Silicon nitride ceramic based on DLP-3D printing and preparation method thereof

By preferring photosensitive resin and dispersant, combined with ball milling, a high solid-phase content and low viscosity silicon nitride ceramic slurry is formed. DLP-3D printing and pneumatic sintering technology are used to solve the poor performance of DLP-3D printing silicon nitride ceramics. The problem of this problem is to realize the preparation of silicon nitride ceramics with high density and high mechanical properties, which promotes its development in practical applications.

CN118930281APending Publication Date: 2024-11-12SHANGHAI INST OF TECH

Patent Information

Application Number
CN202410988727.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

DLP-3D printing technology makes it difficult to prepare silicon nitride ceramics with high mechanical properties, mainly due to the difference in refractive index between resin and ceramic powder, high absorbance, low curing depth, and high viscosity of ceramic slurry with high solid phase content The problem of difficulty in forming uniformly.

Method used

The preferred photosensitive resin and dispersant are used, combined with silicon nitride powder and photoinitiator, and the silicon nitride ceramic slurry with high solid phase content and low viscosity are formed by ball milling, and then pneumatic sintering is performed after DLP-3D printing. Silicon nitride ceramics with high density and high mechanical properties are obtained.

Benefits of technology

The preparation of silicon nitride ceramics with a relative density of up to 96.35% and a flexural strength of 650.19MPa was achieved, which made up for the shortcomings of poor DLP-3D printing performance and promoted the development of silicon nitride ceramics in practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930281A_ABST
    Figure CN118930281A_ABST
Patent Text Reader

Abstract

The invention relates to silicon nitride ceramic based on DLP-3D printing and a preparation method thereof, silicon nitride ceramic slurry comprises the following components in parts by mass: 60-80 parts of silicon nitride powder, 10-30 parts of photosensitive resin, 1-10 parts of dispersing agent and 0.1-5 parts of photoinitiator; the photosensitive resin is a mixture of monofunctional resin, bifunctional resin and trifunctional resin. The preparation method comprises the following steps: uniformly mixing and stirring photosensitive resin, a dispersing agent and silicon nitride powder, adding silicon nitride grinding balls, carrying out ball milling, adding a photoinitiator, continuously carrying out ball milling to obtain silicon nitride ceramic slurry, and carrying out DLP-3D printing and cleaning to obtain a silicon nitride ceramic green body; and performing degreasing and degumming treatment on the silicon nitride ceramic green body, and performing air pressure sintering to obtain the silicon nitride ceramic. Compared with the prior art, the stable silicon nitride photosensitive slurry with high solid content and low viscosity can be formed, and the silicon nitride ceramic with excellent mechanical properties can be obtained through DLP-3D printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon nitride ceramic preparation, and in particular to a silicon nitride ceramic based on DLP-3D printing and a preparation method thereof. Background Art

[0002] Silicon nitride (Si3N4) ceramics are the ceramics with the best comprehensive performance among nitride ceramics. They not only have the excellent comprehensive properties inherent in ceramic materials, such as high strength, high fracture toughness, high temperature resistance, oxidation resistance and low thermal expansion coefficient, but also have relatively low dielectric constant and dielectric loss. This unique advantage makes it shine in aerospace and other fields. For example, by taking advantage of its excellent dielectric properties, good thermal shock resistance and high temperature stability, it can be applied to aircraft and new missile antenna covers after being processed by sealing, coating and other processes, thus being favored by material researchers at home and abroad, and has now become one of the important candidate materials for ultra-wideband wave-transmitting materials. In addition, due to the excellent mechanical properties and good thermal conductivity of silicon nitride ceramics, it perfectly meets the high performance requirements of semiconductor power devices and packaging materials for ceramic substrate materials in the electronics industry. The research and development and large-scale batch production of high thermal conductivity silicon nitride substrate materials have become the general trend of the current industry. For example, leading companies such as Toshiba Materials and Electrical Chemistry in Japan are competing to propose business plans to expand and increase the production capacity of high thermal conductivity silicon nitride ceramic substrates.

[0003] Silicon nitride ceramics, with its excellent comprehensive performance in all aspects, plays a vital role in many fields and has become an indispensable material in the development of modern science and technology. The huge application prospects and possible economic benefits have made nitride ceramic materials a research hotspot worldwide. However, after the ceramic materials are prepared, they usually need to be processed before they can be applied to high-tech industries. Ceramic materials have poor machinability. Although a variety of processing technologies have emerged, they are inefficient, costly, and difficult to guarantee processing quality, and have become a bottleneck restricting their widespread application.

[0004] The emergence of 3D printing technology, also known as additive manufacturing (AM), has provided new ideas for the preparation of Si3N4 ceramic parts with complex shapes and structures. Additive manufacturing includes a series of processes to manufacture three-dimensional (3D) parts by adding materials layer by layer directly from computer-based 3D model data. This alternative to traditional training processes is attracting the interest of the ceramic industry to create geometrically complex parts with almost net shapes without the use of expensive tools. Ceramic materials are used in different fields such as automobiles, aerospace, biomedicine, luxury goods, electronics, casting molds and chips. Due to their special properties, such as hardness, high strength, high fracture toughness, high temperature and good thermal shock resistance, they have a wide range of applications, but compared with polymers and metal materials, the implementation of ceramic material additive manufacturing technology is much slower, so it is difficult to manufacture parts with good resolution and mechanical properties compared with traditional ceramic manufacturing processes. Considering the economic aspects, ceramic parts usually start from a powder mixture with or without binders and other additives, and are formed into the desired shape using conventional techniques, including injection molding, compression molding, tape casting, gel casting, etc., and unlike traditional methods, the total cost of each piece of additive manufacturing technology is independent of the geometric complexity of the component. This has also attracted the attention of the industry, because many applications of ceramic parts require low production volumes, so additive manufacturing can be a particularly practical and economical solution to replace traditional molding processes. Many studies have reported the application of different additive manufacturing technologies in the manufacture of ceramic parts, such as fused deposition modeling (FDM), layered object manufacturing (LOM), stereolithography (SLA), selective laser sintering (SLS) and digital light processing (DLP). Stereolithography based on point scanning and digital light processing based on image projection both use the photocuring reaction of photosensitive resin in ceramic slurry to complete layer-by-layer printing. The difference is that SLA is a photocuring technology based on scanning the surface of ceramic slurry with a point light source to achieve curing, while DLP uses a digital surface projection device and has a larger area and higher efficiency for whole-area material polymerization and curing than a point light source. The photocuring technology based on surface exposure enables DLP technology to ensure the molding accuracy of the printed body while also ensuring the molding efficiency.

[0005] Although DLP-3D printing technology has obvious advantages, there are many difficulties in the preparation of silicon nitride ceramics. It is difficult to obtain silicon nitride ceramics with high mechanical properties through DLP-3D printing. The main difficulties are:

[0006] (1) When the refractive index difference between the resin and the ceramic powder is large, the lateral solidification area tends to increase slightly during the molding process. This behavior is also called over-curing, which is extremely detrimental to the precision of the ceramic blank formed by the photocuring technology. In addition, due to the scattering of energy, the energy used for curing is also reduced, which also has a great impact on the curing depth. Silicon nitride powder has a higher refractive index (n = 2.1), but the refractive index of the resin is generally around 1.35 to 1.55. The large difference in refractive index between the two is not conducive to DLP-3D printing of silicon nitride ceramics. It is necessary to select a suitable resin to reduce the difference in refractive index.

[0007] (2) Si3N4 ceramics have high absorbance. High powder absorbance is another unfavorable factor in the preparation of Si3N4 ceramics using photocuring molding technology. High absorbance will cause the exposure energy acting on the slurry to be lost, resulting in low curing depth or even failure to cure during the printing process. It is necessary to select the color of silicon nitride powder and choose lighter-colored silicon nitride powder to reduce the negative impact of absorbance.

[0008] (3) Ceramic slurry with high solid content is one of the prerequisites for preparing ceramic parts with high density and excellent mechanical properties. Low solid content will cause cracking, collapse and large shrinkage deformation of the ceramic body during the debinding stage. The solid content of ceramic slurry should be kept above 40 vol%, but ceramic slurry with high solid content often has high viscosity, which is not conducive to the forming process of the body. Ceramic slurry for photocuring additive manufacturing has a shear rate of 30s -1 The viscosity should be lower than 5Pa·s to ensure that the ceramic slurry can be evenly coated on the surface of the previous layer during the molding process. However, since the surface of the ceramic powder contains hydrophilic hydroxyl groups, it has poor affinity with the hydrophobic resin, which makes it difficult to evenly disperse the ceramic powder in the photosensitive resin and increase the solid content. This makes it difficult to evenly disperse the ceramic powder in the photosensitive resin, making it difficult to prepare a high-solid-phase, low-viscosity photosensitive ceramic slurry and to prepare silicon nitride ceramics with high mechanical properties.

[0009] In the face of the above difficulties, existing methods usually adopt powder processing or select powders with larger particle size to improve the curing depth and slurry fluidity, but these two methods generally have adverse effects on the product: the powder processing method generally has harsh conditions, which not only complicates the process and increases the cost, but also has a great impact on the quality of later firing, and is accompanied by problems such as environmental pollution; and the powder particle size directly affects the final product mechanical properties. The selection of powders with larger particle size is also accompanied by severe sintering bending. These methods will have an adverse effect on DLP printing. Summary of the invention

[0010] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a silicon nitride ceramic based on DLP-3D printing and a preparation method thereof, so as to obtain a silicon nitride ceramic sample with high density and high mechanical properties.

[0011] The purpose of the present invention can be achieved by the following technical solutions:

[0012] One of the technical solutions of the present invention is to provide a silicon nitride ceramic slurry, characterized in that it includes a photosensitive resin, a dispersant, a silicon nitride powder, and a photoinitiator, which are calculated by mass as follows: 60 to 80 parts of silicon nitride powder, 10 to 30 parts of photosensitive resin, 1 to 10 parts of dispersant, and 0.1 to 5 parts of photoinitiator; the photosensitive resin is a mixture of a monofunctional resin, a difunctional resin, and a trifunctional resin.

[0013] Furthermore, the silicon nitride mixed powder comprises a main powder of silicon nitride (Si3N4) and a sintering aid of alumina (Al2O3) and yttrium trioxide (Y2O3).

[0014] Furthermore, the initial particle size of the Si3N4 is 0.3-1.2 μm, the initial particle size of the Al2O3 is 0.1-0.8 μm, and the initial particle size of the Y2O3 is 0.6-2 μm;

[0015] The mass ratio of Si3N4, Al2O3, and Al2O3 is (25-40):1:(0.5-3).

[0016] Further, the monofunctional resin includes dicyclopentenyl acrylate (DCPA) and cyclotrimethylolpropane formal acrylate (CTFA);

[0017] The bifunctional resin includes hydroxyethyl methacrylate (HEMA) and acryloyl morpholine (ACMO);

[0018] The trifunctional resin includes trimethylolpropane triacrylate (TMPTA), pentaerythritol triacrylate (PET3A), trimethylolpropane trimethacrylate (TMPTMA), propoxylated glycerol triacrylate (GPTA), and tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA).

[0019] Furthermore, the mass ratio of the monofunctional resin, the difunctional resin and the trifunctional resin is 1:(0.5-2):(0.5-2).

[0020] Furthermore, the dispersant includes a combination of one or more of a modified polyolefin solution, an acrylic copolymer solution, a fluorosilicone polymer solution, and a phosphate ester solution.

[0021] Further, the photoinitiator includes one or more combinations of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (photoinitiator TPO), phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide (photoinitiator 819), bis (1- (2,4-difluorophenyl) -3-pyrrolyl) titanocene (photoinitiator 784), and 2-phenylbenzyl-2-dimethylamine-1- (4-morpholinobenzylphenyl) butanone (photoinitiator 369).

[0022] One of the technical solutions of the present invention is to provide a method for preparing silicon nitride ceramic slurry, comprising mixing and stirring a photosensitive resin, a dispersant, and a silicon nitride powder to obtain a mixed suspension; adding silicon nitride grinding balls to the mixed suspension, ball milling, adding a photoinitiator, and continuing ball milling to obtain a silicon nitride ceramic slurry.

[0023] Furthermore, the ball milling time is 4 to 12 hours, and the ball milling time is continued for 1 to 3 hours.

[0024] Furthermore, the photosensitive resin and the dispersant are mixed and stirred, and the silicon nitride powder is added in small amounts and multiple times and mixed and stirred.

[0025] Furthermore, the mass ratio of the added amount of silicon nitride grinding balls to the silicon nitride mixed powder is 1 to 3:1.

[0026] The second technical solution of the present invention is to provide a method for preparing silicon nitride ceramics based on DLP-3D printing, which uses the above-mentioned silicon nitride ceramic slurry as a raw material, performs DLP-3D printing, and obtains a silicon nitride ceramic green body after cleaning; the silicon nitride ceramic green body is degreased and debinded, and gas pressure sintered to obtain silicon nitride ceramics, and the reaction is completed.

[0027] Furthermore, the specific process of the DLP-3D printing is: using silicon nitride ceramic slurry as raw material, adding it into the material box of the DLP-3D printer, preparing the sample model to be printed, importing the model into the printing software, adjusting the printing parameters of the DLP-3D printer to control the exposure conditions for printing, and after printing, removing the printed sample from the printing platform and cleaning it with alcohol. The cleaned sample is a silicon nitride ceramic green body, which is stored in a light-shielding black sealed bag.

[0028] Furthermore, the exposure intensity of the DLP-3D printing is 20 to 100 mW / cm 2 The exposure time is 4 to 12 seconds; the temperature of the degreasing and debinding treatment is 400 to 600° C., the temperature of the gas pressure sintering is 1600 to 1900° C., and the sintering time is 2 to 10 hours.

[0029] The third technical solution of the present invention is to provide a silicon nitride ceramic based on DLP-3D printing, which is prepared by the above-mentioned preparation method.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] (1) After using the preferred photosensitive resin mixed liquid, the number of functional groups directly affects the crosslinking density and viscosity of the resin. Single-functional group and bifunctional group resins can meet the low viscosity requirements required for printing due to their small molecular weight, while trifunctional group resins contain more active groups that can participate in the reaction. Not only does the photocuring rate fast, but the high crosslinking density can also improve the degree of three-dimensional network crosslinking during curing, thereby obtaining a green body with higher strength. By optimizing the mixed selection of photosensitive resins and rationally allocating the advantages of photosensitive resins with different functional groups, the green body can achieve good interlayer crosslinking effects while having a certain toughness. The silicon nitride ceramics finally prepared have high relative density and excellent mechanical properties. Compared with the previous DLP-3D printed samples, its relative density is about 90% and its flexural strength is about 200-450MPa. The silicon nitride ceramics prepared by the present invention have a relative density of up to 96.35% and a bending strength of up to 650.19 MPa, which makes up for the shortcomings of poor performance of DLP-3D printed silicon nitride and greatly promotes the further development of silicon nitride ceramics in practical applications.

[0032] (2) The surface of silicon nitride ceramic powder contains hydrophilic hydroxyl groups, which have poor affinity with hydrophobic resins. This makes it difficult to evenly disperse the ceramic powder in the photosensitive resin, making it difficult to prepare a high-solid-phase, low-viscosity photosensitive ceramic slurry. The present invention reduces the mutual attraction of silicon nitride ceramic powder in the slurry by optimizing the type of photosensitive resin and adjusting the proportion of each component added, so that the particles are less agglomerated, and the silicon nitride powder with more hydroxyl groups forms a stable solidification depth of 50 Vol%, a high solid content, low viscosity silicon nitride ceramic photosensitive slurry with a viscosity of 4000-7000 mPa·s. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the preparation process of the silicon nitride ceramic slurry shown in Example 1;

[0034] Figure 2 Schematic diagram of the preparation process of the silicon nitride ceramic shown in Example 7;

[0035] Figure 3 This is a picture of the finished product of the silicon nitride ceramic prepared in Example 7. DETAILED DESCRIPTION

[0036] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the given embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0037] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art.

[0038] In the following examples, DCPA, CAS No. 12542-30-2, was purchased from Youming (Shanghai) Chemical Co., Ltd.; CTFA, brand EM212, was purchased from Changxing Chemical Industry Co., Ltd.; HEMA, brand HEMA, was purchased from Wanhua Chemical Co., Ltd.; TMPTA, brand 2811, was purchased from Covestro; PET3A, brand BM3235, was purchased from Boxing New Materials Technology Co., Ltd.; TMPTMA, CAS No. 3290-92-4, was purchased from Shanghai McLean Biochemical Technology Co., Ltd. The dispersant, acrylic copolymer solution, brand CPD-07, and modified polyolefin solution, brand CPD-01, were all purchased from Jiaxing Raoji Technology Co., Ltd. The photoinitiator, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819), brand S70431, was purchased from Shanghai Yuanye Biotechnology Co., Ltd., and 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone (photoinitiator 369), brand Omnirad 369, was purchased from IGM.

[0039] Example 1

[0040] A silicon nitride ceramic slurry is prepared by the following steps: Figure 1 As shown:

[0041] (1) Weigh 76 parts of silicon nitride powder, 18 parts of photosensitive resin, 4 parts of dispersant, and 2 parts of photoinitiator by mass. The photosensitive resin is a mixture of DCPA, HEMA, and PET3A, and the mass ratio thereof is 1:1:1.

[0042] The DCPA in the resin is a monofunctional resin, the HEMA is a bifunctional resin, and the PET3A is a trifunctional resin. The silicon nitride powder is a mixture of Si3N4, Al2O3 and Y2O3, and the mass ratio is 94:3:3. The dispersant is a modified polyolefin solution. The photoinitiator is photoinitiator 819.

[0043] (2) The DCPA, HEMA and PET3A measured in step (1) are mixed and stirred, a dispersant is added and mixed and stirred, and the measured silicon nitride mixed powder is added in small amounts and multiple times and mixed and stirred to obtain a mixed suspension.

[0044] (3) Adding silicon nitride grinding balls with a size of 5 mm to the mixed suspension, the mass ratio of the silicon nitride grinding balls to the silicon nitride mixed powder is 1.5:1, then placing it on a rolling ball mill, rolling ball milling at a speed of 80 r / min for 6 h, adding photoinitiator 819, and continuing ball milling for 1 h to obtain silicon nitride ceramic slurry.

[0045] Example 2

[0046] (1) Weigh 76 parts of silicon nitride powder, 18 parts of photosensitive resin, 4 parts of dispersant, and 2 parts of photoinitiator by mass. The photosensitive resin is a mixture of CTFA, HEMA, and TMPTA, and the mass ratio is 1:1:1. The CTFA in the resin is a monofunctional resin, HEMA is a difunctional resin, and PET3A is a trifunctional resin. The silicon nitride powder is a mixture of Si3N4, Al2O3, and Y2O3, and the mass ratio is 94:3:3. The dispersant is an acrylic copolymer solution. The photoinitiator is photoinitiator 369.

[0047] (2) The CTFA, HEMA and TMPTA measured in step (1) are mixed and stirred, a dispersant is added and mixed and stirred, and the silicon nitride mixed powder is added in small amounts and multiple times and mixed and stirred to obtain a mixed suspension.

[0048] (3) Adding silicon nitride grinding balls with a size of 5 mm to the mixed suspension, the mass ratio of the silicon nitride grinding balls to the silicon nitride mixed powder is 2:1, then placing it on a rolling ball mill, rolling ball milling at a speed of 80 r / min for 6 h, adding photoinitiator 369, and continuing ball milling for 1 h to obtain silicon nitride ceramic slurry.

[0049] Example 3

[0050] (1) Weigh 76 parts of silicon nitride powder, 18 parts of photosensitive resin, 4 parts of dispersant, and 2 parts of photoinitiator by mass. The photosensitive resin is a mixture of CTFA, ACMO, and TMPTMA, and the mass ratio is 1:1:1. The CTFA in the resin is a monofunctional resin, ACMO is a difunctional resin, and TMPTMA is a trifunctional resin. The silicon nitride powder is a mixture of Si3N4, Al2O3, and Y2O3, and the mass ratio is 94:3:3. The dispersant is an acrylic copolymer solution. The photoinitiator is photoinitiator 369.

[0051] (2) The CTFA, ACMO and TMPTMA measured in step (1) are mixed and stirred, a dispersant is added and mixed and stirred, and the silicon nitride mixed powder is added in small amounts and multiple times and mixed and stirred to obtain a mixed suspension.

[0052] (3) Adding silicon nitride grinding balls with a size of 5 mm to the mixed suspension, the mass ratio of the silicon nitride grinding balls to the silicon nitride mixed powder is 2:1, then placing it on a rolling ball mill, rolling ball milling at a speed of 80 r / min for 6 h, adding photoinitiator 369, and continuing ball milling for 1 h to obtain silicon nitride ceramic slurry.

[0053] Example 4

[0054] Compared with Example 1, most of them are the same, except that the mass ratio of DCPA, HEMA and PET3A is adjusted to 1:1:2.

[0055] Example 5

[0056] Compared with Example 1, most of them are the same, except that the mass ratio of DCPA, HEMA and PET3A is adjusted to 1:1:0.5.

[0057] Example 6

[0058] Compared with Example 1, most of them are the same, except that the mass ratio of DCPA, HEMA and PET3A is adjusted to 1:0.5:1.

[0059] Example 7

[0060] Compared with Example 1, most of them are the same, except that the mass ratio of DCPA, HEMA and PET3A is adjusted to 1:2:1.

[0061] Example 8

[0062] Compared with Example 1, most of the contents are the same, except that 60 parts of silicon nitride powder, 30 parts of photosensitive resin, 5 parts of dispersant, and 5 parts of photoinitiator are weighed by mass.

[0063] Example 9

[0064] Compared with Example 1, most of the contents are the same, except that 80 parts of silicon nitride powder, 10 parts of photosensitive resin, 9.9 parts of dispersant, and 0.1 parts of photoinitiator are weighed by mass.

[0065] Example 10

[0066] Compared with Example 1, most of the contents are the same, except that 75 parts of silicon nitride powder, 21 parts of photosensitive resin, 1 part of dispersant, and 3 parts of photoinitiator are weighed by mass.

[0067] Embodiment 11

[0068] Compared with Example 1, most of the contents are the same, except that 69 parts of silicon nitride powder, 19 parts of photosensitive resin, 10 parts of dispersant, and 2 parts of photoinitiator are weighed by mass.

[0069] Example 12

[0070] Compared with Example 1, most of the above are the same, except that the silicon nitride powder is a mixture of Si3N4, Al2O3 and Y2O3, and the mass ratio thereof is adjusted to 92:5:3.

[0071] Example 13

[0072] Compared with Example 1, most of the above are the same, except that the silicon nitride powder is a mixture of Si3N4, Al2O3 and Y2O3, and the mass ratio thereof is adjusted to 50:2:1.

[0073] Embodiment 14

[0074] Compared with Example 1, most of the above are the same, except that the silicon nitride powder is a mixture of Si3N4, Al2O3 and Y2O3, and the mass ratio thereof is adjusted to 40:1:3.

[0075] Embodiment 15

[0076] A silicon nitride ceramic based on DLP-3D printing is realized by the following steps: Figure 2 As shown:

[0077] (1) Pour the silicon nitride ceramic slurry prepared in Example 1 into a material tank of a printer;

[0078] (2) Prepare the sample model to be printed, import the model into the printing software, adjust the printing parameters of the DLP-3D printer to control the exposure conditions of the printing, and print out the required silicon nitride ceramic semi-finished product. The printing conditions are an exposure intensity of 50mW / cm 2 , exposure time 8s;

[0079] (3) After printing is completed, the printed silicon nitride ceramic semi-finished product is removed from the printing platform, cleaned with alcohol until a silicon nitride ceramic green body is obtained, and stored in a light-shielding black sealed bag;

[0080] (4) The obtained silicon nitride ceramic green body is first degreased and debinded in air to 500°C for 2 hours, and then sintered in a gas pressure furnace to 1750°C for 2 hours to obtain a silicon nitride ceramic with high density and high mechanical strength. Figure 3 shown.

[0081] Example 16

[0082] Compared with Example 15, most of the steps are the same, except that the slurry used in step (1) is changed to the silicon nitride ceramic slurry of Example 2, and the exposure intensity in step (2) is adjusted to 30 mW / cm 2 , the exposure time is adjusted to 10s; the temperature of degreasing and debinding in step (4) is adjusted to 500℃, the holding time is 2h, and the temperature of gas pressure sintering is adjusted to 1800℃, the holding time is 2h.

[0083] Embodiment 17

[0084] Compared with Example 15, most of the above are the same, except that the exposure intensity in step (2) is adjusted to 25 mW / cm 2 , the exposure time is adjusted to 10s; the temperature of degreasing and debinding in step (4) is adjusted to 550°C, the holding time is 2h, and the temperature of gas pressure sintering is adjusted to 1800°C, the holding time is 4h.

[0085] Embodiment 18

[0086] (1) Pour the silicon nitride ceramic slurry prepared in Example 3 into the material tank of the printer;

[0087] (2) Prepare the sample model to be printed, import the model into the printing software, adjust the printing parameters of the DLP-3D printer to control the exposure conditions of the printing, and print out the required silicon nitride ceramic semi-finished product. The printing conditions are an exposure intensity of 50mW / cm 2 , exposure time 8s;

[0088] (3) After printing is completed, the printed silicon nitride ceramic semi-finished product is removed from the printing platform, cleaned with alcohol until a silicon nitride ceramic green body is obtained, and stored in a light-shielding black sealed bag;

[0089] (4) The obtained silicon nitride ceramic green body is first degreased and debinded in air to 450°C for 2 hours, and then sintered in a gas pressure furnace to 1750°C for 4 hours to obtain a silicon nitride ceramic with high density and high mechanical strength. Figure 3 shown.

[0090] Embodiment 19

[0091] Compared with Example 15, most of the steps are the same, except that the exposure intensity in step (2) is adjusted to 45 mW / cm 2 , the exposure time is adjusted to 10s; the temperature of degreasing and debinding in step (4) is adjusted to 500°C, the holding time is 1h, and the temperature of gas pressure sintering is adjusted to 1800°C, the holding time is 2h.

[0092] Embodiment 20

[0093] Compared with Example 15, most of the steps are the same, except that the temperature of degreasing and debinding in step (4) is adjusted to 550°C and the holding time is 2 hours, and the temperature of gas pressure sintering is adjusted to 1800°C and the holding time is 4 hours.

[0094] Embodiment 21

[0095] Compared with Example 15, most of the steps are the same, except that the temperature of degreasing and debinding in step (4) is adjusted to 550°C and the holding time is 2 hours, and the temperature of gas pressure sintering is adjusted to 1800°C and the holding time is 4 hours.

[0096] Embodiment 22

[0097] Compared with Example 15, most of the contents are the same, except that the temperature of degreasing and debinding in step (4) is adjusted to 400°C and the holding time is 2 hours, and the temperature of gas pressure sintering is adjusted to 1600°C and the holding time is 6 hours.

[0098] Embodiment 23

[0099] Compared with Example 15, most of the contents are the same, except that the temperature of degreasing and debinding in step (4) is adjusted to 600°C and the holding time is 2 h, and the temperature of gas pressure sintering is adjusted to 1900°C and the holding time is 2 h.

[0100] Embodiment 24

[0101] Compared with Example 15, most of the steps are the same, except that the exposure intensity in step (2) is adjusted to 20 mW / cm 2 , the exposure time is adjusted to 12s.

[0102] Embodiment 25

[0103] Compared with Example 15, most of the steps are the same, except that the exposure intensity in step (2) is adjusted to 100 mW / cm 2 , the exposure time is adjusted to 4s.

[0104] Comparative Example 1

[0105] Compared with Example 1, most of the steps are the same, except that the photosensitive resin mixture in step (1) is changed to CTFA and HEMA, with a mass ratio of 1:1.5. The CTFA in the resin is a monofunctional resin, and the HEMA is a difunctional resin.

[0106] Comparative Example 2

[0107] Compared with Example 15, most of the above are the same, except that when the silicon nitride ceramic slurry prepared in Comparative Example 1 is poured into the material cylinder of the printer, no formed silicon nitride ceramic can be obtained.

[0108] Comparative Example 3

[0109] Compared with Example 1, most of the steps are the same, except that the photosensitive resin mixture in step (1) is changed to CTFA. The CTFA in the resin is a monofunctional resin.

[0110] Comparative Example 4

[0111] Compared with Example 15, most of the above are the same, except that when the silicon nitride ceramic slurry prepared in Comparative Example 3 is poured into the material cylinder of the printer, no formed silicon nitride ceramic can be obtained.

[0112] The performance tests of Examples 15 to 20 and the prepared silicon nitride ceramics were carried out to test their relative density and flexural strength. The density was measured by the Archimedean drainage method, and the flexural strength was measured by the three-point bending method. The test standard of the three-point bending method was the national standard "Fine Ceramics Flexural Strength Test Method" (GB / T6569-2006). The final test results are shown in Table 1.

[0113] Table 1 Performance test results of silicon nitride ceramics

[0114] Relative density (%) Flexural strength(MPa) Embodiment 15 96.35 650.19 Example 16 95.81 625.51 Embodiment 17 95.99 631.81 Embodiment 18 95.13 605.30 Embodiment 19 96.08 641.99 Embodiment 20 94.94 592.82

[0115] As can be seen from Table 1, the silicon nitride ceramics prepared by the present invention have high relative density and excellent mechanical properties for DLP-3D printed samples. And through Examples 15 to 20 and Comparative Examples 1 to 4, it can be found that when only monofunctional resins, monofunctional resins and bifunctional resins are added, the obtained silicon nitride ceramic slurry has poor curing performance and cannot be formed when it is subjected to DLP-3D. This is because compared with the addition of monofunctional and bifunctional photosensitive resins, the addition of trifunctional groups greatly increases the cross-linking points of the slurry system, and a dense cross-linking network can be quickly formed during the printing process, so that the prepared sample has high interlayer bonding. By selecting the types of photosensitive resins and dispersants and adjusting the addition ratio of each component, the mutual attraction of silicon nitride ceramic powders in the slurry is weakened, the particles are less agglomerated, and silicon nitride ceramic slurry with high solid content and low viscosity is prepared. In summary, the present invention makes up for the shortcomings of poor performance of DLP-3D printing of silicon nitride, and greatly promotes the further development of silicon nitride ceramics in practical applications.

[0116] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A silicon nitride ceramic slurry, characterized in that: It includes photosensitive resin, dispersant, silicon nitride powder and photoinitiator, which are calculated by weight as follows: 60-80 parts of silicon nitride powder, 10-30 parts of photosensitive resin, 1-10 parts of dispersant and 0.1-5 parts of photoinitiator; The photosensitive resin is a mixture of monofunctional resin, bifunctional resin and trifunctional resin.

2. The silicon nitride ceramic slurry according to claim 1, characterized in that: The silicon nitride mixed powder comprises a mixed powder of main powder Si3N4 and sintering aids Al2O3 and Y2O3.

3. The silicon nitride ceramic slurry according to claim 2, characterized in that: The initial particle size of Si3N4 is 0.3-1 μm, the initial particle size of Al2O3 is 0.1-0.8 μm, and the initial particle size of Al2O3 is 0.6-2 μm; The mass ratio of Si3N4, Al2O3, and Al2O3 is (25-40):1:(0.5-3).

4. The silicon nitride ceramic slurry according to claim 1, characterized in that: The monofunctional resin includes DCPA and CTFA; The bifunctional resin includes HEMA and ACMO; The trifunctional resins include TMPTA, PET3A, TMPTMA, GPTA, and THEICTA.

5. The silicon nitride ceramic slurry according to claim 1, characterized in that: The mass ratio of the monofunctional resin, the bifunctional resin and the trifunctional resin is 1:(0.5-2):(0.5-2).

6. The silicon nitride ceramic slurry according to claim 1, characterized in that: The dispersant includes a combination of one or more of a modified polyolefin solution, an acrylic copolymer solution, a fluorosilicone polymer solution, and a phosphate ester solution; The photoinitiator includes one or more combinations of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, bis (1- (2,4-difluorophenyl) -3-pyrrolyl) titanocene, and 2-phenylbenzyl-2-dimethylamine-1- (4-morpholinobenzylphenyl) butanone.

7. A method for preparing a silicon nitride ceramic slurry according to any one of claims 1 to 6, characterized in that: The photosensitive resin mixed liquid, dispersant and silicon nitride powder are mixed and stirred evenly to obtain a mixed suspension; silicon nitride grinding balls are added to the mixed suspension for ball milling, and after adding a photoinitiator, the ball milling is continued to obtain a silicon nitride ceramic slurry.

8. A method for preparing silicon nitride ceramics based on DLP-3D printing, characterized in that: The silicon nitride ceramic slurry according to any one of claims 1 to 6 is used as a raw material, DLP-3D printing is performed, and a silicon nitride ceramic green body is obtained after cleaning; the silicon nitride ceramic green body is degreased and debinded, and gas pressure sintering is performed to obtain silicon nitride ceramics, and the preparation is completed.

9. The method for preparing silicon nitride ceramics based on DLP-3D printing according to claim 8, characterized in that: The exposure intensity of the DLP-3D printing is 20-100 mW / cm 2 The exposure time is 4 to 12 seconds, the temperature of the degreasing and debinding treatment is 400 to 600° C., the temperature of the gas pressure sintering is 1600 to 1900° C., and the sintering time is 2 to 10 hours.

10. A silicon nitride ceramic based on DLP-3D printing, characterized in that: The preparation method is described in claim 8 or 9.

Citation Information

Patent Citations

  • Photosensitive resin-based carbon source / silicon carbide ceramic slurry, method for preparing porous carbon / silicon carbide green body, structural member and preparation method of structural member

    CN111116205A

  • Aluminum oxide ceramic slurry for photocuring 3D printing, preparation method and aluminum oxide ceramic

    CN114075069A

  • Zirconium oxide ceramic slurry, preparation method, application and zirconium oxide ceramic

    CN116751054A

  • Preparation method of 3D printing oil-containing ceramic lubricating composite material with porous structure

    CN117466633A

  • Silicon nitride ceramic generation method based on photocuring 3D printing

    CN118344159A

Cited By

  • 3D printing ceramic slurry, preparation method and application thereof, and preparation method of silicon nitride ceramic

    CN119430955A

  • Bone ingrowth type integrated silicon nitride ceramic acetabular cup for total hip arthroplasty

    CN121015961A