Silicon nitride ceramic containing intergranular glass phase wrapped monometal core-shell structure and preparation method thereof

By using the preparation method of intergranular glass phase wrapped single metal core-shell structure in silicon nitride ceramics, the high brittleness and interface thermal mismatch stress of silicon nitride ceramics are solved, and its mechanical properties and wear properties are improved, thus achieving Optimization of material properties.

CN118930280APending Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY +1

Patent Information

Application Number
CN202411158094.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The high brittleness and interfacial thermal mismatch stress of silicon nitride ceramics limit their application in the engineering field. In the prior art, the interface bonding strength is insufficient when forming core-shell structures with multiple metals, which reduces the mechanical properties and wear properties of the material. .

Method used

The preparation method of the intergranular glass phase encapsulates a single metal core-shell structure, and the presintering and liquid phase sintering of the sintering aid powder and the second phase metal powder are formed to form a composite powder with a core-shell structure and silicon nitride powder. Mix and sintering to adjust the interface thermal mismatch stress and improve the mechanical properties and wearability of the material.

Benefits of technology

Effectively improve the mechanical properties and wearability of silicon nitride ceramics, solve the problem of interfacial thermal mismatch stress in silicon nitride ceramics formed by multiple toughened phases, avoid the introduction of impurities, and optimize the comprehensive performance of the material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930280A_ABST
    Figure CN118930280A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silicon nitride ceramic preparation, in particular to silicon nitride ceramic containing an intergranular glass phase wrapped monometal core-shell structure and a preparation method thereof.The preparation method specifically comprises the steps that sintering aid powder and metal powder are pre-sintered at the temperature of 800-1200 DEG C to form composite powder with the core-shell structure, and the composite powder with the core-shell structure is prepared; the preparation method comprises the following steps: mixing a single metal and intergranular glass phase-containing composite powder with silicon nitride powder, and carrying out air pressure sintering to prepare the high-performance silicon nitride ceramic. According to the composite silicon nitride ceramic disclosed by the invention, phase addition is reduced, and meanwhile, a core-shell structure is formed to adjust distribution of interface thermal mismatch stress; the mechanical property and the wear resistance of the silicon nitride ceramic material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon nitride ceramic preparation, and in particular to a silicon nitride ceramic containing a single metal core-shell structure wrapped by an intercrystalline glass phase and a preparation method thereof. Background Art

[0002] Silicon nitride ceramics are a kind of ceramic material with excellent comprehensive performance, with excellent properties such as high temperature resistance, wear resistance, and high strength. However, the high brittleness of silicon nitride ceramics restricts its application in the engineering field. The introduction of second-phase metal particles is a simple and effective method to improve the fracture performance of silicon nitride ceramics. However, there are obvious differences between the second phase and silicon nitride ceramics in terms of thermal expansion coefficient, sintering activity, etc., which will produce thermal mismatch stress near the material interface. Excessive interfacial thermal mismatch stress will cause material defects such as microcracks and pores at the material interface, reducing the strength and wear performance of the material. For example, Zeng Yuping et al. disclosed "A high-toughness silicon nitride ceramic and its preparation method" (publication number CN111517806B). The patent adds at least one of SiC fiber, carbon fiber, graphene, carbon nanotubes and YB2C2 as a second phase on the basis of adding a sintering aid, which only breaks through the limitation of the current Si3N4 composite ceramics using an independent phase as a toughening phase. Qiao Zhuhui et al. disclosed "A silicon nitride ceramic sintered body and its preparation method" (publication number CN115180960B). This patent buries a tungsten-toughened silicon nitride ceramic sintered body in buried powder for heat treatment to produce a carbonization reaction, thereby obtaining the silicon nitride ceramic sintered body; however, C that does not participate in the reaction will exist in the silicon nitride ceramic in a single substance form, becoming a new formation point for material interface defects, and will also reduce the material strength and wear performance. Wu Ning et al. disclosed "A core-shell structure TiB2-based metal ceramic and its preparation method" (publication number CN113106314A). This patent forms a core-shell structure inside the material on the basis of adding multiple second phases such as TiC, WC, Co and Ni, regulates the distribution of interface thermal stress, and inhibits the generation of interface defects to a certain extent. However, TiC, WC, Co and Ni that do not participate in the construction of the core-shell structure exist alone inside the material, becoming a new formation point for material interface defects, and will also reduce the material strength and wear performance.

[0003] In general, there are two main characteristics of the research on Si3N4-based cermets: (1) Most of the research uses one or two or more metals as independent toughening phases to prepare Si3N4-based cermets. (2) Two or more metals form a core-shell structure as a toughening phase or reinforcement phase, but due to the different thermal expansion coefficients of the materials, the bonding strength between the two metals and between Si3N4 and the metal bonding phase is not high enough, which reduces the mechanical properties and wear properties of the material. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a silicon nitride ceramic containing a single metal core-shell structure wrapped by an intercrystalline glass phase and a preparation method thereof. The present invention not only breaks through the limitation of using an independent phase as a toughening phase, but also solves the problem of forming a core-shell structure with multiple toughening phases to form an interface thermal mismatch stress in silicon nitride to reduce the comprehensive performance of the material.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for preparing a silicon nitride ceramic containing a single metal core-shell structure wrapped by an intercrystalline glass phase comprises the following steps:

[0007] The sintering aid powder and the second phase metal powder are used as raw materials, and the composite raw material is obtained by ball milling and mixing; after the composite raw material is pressed into shape, it is pre-sintered in a protective atmosphere, and then crushed. Combined with the XRD phase detection result, it can be seen that a composite powder containing an intercrystalline glass phase core-shell structure is formed, and the second phase metal powder refers to other metal phases except the matrix phase; it can be seen from the figure that W / Cr / Mo still maintains a single substance state in the (Y2O3, Al2O3, W / Cr / Mo) particles, most of the Y2O3 and Al2O3 maintain the initial state, and a small amount of Y2O3 reacts chemically with Al2O3 to form a new substance Y3Al5O 12 It can be seen that during the pre-sintering process, Y2O3 and Al2O3 form a new substance Y3Al5O 12 There is no chemical reaction with the W / Cr / Mo particles, and the W / Cr / Mo particles are encapsulated by generating a liquid phase around the particles.

[0008] The composite powder containing an intercrystalline glass phase core-shell structure is mixed with α-Si3N4 powder, pressed into shape, and then sintered under a protective atmosphere to obtain a silicon nitride ceramic containing a single metal core-shell structure wrapped in an intercrystalline glass phase. Since the melting point of the sintering aid is lower than the melting point of the added metal element, when heated to a certain temperature, the sintering aid powder reacts with the silicon dioxide on the surface of the silicon nitride particles to form a liquid phase, thereby wrapping the metal to form a composite powder containing an intercrystalline glass phase core-shell structure; the sintering of silicon nitride is formed by liquid phase sintering in addition to reaction sintering, and liquid phase sintering is a process in which the sintering aid reacts with SiO2 or oxynitride on the surface of the silicon nitride powder during the sintering process to form a liquid phase, dissolving-precipitating-precipitating β-Si3N4.

[0009] In a preferred embodiment of the present invention, the sintering aid powder is a mixture of oxidizing and non-oxidizing sintering aid powders, the oxidizing sintering aid powder is one of aluminum oxide powder or magnesium oxide powder, and the non-oxidizing sintering aid powder is a rare earth oxide, and the rare earth oxide is one of Y2O3, La2O3, and Yb2O3.

[0010] In a preferred embodiment of the present invention, the mass ratio of the non-oxidizing sintering aid powder, the oxidizing sintering aid powder, and the second phase metal powder is 1-10:1-10:1-10.

[0011] In a preferred embodiment of the present invention, the second phase metal powder is one of tungsten powder, molybdenum powder and chromium powder.

[0012] In a preferred embodiment of the present invention, the mass ratio of the composite powder containing the intercrystalline glass phase core-shell structure to the silicon nitride powder is 1-20:80-99.

[0013] In a preferred embodiment of the present invention, the pre-sintering temperature is 800-1200° C., the pre-sintering heating rate is 1-20° C. / min, and the pre-sintering holding time is 0.5-5 h.

[0014] More preferably, the pre-sintering temperature is 1100-1200° C., and the pre-sintering heating rate is 5-10° C. / min.

[0015] In a preferred embodiment of the present invention, the sintering temperature after pressing is 1600-1800° C., the sintering heating rate after pressing is 1-20° C. / min, and the sintering holding time after pressing is 1-2h.

[0016] More preferably, the sintering temperature after press molding is 1780-1800° C., and the sintering heating rate after press molding is 5-10° C. / min.

[0017] In a preferred embodiment of the present invention, the pressing method is dry pressing and / or isostatic pressing. More preferably, the pressing method is dry pressing followed by isostatic pressing, and the isostatic pressing is cold isostatic pressing.

[0018] In a preferred embodiment of the present invention, the dry pressing pressure is 10 to 50 MPa, and the isostatic pressing pressure is 200 to 300 MPa.

[0019] In a preferred embodiment of the present invention, the protective atmosphere is nitrogen, and the gas pressure is ≥1MPa, wherein the high N2 pressure during gas pressure sintering can avoid the decomposition of silicon nitride at high temperature (above 1780°C), improve the sintering activity, and is conducive to densification and grain growth.

[0020] In a preferred embodiment of the present invention, the mixed powder is mixed evenly in a ball mill, the medium is anhydrous ethanol and zirconium oxide balls, the material is dried at 60-100° C., and finally ground and sieved, and the sieve mesh number is 20-100 mesh.

[0021] In a preferred embodiment of the present invention, the purity of yttrium oxide powder, aluminum oxide powder and metal powder are all 99.95% and the particle size is 1 micron.

[0022] Another object of the present invention is to provide a silicon nitride ceramic having a single metal core-shell structure encapsulated by an intercrystalline glass phase, which is prepared by any of the preparation methods described above.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention first pre-sinters the sintering aid powder and the metal powder at 800-1200° C. to form a composite powder with a core-shell structure, then mixes the composite powder containing a single metal@intercrystalline glass phase with silicon nitride powder, and prepares high-performance silicon nitride ceramics by gas pressure sintering. The composite silicon nitride ceramics of the present invention form a core-shell structure while reducing the addition of physical phases, thereby adjusting the distribution of interfacial thermal mismatch stress, and effectively improving the mechanical properties and wear resistance of silicon nitride ceramic materials. It not only breaks through the limitation of using an independent physical phase as a toughening phase, but also solves the problem of using multiple toughening phases to form a core-shell structure to form an interfacial thermal mismatch stress in silicon nitride ceramics to reduce the comprehensive performance of the material.

[0025] 2. The method of preparing high-performance silicon nitride ceramics containing a single metal @ intercrystalline glass phase core-shell structure of the present invention uses sintering aids such as Al2O3 / Y2O3 as the outer layer of the core-shell structure, which effectively avoids the introduction of other impurities. Compared with the core-shell structure formed by multiple metals, it can effectively regulate the interface thermal stress mismatch and achieve the purpose of optimizing the mechanical properties and wear properties of silicon nitride ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic structural diagram of a single metal@intercrystalline glass phase core-shell structure composite material in Example 1 of the present invention;

[0027] Figure 2 is a flow chart for preparing the silicon nitride ceramic of the present invention;

[0028] Figure 3 SEM images of silicon nitride samples prepared by (a) introducing tungsten particles alone and (b) introducing tungsten-intercrystalline glass phase core-shell structure in Example 1 of the present invention;

[0029] Figure 4 SEM images of silicon nitride samples prepared by (a) introducing chromium particles alone and (b) introducing chromium-intercrystalline glass phase core-shell structure in Example 2 of the present invention;

[0030] Figure 5 SEM images of silicon nitride samples prepared by (a) introducing molybdenum particles alone and (b) introducing molybdenum-intercrystalline glass phase core-shell structure in Example 3 of the present invention;

[0031] Figure 6 This is the XRD spectrum of Y2O3, Al2O3, W / Cr, and Mo particles after pre-sintering of the silicon nitride ceramic prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0034] Example 1

[0035] A method for preparing high-performance silicon nitride ceramics containing a single metal@intercrystalline glass phase core-shell structure, comprising the following steps:

[0036] (1) 5 wt% yttrium oxide powder, 5 wt% aluminum oxide powder and 5 wt% tungsten powder are mixed to obtain a uniformly mixed powder;

[0037] (2) placing the mixed powder obtained in step (1) into a graphite mold, keeping the temperature at 1200° C. for 0.5 h under a nitrogen protective atmosphere, with a heating rate of 3° C. / min. After sintering, cool the mixture to room temperature with the furnace and take out the sample. The sintered block is crushed into powder by a crusher, and then mixed with 85 wt% of silicon nitride powder to obtain a uniformly mixed composite powder;

[0038] (3) The composite powder obtained in step (2) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, it is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain high-performance silicon nitride ceramics. The preparation flow chart is as follows: Figure 2 As shown, the fracture toughness of the material is 9.1MPa·m 1 / 2 , material bending strength is 1038MPa, material wear rate is 1.19×10 -6 mm 3 ·N -1 ·m -1 .

[0039] Example 2

[0040] A method for preparing high-performance silicon nitride ceramics containing a single metal@intercrystalline glass phase core-shell structure, comprising the following steps:

[0041] (1) mixing 5 wt% of yttrium oxide powder, 5 wt% of aluminum oxide powder and 5 wt% of chromium powder to obtain a uniformly mixed powder;

[0042] (2) placing the mixed powder obtained in step (1) into a graphite mold, keeping the temperature at 1200° C. for 0.5 h under a nitrogen protective atmosphere, with a heating rate of 3° C. / min. After sintering, cool the mixture to room temperature with the furnace and take out the sample. The sintered block is crushed into powder by a crusher, and then mixed with 85 wt% of silicon nitride powder to obtain a uniformly mixed composite powder;

[0043] (3) The composite powder obtained in step (2) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, the composite powder is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain a high-performance silicon nitride ceramic with a fracture toughness of 9.5 MPa·m 1 / 2 , material bending strength is 1160MPa, material wear rate is 1.03×10 -6 mm 3 ·N -1 ·m -1 .

[0044] Example 3

[0045] A method for preparing high-performance silicon nitride ceramics containing a single metal@intercrystalline glass phase core-shell structure, comprising the following steps:

[0046] (1) mixing 5 wt% of yttrium oxide powder, 5 wt% of aluminum oxide powder and 5 wt% of molybdenum powder to obtain a uniformly mixed powder;

[0047] (2) placing the mixed powder obtained in step (1) into a graphite mold, keeping the temperature at 1200° C. for 0.5 h under a nitrogen protective atmosphere, with a heating rate of 3° C. / min. After sintering, cool the mixture to room temperature with the furnace and take out the sample. The sintered block is crushed into powder by a crusher, and then mixed with 85 wt% of silicon nitride powder to obtain a uniformly mixed composite powder;

[0048] (3) The composite powder obtained in step (2) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, the composite powder is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain a high-performance silicon nitride ceramic with a fracture toughness of 9.6 MPa·m 1 / 2 , material bending strength is 1096MPa, material wear rate is 1.14×10 -6 mm 3 ·N -1 ·m -1 .

[0049] Example 4

[0050] A method for preparing high-performance silicon nitride ceramics containing a single metal@intercrystalline glass phase core-shell structure, comprising the following steps:

[0051] (1) 5 wt% yttrium oxide powder, 5 wt% aluminum oxide powder and 5 wt% tungsten powder are mixed to obtain a uniformly mixed powder;

[0052] (2) placing the mixed powder obtained in step (1) into a graphite mold, keeping the temperature at 800° C. for 0.5 h under a nitrogen protective atmosphere, with a heating rate of 1° C. / min. After sintering, cool the mixture to room temperature with the furnace and take out the sample. The sintered block is crushed into powder by a crusher, and then mixed with 80 wt % of silicon nitride powder to obtain a uniformly mixed composite powder;

[0053] (3) The composite powder obtained in step (2) is dry-pressed at a pressure of 10 MPa, and then cold isostatically pressed at a pressure of 250 MPa. The obtained green body is placed in a graphite mold and sintered at 1600°C under a N2 atmosphere, wherein the heating rate is 1°C / min, the N2 pressure is 4 MPa, and the holding time is 1.5 h. After the sintering is completed, it is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature in the furnace to obtain a high-performance silicon nitride ceramic.

[0054] Example 5

[0055] A method for preparing high-performance silicon nitride ceramics containing a single metal@intercrystalline glass phase core-shell structure, comprising the following steps:

[0056] (1) 5 wt% yttrium oxide powder, 5 wt% aluminum oxide powder and 5 wt% tungsten powder are mixed to obtain a uniformly mixed powder;

[0057] (2) placing the mixed powder obtained in step (1) into a graphite mold, and keeping the temperature at 1000° C. for 0.5 h under a nitrogen protective atmosphere, with a heating rate of 20° C. / min. After sintering, cool the sample to room temperature with the furnace, and then take out the sample. The sintered block is crushed into powder by a crusher, and then mixed with 99wt% silicon nitride powder to obtain a uniformly mixed composite powder;

[0058] (3) The composite powder obtained in step (2) is dry-pressed at a pressure of 50 MPa, and then cold isostatically pressed at a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1800°C under a N2 atmosphere, wherein the heating rate is 20°C / min, the N2 pressure is 4 MPa, and the holding time is 1 h. After the sintering is completed, it is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature in the furnace to obtain a high-performance silicon nitride ceramic.

[0059] Comparative Example 1

[0060] A method for preparing silicon nitride ceramics comprises the following steps:

[0061] (1) 5 wt% of yttrium oxide powder, 5 wt% of aluminum oxide powder, 5 wt% of tungsten powder and 85 wt% of silicon nitride powder are mixed to obtain a uniformly mixed powder;

[0062] (2) The mixed powder obtained in step (1) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, the mixed powder is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain a silicon nitride ceramic with a fracture toughness of 9.6 MPa·m 1 / 2 , material bending strength is 820MPa, material wear rate is 1.49×10 -6 mm 3 ·N -1 ·m -1 .

[0063] Comparative Example 2

[0064] A method for preparing silicon nitride ceramics comprises the following steps:

[0065] (1) 5 wt% of yttrium oxide powder, 5 wt% of aluminum oxide powder, 5 wt% of chromium powder and 85 wt% of silicon nitride powder are mixed to obtain a uniformly mixed powder;

[0066] (2) The mixed powder obtained in step (1) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, the mixed powder is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain a silicon nitride ceramic with a fracture toughness of 9.8 MPa·m 1 / 2 , material bending strength is 925MPa, material wear rate is 1.28×10 -6 mm 3 ·N -1 ·m -1 .

[0067] Comparative Example 3

[0068] A method for preparing silicon nitride ceramics comprises the following steps:

[0069] (1) 5 wt% of yttrium oxide powder, 5 wt% of aluminum oxide powder, 5 wt% of molybdenum powder and 85 wt% of silicon nitride powder are mixed to obtain a uniformly mixed powder;

[0070] (2) The mixed powder obtained in step (1) is dry pressed under a pressure of 20 MPa, and then cold isostatically pressed under a pressure of 250 MPa. The obtained green blank is placed in a graphite mold and sintered at 1780°C under a N2 atmosphere, wherein the heating rate is 10°C / min, the N2 pressure is 4 MPa, and the holding time is 2 h. After the sintering is completed, the mixed powder is cooled to 1200°C at a cooling rate of 10°C / min, and then cooled to room temperature with the furnace to obtain a silicon nitride ceramic with a fracture toughness of 10.1 MPa·m 1 / 2 , material bending strength is 916MPa, material wear rate is 1.32×10 -6 mm 3 ·N -1 ·m -1 .

[0071] Results Analysis

[0072] Figure 1 This is a schematic structural diagram of a single metal@intercrystalline glass phase core-shell structure composite material prepared by the present invention, wherein the shell is the intercrystalline glass phase and the core is a single metal.

[0073] Figure 3The SEM images of the silicon nitride samples prepared by (a) introducing tungsten particles alone and (b) introducing tungsten-intercrystalline glass phase core-shell structure prepared in Example 1 of the present invention show that the gray-white color is the metal tungsten element, and the gray-black color around it is the intercrystalline glass phase that wraps the metal. The results show that the liquid phase gathered around the metal particles solidifies to form an intercrystalline glass phase, which wraps the tungsten particles and finally forms a core-shell structure in the silicon nitride ceramic material. The bonding surface is well connected, and there is no generation of defects such as pores, which adjusts the distribution of the interface thermal mismatch stress.

[0074] Figure 4 SEM images of silicon nitride samples prepared in Example 2 of the present invention (a) by introducing chromium particles alone, and (b) by introducing a chromium-intercrystalline glass phase core-shell structure. It can be seen from the figure that the gray-black color in the middle is metallic chromium alone, and the circle around it is the intercrystalline glass phase that wraps the metal. The results show that the liquid phase gathered around the metal particles solidifies to form an intercrystalline glass phase, which wraps the chromium particles, and finally forms a core-shell structure in the silicon nitride ceramic material with good bonding surfaces, without the generation of defects such as pores, and adjusts the distribution of interfacial thermal mismatch stress.

[0075] Figure 5 SEM images of silicon nitride samples prepared in Example 3 of the present invention (a) by introducing molybdenum particles alone, and (b) by introducing a molybdenum-intercrystalline glass phase core-shell structure. It can be seen from the figure that the grayish white color is metallic molybdenum alone, and the circle around it is the intercrystalline glass phase that wraps the metal. The results show that the liquid phase gathered around the metal particles solidifies to form an intercrystalline glass phase, which completes the wrapping of the molybdenum particles, and finally forms a core-shell structure in the silicon nitride ceramic material with good bonding surfaces, without the generation of defects such as pores, and adjusts the distribution of interfacial thermal mismatch stress.

[0076] Figure 6 The XRD spectrum of the Y2O3, Al2O3, W / Cr, and Mo particles after pre-sintering of the silicon nitride ceramic prepared in Example 1 of the present invention, combined with the XRD phase detection results, it can be seen that a composite powder containing an intercrystalline glass phase core-shell structure is formed after pre-sintering; it can be seen from the figure that W / Cr / Mo still maintains a single substance state in the (Y2O3, Al2O3, W / Cr / Mo) particles, most of the Y2O3 and Al2O3 maintain the initial state, and a small amount of Y2O3 reacts chemically with Al2O3 to form a new substance Y3Al5O 12 It can be seen that during the pre-sintering process, Y2O3 and Al2O3 form a new substance Y3Al5O 12 There is no chemical reaction with the W / Cr / Mo particles, and the W / Cr / Mo particles are encapsulated by generating a liquid phase around the particles.

[0077] In summary, the present invention first pre-sinters the sintering aid powder and the metal powder at 800-1200° C. to form a composite powder with a core-shell structure, and then mixes the composite powder containing a single metal@intercrystalline glass phase with silicon nitride powder, and prepares high-performance silicon nitride ceramics by gas pressure sintering. The composite silicon nitride ceramics of the present invention form a core-shell structure while reducing the addition of physical phases, thereby adjusting the distribution of interfacial thermal mismatch stress, and effectively improving the mechanical properties and wear resistance of silicon nitride ceramic materials. It not only breaks through the limitation of using an independent physical phase as a toughening phase, but also solves the problem of using a plurality of toughening phases to form a core-shell structure to form an interfacial thermal mismatch stress in silicon nitride ceramics to reduce the comprehensive performance of the material.

[0078] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0079] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a silicon nitride ceramic having a single metal core-shell structure encapsulated by an intercrystalline glass phase, It is characterized in that The following steps are involved: Sintering aid powder and metal powder are used as raw materials, and ball milling is performed to mix the raw materials to obtain composite raw materials; After the composite raw material is pressed into shape, it is pre-sintered and crushed in a protective atmosphere to form a composite powder containing an intercrystalline glass phase core-shell structure; The composite powder containing an intercrystalline glass phase core-shell structure is mixed with silicon nitride powder, pressed into shape, and then sintered under a protective atmosphere to obtain a silicon nitride ceramic containing an intercrystalline glass phase-encapsulated single metal core-shell structure.

2. The method for preparing the silicon nitride ceramic containing a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The sintering aid powder is a mixture of oxidizing and non-oxidizing sintering aid powders, the oxidizing sintering aid powder is one of aluminum oxide powder and magnesium oxide powder, and the non-oxidizing sintering aid powder is rare earth oxide.

3. The method for preparing the silicon nitride ceramic containing a single metal core-shell structure wrapped by an intercrystalline glass phase according to claim 2, It is characterized in that The mass ratio of the non-oxidizing sintering aid powder, the oxidizing sintering aid powder and the metal powder is 1-10:1-10:1-10.

4. The method for preparing the silicon nitride ceramic containing a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The metal powder is one of tungsten powder, molybdenum powder and chromium powder.

5. The method for preparing the silicon nitride ceramic containing a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The mass ratio of the composite powder containing the intercrystalline glass phase core-shell structure to the silicon nitride powder is 1-20:80-99.

6. The method for preparing the silicon nitride ceramics containing a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The pre-sintering temperature is 800-1200° C., and the pre-sintering heating rate is 1-20° C. / min.

7. The method for preparing the silicon nitride ceramics containing a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The sintering temperature after pressing and molding is 1600-1800°C, the sintering heating rate after pressing and molding is 1-20°C / min, and the sintering holding time after pressing and molding is 1-2h.

8. The method for preparing the silicon nitride ceramics having a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 1, It is characterized in that The pressing method is dry pressing and / or isostatic pressing.

9. The method for preparing the silicon nitride ceramics having a single metal core-shell structure encapsulated by an intercrystalline glass phase according to claim 8, It is characterized in that The dry pressing pressure is 10-50 MPa, and the isostatic pressing pressure is 200-300 MPa.

10. A silicon nitride ceramic having a single metal core-shell structure encapsulated by an intercrystalline glass phase, obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A high-toughness silicon nitride ceramic and its preparation method

    CN111517806B

  • TiB2-based metal ceramic with core-shell structure and preparation method of TiB2-based metal ceramic

    CN113106314A

  • A silicon nitride ceramic sintered body and its preparation method

    CN115180960B

  • Anti-abrasion metal-ceramic composite product and preparation method thereof

    CN103418790A

  • Ceramic / metal high-temperature packaging material of gradient structure and preparing method thereof

    CN108620594A

Cited By

  • Silicon nitride ceramic for high-power electric heating element and low-temperature normal-pressure sintering preparation method of silicon nitride ceramic

    CN121449436A

  • Tungsten-silicon nitride toughened ceramic material as well as preparation method and application thereof

    CN122277263A