sodium hydroxide to room temperature to obtain an alkaline activator, and then adding the functionalized silicon carbide nanofibers to the prepared alkaline activator solution, magnetically stirring and ultrasonically shaking to obtain a functionalized silicon carbide nanofiber mixed solution;

[0074] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0075]

[0076] Embodiment 7

[0077] The alkali-activated cementitious material of this embodiment for improving low-carbon durability comprises, by mass, 70 parts of industrial granulated blast furnace slag, 10 parts of calcined kaolin, 0.10 parts of functionalized silicon carbide nanofibers, 10 parts of water glass, 4 parts of sodium hydroxide, 12 parts of water, and 11 parts of quartz sand.

[0078] The preparation method comprises the following steps:

[0079] 1) The original silicon carbide nanofibers are treated with hydrochloric acid and caustic soda aqueous solution successively to obtain functionalized silicon carbide nanofibers. First, the weighted silicon carbide nanofibers are placed in 0.2M hydrochloric acid, ultrasonicated at 40°C for 30 minutes, washed with a large amount of deionized water, and then dried. The dried silicon carbide nanofibers are then placed in a 5M caustic soda solution, stirred at 80°C for 24 hours, rinsed with a sufficient amount of deionized water, and dried at room temperature to obtain functionalized silicon carbide nanofibers;

[0080] 2) uniformly stirring and mixing industrial granulated blast furnace slag and calcined kaolin for 60 seconds to obtain an inorganic powder mixture; stirring and cooling water glass and sodium hydroxide to room temperature to obtain an alkaline activator, and then adding the functionalized silicon carbide nanofibers to the prepared alkaline activator solution, magnetically stirring and ultrasonically shaking to obtain a functionalized silicon carbide nanofiber mixed solution;

[0081] 3) Add quartz sand, water, and a mixture of functionalized silicon carbide nanofibers to the inorganic powder mixture in sequence, stir evenly for 45 seconds to obtain a low-carbon durable alkali-activated cementitious material, and perform mechanical strength, frost resistance, and sodium sulfate corrosion resistance tests after curing for 28 days.

[0082]

[0083] Combined with the above data, it can be seen that the present invention obtains a 28d compressive strength of more than 70MPa and a 28d flexural strength of more than 8MPa, which meets the national standard for mechanical strength. At the same time, lower mass loss rate and strength loss rate were obtained in sulfate corrosion and freeze-thaw cycle tests. This is related to the composite effect of calcined kaolin and functionalized silicon carbide nanofibers. The incorporation of calcined kaolin effectively improves the structural density and reduces the porosity; and the appropriate amount of functionalized silicon carbide nanofibers undergo a dehydration condensation reaction with the matrix, which effectively plays a bridging role and filling effect, preventing freeze-thaw damage and sulfate corrosion from affecting the performance of the system.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. An alkali-activated gelling material for improving low carbon durability, characterized in that: The raw materials include 70-100 parts of inorganic powder, 0.05-0.10 parts of functionalized silicon carbide nanofibers, 8-16 parts of alkaline activator, 11-15 parts of water and 13-15 parts of quartz sand by weight. The functionalized silicon carbide nanofibers are formed by silanol groups attached to the surface of the silicon carbide nanofibers.

2. The alkali-activated gelling material for improving low carbon durability according to claim 1, characterized in that: The functionalized silicon carbide nanofiber is prepared by the following method: a thin layer of amorphous oxide is generated on the surface of the silicon carbide nanofiber, and then the amorphous oxide is converted into silanol groups attached to the surface of the silicon carbide nanofiber under acid and alkali conditions.

3. The alkali-activated gelling material for improving low carbon durability according to claim 2, characterized in that: The functionalized silicon carbide nanofibers are prepared by placing the silicon carbide nanofibers in an acid for ultrasonic treatment, washing and drying, then placing the dried silicon carbide nanofibers in an alkaline solution for stirring, and finally washing and drying to obtain the functionalized silicon carbide nanofibers.

4. The alkali-activated gelling material for improving low carbon durability according to claim 3, characterized in that: The acid is hydrochloric acid, and the base is caustic soda.

5. The alkali-activated gelling material for improving low carbon durability according to claim 1, characterized in that: The alkaline activator is water glass and sodium hydroxide, and by weight, the water glass is 6-12 parts and the sodium hydroxide is 2-4 parts.

6. The alkali-activated gelling material for improving low carbon durability according to claim 5, characterized in that: The inorganic powder is a mixture of calcined kaolin and granulated blast furnace slag, wherein the granulated blast furnace slag is 60-80 parts by weight and the calcined kaolin is 10-20 parts by weight.

7. The alkali-activated gelling material for improving low carbon durability according to claim 5, characterized in that: The raw materials include 70 parts of granulated blast furnace slag, 15 parts of calcined kaolin, 0.075 parts of functionalized silicon carbide nanofibers, 9 parts of water glass, 3 parts of sodium hydroxide, 13 parts of water, and 14 parts of quartz sand in parts by mass.

8. The alkali-activated gelling material for improving low carbon durability according to claim 7, characterized in that: The mesh number of the quartz sand is 150-250 meshes; the mesh number of the calcined kaolin is 1200-1300 meshes.

9. The method for preparing an alkali-activated gelling material with improved low carbon durability according to claim 1, characterized in that: The following steps are involved: S1, mixing the functionalized silicon carbide nanofibers with an alkaline activator by magnetic stirring and ultrasonic oscillation to prepare a functionalized silicon carbide nanofiber mixed solution; S2, mixing quartz sand, water, functionalized silicon carbide nanofiber mixed liquid and inorganic powder to prepare an alkali-activated cementitious material with improved low carbon durability.