Preparation method of silicon dioxide ceramic
Through the modification and degreasing and impregnation of silica powder, combined with high-temperature sintering, the problem of low strength during the molding of 3D printed silica ceramics by adhesive spraying is solved, and high-strength and high-quality ceramic products are achieved.
Patent Information
- Application Number
- CN202411019384.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing silica ceramics are prone to cracks during the adhesive spray 3D printing process, and the strength after sintering is low, so it cannot accurately ensure the quality and performance of the product, especially in the production of large-size special-shaped parts.
By modifying the silica powder and degreasing and impregnating the molded green body, adding an inorganic binder, vitrification of the inorganic binder is made by high-temperature sintering, thereby improving the physical properties and strength of the silica ceramics.
It significantly improves the strength and performance of silica ceramics, solves the crack problems during the molding process, ensures the high strength and quality of the product, and is suitable for the production of large-size special-shaped parts.
Smart Images

Figure BDA0004966752510000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic material preparation, and more specifically, to a preparation process of high-strength silicon dioxide ceramics by binder jetting 3D printing. Background Art
[0002] Silica ceramics are widely used in many fields due to their unique physical and chemical properties. For example, good insulation performance, excellent heat resistance, extremely high hardness and wear resistance enable it to withstand extreme working environments in the aerospace, defense and military fields; good biocompatibility and chemical stability make it a hot topic in the field of medical devices; high insulation, low dielectric constant and low thermal expansion coefficient make it an ideal material in the field of electronics and communications; corrosion resistance and chemical stability make it valuable in the fields of chemical industry and environmental protection.
[0003] At present, the molding methods of silica ceramics mainly rely on compression molding and slip injection molding. Due to mold limitations, low personalization, and defects inside the molded green body, the production and application of large-sized special-shaped silica ceramic products are limited. Binder jet 3D printing technology has become the 3D printing technology with the most promising industrial application prospects due to its advantages such as fast molding, low cost, suitability for large and special components, and environmental friendliness. However, silica ceramics produced using this technology are prone to cracks during the molding process, low strength or almost no strength after sintering, and the quality and performance of the product cannot be accurately guaranteed. Summary of the invention
[0004] Based on this, the present invention aims at the above-mentioned problems and provides a method for preparing high-strength silica ceramics, which improves the physical properties of the silica ceramics by modifying the silica powder and impregnating the formed green body.
[0005] A method for preparing silicon dioxide ceramics comprises the following steps:
[0006] Powder preparation: fully disperse the silicon dioxide powder in anhydrous ethanol, stir, add a sintering aid and mix, and dry to obtain a silicon dioxide mixed powder coated with a sintering aid;
[0007] Green body molding: The obtained silicon dioxide mixed powder is 3D printed by a binder jet and then solidified to obtain a silicon dioxide green body;
[0008] Degreasing and impregnation: The obtained silicon dioxide green body is degreased, and after degreasing, an inorganic binder is added, followed by vacuum impregnation;
[0009] Green body sintering: The silicon dioxide green body after vacuum impregnation is sintered at high temperature to obtain high-strength silicon dioxide ceramic products.
[0010] The silica powder is modified and made into a green body through binder jet 3D printing, which is then immersed in an inorganic binder. The inorganic binder that has penetrated into the green body is vitrified through high-temperature sintering, thereby improving the performance of the silica ceramic and obtaining a high-strength silica ceramic.
[0011] In one embodiment, the degreasing and dipping process may be repeated multiple times.
[0012] Impregnation can penetrate the inorganic binder into the silicon dioxide green body, thereby improving the initial strength of the green body. Repeating the process multiple times can make the penetration depth deeper and the penetration effect better.
[0013] In one embodiment, in the degreasing and dipping step, the degreasing process is as follows:
[0014] Raise the temperature to 200°C at a rate of 1-5°C / min;
[0015] Raise the temperature to 600-1000°C within 250-300 minutes and keep warm for 120-360 minutes.
[0016] By using stepped temperature for degreasing, the binder in the silicon dioxide green body can be effectively removed, which is conducive to the infiltration of inorganic binder. At the same time, the gradient temperature increase can also prevent the green body from cracking and deformation during the degreasing process.
[0017] In one embodiment, in the degreasing impregnation step, the vacuum impregnation adopts a pressure of 20 to 50 KPa and an impregnation time of 30 to 180 minutes.
[0018] Through vacuum pressure and long-term immersion, the inorganic binder can penetrate more evenly and deeper.
[0019] In one embodiment, in the powder preparation step, the mass ratio of the anhydrous ethanol to the silicon dioxide powder is 50-80:50-20; the mass ratio of the silicon dioxide powder to the sintering aid is 85-97:15-3.
[0020] In one embodiment, the sintering aid is a silicate; preferably, the silicate may be sodium silicate or calcium silicate.
[0021] In one embodiment, in the green body forming step, the curing process is as follows:
[0022] Raise the temperature to 70-100°C at a rate of 1-5°C / min and keep warm for 60-180min;
[0023] Raise the temperature to 150-180°C within 60-90 minutes and keep warm for 120-360 minutes.
[0024] In one embodiment, in the green body sintering step, the sintering process is as follows:
[0025] Raise the temperature to 400-500°C at a rate of 1-5°C / min and keep warm for 3-6 hours;
[0026] Then raise the temperature to 1250-1400°C at a rate of 1-5°C / min and keep it at that temperature for 4-6 hours;
[0027] Cool with the furnace.
[0028] In this step, the silicon dioxide green body impregnated in the inorganic binder is sintered at a high temperature, and the inorganic binder impregnated into the green body is vitrified, thereby improving the strength of the green body.
[0029] In one embodiment, in the powder preparation step, the particle size of the obtained silicon dioxide mixed powder is 10 to 120 μm.
[0030] If the powder particle size is too small and too fine, the fluidity is poor, which is not conducive to the subsequent green body molding; if the powder particle size is too large, the pore gap after molding is too large, which affects the density and strength of the subsequent green body after sintering. The particle size of 10-120μm meets the requirements for fluidity and strength of the green body after sintering and has the best performance.
[0031] In one embodiment, in the powder preparation step, the anhydrous ethanol and the silicon dioxide powder are mixed and stirred at room temperature.
[0032] Stirring at room temperature can prolong the mixing and stirring time of silica in anhydrous ethanol, making the powder more dispersible and facilitating uniform mixing with the sintering aid.
[0033] By modifying the silica powder and then impregnating the green body with an inorganic binder, the strength of the silica ceramic is improved, the problem of easy cracking of silica ceramic products is improved, and the performance of the silica ceramic after sintering is improved. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of the present invention, a plurality of embodiments will be given below to describe the present invention more comprehensively. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood. The binder jet 3D printing (3DP or BJ) herein is that the powder spreader lays a layer of powder, and then the print head sprays the binder at the position where the molding is required, and finally prints layer by layer to form a three-dimensional printed product. Herein, the silicon dioxide green body molding method adopts binder jet 3D printing. The D50 in the embodiment represents the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 50%, also called the median diameter. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0035] In one embodiment, the present application provides a method for preparing a silicon dioxide ceramic, comprising the following steps:
[0036] Powder preparation: fully disperse the silicon dioxide powder in anhydrous ethanol, stir, add the sintering aid, mix and dry to obtain the silicon dioxide mixed powder coated with the sintering aid;
[0037] Green body molding: The obtained silicon dioxide mixed powder is 3D printed by a binder jet and then solidified to obtain a silicon dioxide green body;
[0038] Degreasing and impregnation: The obtained silicon dioxide green body is degreased, and after degreasing, an inorganic binder is added, followed by vacuum impregnation;
[0039] Green body sintering: The silicon dioxide green body after vacuum impregnation is sintered at high temperature to obtain high-strength silicon dioxide ceramic products.
[0040] Adding sintering aids to the silica powder for modification makes the modified silica powder have good fluidity and strong bonding, which also lays the foundation for improving the subsequent sintering strength of the green body. The modified powder can be efficiently and accurately obtained by binder jet 3D printing; the green body can be degreased and then immersed in an inorganic binder to allow the inorganic binder to penetrate into the pores of the green body, and then sintered at high temperature to vitrify the inorganic binder, thereby improving the physical properties of silica ceramics.
[0041] The preparation method of the high-strength silica ceramic is described below in conjunction with specific examples to further understand the concept of the preparation method of the high-strength silica ceramic.
[0042] In one embodiment, a method for preparing a high-strength silicon dioxide ceramic comprises the following steps:
[0043] Powder preparation: first disperse the silica powder (raw powder) in anhydrous ethanol, and then stir at room temperature for 30 to 60 minutes to allow the silica powder to be fully dispersed in the anhydrous ethanol; then add the sintering aid powder to obtain a mixture, stir at room temperature for 1 to 2 hours, and after the mixture is dried, obtain a silica mixed powder coated with a sintering aid, and then screen the mixed powder to select a mixed powder with a particle size of 10 to 120 μm for standby use.
[0044] The mass ratio of anhydrous ethanol to silicon dioxide (raw powder) is 50-80:50-20; the mass ratio of silicon dioxide powder to sintering aid is 85-97:15-3. The sintering aid includes but is not limited to various silicates such as sodium silicate and calcium silicate.
[0045] Green body molding: Put the sieved silica mixed powder into the powder spreader of the binder jet 3D printing equipment, and lay a uniform and flat layer of silica modified powder on the 3D printing powder bed through the powder spreading and compacting device. Then the print head sprays the binder evenly on the powder bed surface according to the program settings, and so on, layer by layer until the 3D model is printed. After printing, move the powder bed to the oven for drying and curing. The curing process can be:
[0046] First, the temperature is raised to 70-100°C at a rate of 1-5°C / min and kept at this temperature for 60-180min; then, the temperature is raised to 150-180°C within 60-90min and kept at this temperature for 120-360min; finally, the powder bed is moved to a powder cleaning station to remove excess powder on the surface and inside of the green body to obtain a modified silica green body.
[0047] It should be noted that this step is to improve the initial strength of the silicon dioxide green body and facilitate the removal of the green body for post-processing.
[0048] Degreasing and impregnation: Put the solidified and cleaned silica green body into a crucible, and put the crucible into a vacuum sintering furnace for vacuum degreasing in steps. The degreasing process is mainly to remove the binder in the 3D printing process. The degreasing process adopts a step temperature. The specific process is: heating to 200℃ at a rate of 1-5℃ / min, then heating to 600-1000℃ within 250-300min, and keeping warm for 120-360min.
[0049] After degreasing, add inorganic binder to the crucible until the green body is submerged, and then move the whole body to a vacuum curing furnace and immerse it for 30 to 180 minutes under a vacuum pressure of 20 to 50 KPa. Then degreasing and immersion are repeated 2 to 3 times.
[0050] Green body sintering: Put the impregnated silicon dioxide green body into a crucible, and move the crucible to a box-type high-temperature sintering furnace for sintering. The specific steps of sintering are: heating to 400-500℃ at a rate of 1-5℃ / min and keeping it for 3-6h, then heating to 1250-1400℃ at a rate of 1-5℃ / min and keeping it for 4-6h, and then cooling it with the furnace. At this point, a high-strength silicon dioxide ceramic sintered part can be obtained.
[0051] In order to further illustrate the technical solution of the present application, two specific embodiments are given to facilitate understanding.
[0052] Embodiment 1
[0053] Powder preparation: First, weigh anhydrous ethanol and silicon dioxide powder in a mass ratio of 60:40, and weigh silicon dioxide powder and sintering aid in a mass ratio of 95:5. Disperse silicon dioxide powder in anhydrous ethanol and stir at room temperature for 30 minutes to fully disperse silicon dioxide powder in anhydrous ethanol. Then add calcium silicate powder to anhydrous ethanol mixed with silicon dioxide to form a mixture, and stir at room temperature for 1 hour. After the mixture is dried, screen it with a sieve and select a mixed powder with a particle size of D50 = 30 μm for standby use.
[0054] Green body molding: The silicon dioxide mixed powder with a particle size of D50 = 30 μm is made into a green body by binder jet 3D printing. After the green body is printed, it is moved to an oven for curing. The curing steps are as follows:
[0055] First, the temperature was raised to 80°C at a rate of 3°C / min and kept for 60 minutes, then the temperature was raised to 160°C within 60 minutes and kept for 120 minutes. Finally, the excess powder on the surface and inside of the green body was removed to obtain a modified silicon dioxide ceramic green body.
[0056] Degreasing and impregnation: Place the solidified green body into a crucible, and place the crucible into a vacuum sintering furnace for vacuum degreasing (this process is to remove the 3D printing binder). The degreasing process is as follows: first heat up to 200°C at a rate of 5°C / min, then heat up to 1000°C within 300 minutes, and keep warm for 120 minutes. After degreasing, add inorganic binder to the crucible until the green body is submerged, and then move the crucible containing the green body into a vacuum curing furnace as a whole, and impregnate it at a pressure of 20KPa for 30 minutes. This process is repeated 3 times, namely degreasing-vacuum impregnation-degreasing-vacuum impregnation-degreasing-vacuum impregnation.
[0057] Green body sintering: The impregnated silicon dioxide ceramic green body is moved to a box-type high-temperature sintering furnace for sintering. The sintering process is: heating to 400°C at a rate of 3°C / min and keeping it for 180 minutes, then heating to 1250°C at a rate of 1°C / min and keeping it for 240 minutes, and then cooling with the furnace to obtain silicon dioxide ceramic products.
[0058] Performance testing: The silica ceramic bending test specimens obtained by the above process were placed on a universal testing machine for testing, and the bending strength could reach 15.85 MPa.
[0059] Embodiment 2
[0060] Powder preparation: First, select anhydrous ethanol and silicon dioxide powder in a mass ratio of 70:30, and select silicon dioxide powder and sintering aid in a mass ratio of 85:15. Among them, the sintering aid is sodium silicate. Then disperse the silicon dioxide powder in anhydrous ethanol and stir at room temperature for 30 minutes to make the silicon dioxide powder fully dispersed in the anhydrous ethanol. Then add sintering aid powder to the anhydrous ethanol mixed with silicon dioxide to form a mixture, and stir at room temperature for 30 minutes. After the mixture is dried, screen it with a sieve and select a mixed powder with a particle size of D50 = 70μm for standby use.
[0061] Green body molding: The silicon dioxide mixed powder with a particle size of D50 = 70 μm is made into a green body by binder jet 3D printing. After the green body is printed, it is moved to an oven for curing. The curing steps are as follows:
[0062] First, the temperature was raised to 70°C at a rate of 2°C / min and kept at that temperature for 60 minutes, and then the temperature was raised to 180°C within 80 minutes and kept at that temperature for 180 minutes. Finally, the excess powder on the surface and inside of the green body was removed to obtain a modified silicon dioxide ceramic green body.
[0063] Degreasing and impregnation: Place the solidified green body into a crucible, and place the crucible into a vacuum sintering furnace for degreasing (this process is to remove the 3D printing binder). The degreasing process is as follows: first heat up to 200°C at a rate of 3°C / min, then heat up to 600°C within 250 minutes, and keep warm for 300 minutes. After degreasing, add inorganic binder to the crucible until the green body is submerged, then move the crucible containing the green body into a vacuum curing furnace as a whole, and impregnate it at a pressure of 30KPa for 60 minutes. This process is repeated twice, i.e. degreasing-vacuum impregnation-degreasing-vacuum impregnation.
[0064] Green body sintering: The impregnated silicon dioxide ceramic green body is moved to a box-type high-temperature sintering furnace for sintering. The sintering process is: heating to 500°C at a rate of 2°C / min and keeping the temperature for 180 minutes, then heating to 1400°C at a rate of 3°C / min and keeping the temperature for 240 minutes, and then cooling with the furnace to obtain silicon dioxide ceramic products.
[0065] Performance testing: The silica ceramic bending test specimens obtained by the above process are placed on a universal testing machine for testing, and the bending strength can reach 17MPa.
[0066] In order to intuitively reflect the advantages of the technical solution of the present application, the following table is a comparison of the strength tests of samples at each stage in the silicon dioxide ceramic preparation process of the applicant. The preparation parameters in the table are the same as those in Example 2.
[0067] Table 1 shows the strength comparison of silicon dioxide green body formed by binder jet printing before and after silicon dioxide powder modification. It can be seen from the table that after the silicon dioxide powder is modified, the strength of the tested sample is more than twice that before modification.
[0068] Table 1
[0069] contrast Sample type Bending strength Comparative Example (Original Powder) <![CDATA[As-printed green body of pure SiO2]]> 2MPa Example (modified powder) <![CDATA[SiO2 + sodium silicate green body]]> 5.98MPa
[0070] Table 2 shows the green body formed by 3D printing with binder jet using silica modified powder. The comparative example is direct sintering, and the example is inorganic binder impregnation + sintering. It can be seen from the table that the strength of the sample impregnated with inorganic binder is much higher than that without inorganic binder impregnation. (Note that the samples of the comparative example and the example in the table are consistent with the comparative example except that the example has an inorganic binder impregnation process after degreasing.)
[0071] Table 2
[0072]
[0073] The test results in the above table show that the strength of the green body generated by the modified silica powder in the technical solution of this application is significantly improved compared with that before modification. The green body generated by the modified powder is subsequently impregnated and infiltrated with an inorganic binder, and the strength after sintering is significantly improved compared with the green body not impregnated with an inorganic binder. The strength of the silica ceramics made by the technical solution of this application is significantly improved.
[0074] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0075] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing silicon dioxide ceramics, characterized in that: The following steps are involved: Powder preparation: dispersing silicon dioxide powder in anhydrous ethanol and then adding a sintering aid, mixing and drying to obtain a silicon dioxide mixed powder coated with a sintering aid; Green body molding: The obtained silicon dioxide mixed powder is 3D printed by a binder jet and then solidified to obtain a silicon dioxide green body; Degreasing and impregnation: The obtained silicon dioxide green body is degreased, and after degreasing, an inorganic binder is added, followed by vacuum impregnation; Green body sintering: The silicon dioxide green body after vacuum impregnation is sintered at high temperature to obtain high-strength silicon dioxide ceramic products.
2. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: The degreasing and dipping step may be repeated multiple times.
3. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the degreasing and dipping step, the degreasing process is as follows: Raise the temperature to 200°C at a rate of 1-5°C / min; Raise the temperature to 600-1000°C within 250-300 minutes and keep warm for 120-360 minutes.
4. The method for preparing silicon dioxide ceramics according to claim 3, characterized in that: In the degreasing and impregnation step, the vacuum impregnation adopts a pressure of 20 to 50 KPa and an impregnation time of 30 to 180 minutes.
5. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the powder preparation step, the mass ratio of the anhydrous ethanol to the silicon dioxide powder is 50-80:50-20; the mass ratio of the silicon dioxide powder to the sintering aid is 85-97:15-3.
6. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: The sintering aid is a silicate; preferably, the silicate may be sodium silicate or calcium silicate.
7. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the green molding step, the curing process is as follows: Raise the temperature to 70-100°C at a rate of 1-5°C / min and keep warm for 60-180min; Raise the temperature to 150-180°C within 60-90 minutes and keep warm for 120-360 minutes.
8. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the green body sintering step, the sintering process is as follows: Raise the temperature to 400-500°C at a rate of 1-5°C / min and keep warm for 3-6 hours; Then raise the temperature to 1250-1400°C at a rate of 1-5°C / min and keep it at that temperature for 4-6 hours; Cool with the furnace.
9. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the powder preparation step, the obtained silicon dioxide mixed powder has a particle size of 10 to 120 μm.
10. The method for preparing silicon dioxide ceramics according to claim 1, characterized in that: In the powder preparation step, the anhydrous ethanol and the silicon dioxide powder are mixed and stirred at room temperature.
Citation Information
Patent Citations
Rapid forming method of injection molding infiltration type ceramic-based wave transmission composite from slurry with high solid content and low viscosity
CN107827474A
Method for preparing ceramic through 3D printing forming based on modified Na2SiO3 binder
CN110395995A
Photocuring 3D printing modified ceramic core and preparation method thereof
CN114105621A
Degreasing and sintering method of silicon nitride ceramic powder product
CN116535220A
Ceramic slurries for additive manufacturing techniques
US20190284096A1