Pelletizing method of silicon nitride or aluminum nitride ceramic powder

By optimizing the process flow, including the selection and treatment of raw materials and additives, the problem of low pelletization efficiency of silicon nitride and aluminum nitride ceramic powders is solved, and efficient pelletization and excellent molding and sintering performance are achieved.

CN118930287APending Publication Date: 2024-11-12ZHONGYUAN CRITICAL METAL LAB
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410924508.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The pelletization efficiency of existing silicon nitride and aluminum nitride ceramic powders is low, which affects the forming and sintering properties of the material.

Method used

By optimizing the process flow, including raw material selection and pretreatment, additive selection and introduction, mixing and granulation, pelletization treatment and subsequent detection, we ensure the high purity of the powder, uniform particle size and uniform distribution of appropriate additives, and control pelletization and sintering parameters to achieve efficient pelletization.

Benefits of technology

The pelletization efficiency of silicon nitride and aluminum nitride ceramic powders is improved, and the pellets with excellent performance are obtained, which solves the problem of low pelletization efficiency and achieves efficient molding and sintering.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic powder raw material pelletizing methods, in particular to a silicon nitride or aluminum nitride ceramic powder pelletizing method which comprises the following steps: raw material selection and pretreatment, raw material selection and purchase, and drying and screening. Additive selection and introduction, including selection of additive types and selection of additive introduction modes; mixing and granulating; pelletizing treatment is conducted, specifically, the pelletized pellets are subjected to pre-sintering treatment and then subjected to main sintering; carrying out subsequent processing and detection; the pelletizing method for the silicon nitride or aluminum nitride ceramic powder, provided by the invention, has the beneficial effects that the optimal pelletizing effect of the silicon nitride or aluminum nitride ceramic powder is obtained by optimizing the working procedures of the existing method; the problem of low pelletizing efficiency of the existing silicon nitride and aluminum nitride ceramic powder is further solved; and the pelletizing method of the silicon nitride or aluminum nitride ceramic powder can be efficiently realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic powder raw material pelletizing method, in particular to a pelletizing method for silicon nitride or aluminum nitride ceramic powder. Background Art

[0002] The pelletization of silicon nitride (Si3N4) or aluminum nitride (AlN) ceramic powder is an important process, which aims to improve the fluidity, bulk density and subsequent sintering performance of the powder. The pelletized powder is easier to form and sinter, thereby preparing silicon nitride and aluminum nitride ceramic materials with excellent performance.

[0003] In the prior art, during the entire pelletization process, it is necessary to strictly control the process parameters and operating conditions of each step to ensure that the quality and performance of the pellets are stable and reliable; at the same time, it is also necessary to promptly analyze and deal with problems arising in the pelletization process to improve the efficiency and success of pelletization.

[0004] To this end, we need a method for pelletizing silicon nitride or aluminum nitride ceramic powders to solve the problem of low pelletizing efficiency of existing silicon nitride and aluminum nitride ceramic powders; a method for pelletizing silicon nitride or aluminum nitride ceramic powders that can efficiently achieve pelletizing. Summary of the invention

[0005] The object of the present invention is to provide a method for pelletizing silicon nitride or aluminum nitride ceramic powders to solve the problem of low pelletizing efficiency of existing silicon nitride and aluminum nitride ceramic powders proposed in the above background technology; a method for pelletizing silicon nitride or aluminum nitride ceramic powders can be efficiently realized.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for pelletizing silicon nitride or aluminum nitride ceramic powder, the method comprising the following steps:

[0007] Raw material selection and pretreatment, raw material selection and procurement, as well as drying and screening;

[0008] Selection and introduction of additives, including selection of additive types and methods of additive introduction;

[0009] Mixing and granulation;

[0010] Pelletizing treatment, pre-burning the pellets after granulation and then main sintering;

[0011] Subsequent processing and testing: After the sintered pellets are cooled and crushed, performance testing is carried out.

[0012] Preferably, the specific operations of raw material selection and pretreatment include:

[0013] Raw material selection and procurement: According to product performance and process requirements, high-purity silicon nitride or aluminum nitride ceramic powders with uniform particle size distribution are selected to ensure that the raw materials are free of impurities, agglomerates, and have good fluidity;

[0014] Drying and screening: Dry the selected powder to remove moisture and volatile impurities. The drying temperature and time are adjusted according to the characteristics of the powder to avoid powder agglomeration or oxidation. After drying, use screening equipment to grade the powder to ensure that the powder size meets the pelletization requirements.

[0015] Preferably, the specific operations of selecting and introducing the additives include:

[0016] Selection of additives: According to the characteristics of the powder and the requirements of pelletization, select binders, sintering aids and dispersants to improve the fluidity of the powder, increase the strength of the pellets and promote densification during the sintering process;

[0017] Additive introduction method: Additives are introduced into the powder by dry mixing or wet mixing. During the mixing process, it is necessary to ensure that the additives are evenly distributed in the powder to avoid local concentrations that are too high or too low.

[0018] Preferably, the specific operations of mixing and granulating include:

[0019] Mixing process: the pretreated powder is mixed with the additives evenly. During the mixing process, stirring and ball milling are used to ensure that the powder and the additives are fully contacted and mixed evenly;

[0020] Granulation method: according to product requirements and production scale, one of the granulation methods of spray drying and extrusion granulation is selected. During the granulation process, the rotation speed, pressure and temperature parameters of the granulator are controlled to obtain pellets of uniform size and regular shape; the average particle size of the raw material powder is 1.2-1.5 microns; the specific surface area is 2.3-2.9m2 / g; the oxygen content is 0.85%;

[0021] Granulation index: Particle size: ≤80 mesh accounts for 100%, 80-200 mesh accounts for 30%; 200-325 mesh accounts for 10%; 325-400 mesh accounts for 15%; ≤400 mesh accounts for 30-35%.

[0022] Preferably, the specific operations of the pelletization treatment include:

[0023] Pre-burning treatment: the pellets after granulation are pre-burned to remove residual moisture and organic additives in the pellets and make the pellet structure more compact. The pre-burning temperature and time are adjusted according to the characteristics of the powder and the type of additives;

[0024] The main sintering is carried out in a controlled atmosphere, and the pellets are further densified by heating to improve their strength and stability. The sintering temperature, time and atmosphere parameters have an important influence on the performance of the pellets and should be optimized according to the specific situation.

[0025] Preferably, the specific operations of the subsequent processing and detection include:

[0026] Cooling and crushing: the sintered pellets are cooled, crushed or ground to adjust the particle size distribution of the pellets; during the crushing process, the crushing force and particle size range are controlled to obtain the pellet size that meets the requirements;

[0027] Performance testing: density, hardness, and compressive strength tests are conducted on the pellets to ensure that they meet the use requirements; chemical composition analysis and microstructure observation and testing methods are conducted to fully understand the performance and quality status of the pellets. For unqualified pellets, the cause analysis is conducted and corresponding measures are taken to improve them.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The pelletizing method of silicon nitride or aluminum nitride ceramic powder proposed in the present invention obtains the best pelletizing effect of silicon nitride and aluminum nitride ceramic powder by optimizing the process of the existing method; further solves the problem of low pelletizing efficiency of existing silicon nitride and aluminum nitride ceramic powders; and can efficiently realize the pelletizing method of silicon nitride or aluminum nitride ceramic powder. DETAILED DESCRIPTION

[0030] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1

[0032] The present invention provides a technical solution: a method for pelletizing silicon nitride or aluminum nitride ceramic powder, the method comprising the following steps:

[0033] 1. Raw material selection and pretreatment, including raw material selection and procurement, as well as drying and screening;

[0034] Detailed description of the specific operation:

[0035] Raw material selection and procurement:

[0036] Performance and process requirements analysis: First, we need to have an in-depth understanding of the product performance, including its hardness, strength, corrosion resistance, etc. At the same time, we also need to analyze the characteristics of the pelletizing process, such as molding temperature, sintering time, etc., to determine the specific requirements for raw materials.

[0037] Raw material purity and particle size considerations: Based on the above analysis, we need to select high-purity silicon nitride and aluminum nitride ceramic powders to ensure the purity and performance of the final product; taking aluminum nitride ceramic powder as an example, the oxygen content of aluminum nitride ceramic powder is <0.6wt.%; carbon content is <4000ppm; iron content is <15ppm, silicon content is <40ppm, calcium content is <300ppm, and specific surface area is ≥2.5m 2 / g. At the same time, the particle size distribution of the raw materials is also critical. Uniform particle size distribution helps to uniformly mix and shape the powder in the subsequent pelletization process.

[0038] Raw material fluidity assessment: The fluidity of raw materials is also important for the pelletization process. Powders with good fluidity are easier to handle during mixing and molding.

[0039] Raw material procurement and quality inspection: After determining the raw material specifications, purchase the raw materials from reliable suppliers and conduct strict quality inspections on the raw materials to ensure that they are free of impurities and lumps.

[0040] Drying and sieving:

[0041] Drying treatment: Drying equipment selection: According to the characteristics of the raw materials and the production scale, select suitable ovens, dryers, etc.

[0042] Drying temperature and time control: According to the characteristics of the powder, set the appropriate drying temperature and time. Too low temperature or insufficient time may lead to incomplete drying, while too high temperature or too long time may cause powder agglomeration or oxidation.

[0043] Ambient humidity control: During the drying process, keep the ambient humidity at a low level to prevent the powder from reabsorbing moisture during the drying process.

[0044] Screening operation: Screening equipment selection and debugging: Select screening equipment suitable for the powder particle size range, such as vibrating screen, rotary screen, etc.

[0045] Particle size classification: According to the requirements of the pelletization process for the powder particle size, the sieve aperture is set to 50 microns to 150 microns. The dried powder is passed through the screening equipment for particle size classification to remove oversized or undersized particles to ensure that the powder particle size meets the process requirements.

[0046] Screening effect check: Check the particle size distribution of the screened powder to ensure that it meets the process requirements. If necessary, adjust the screen aperture or screening time to obtain better screening effect.

[0047] 2. Additive selection and introduction, including the selection of additive types and the method of introducing additives; specific operations:

[0048] Additive type selection:

[0049] Analyze powder properties: First, deeply understand the physical and chemical properties of the silicon nitride and aluminum nitride ceramic powders used, and select one or more of the following additives: polyvinyl alcohol (PVA), polystyrene (PS), phenolic resin (PF), polymethyl acrylate (PMA), beeswax (BW), etc.

[0050] Determine the pelletization requirements: According to the product performance requirements and production process, clarify the strength, density, sintering properties and other indicators required for pelletization.

[0051] Choose the right additive:

[0052] Binder: Choose a binder that can effectively combine with powder particles to improve the agglomeration of powder and the strength of pellets. Common binders include organic binders and inorganic binders. Organic binders such as polyvinyl alcohol and polyvinyl butyral have good wettability and adhesion and are suitable for a variety of powders; inorganic binders such as silicates and phosphates have the advantages of high temperature resistance and chemical corrosion resistance and are suitable for applications in high temperature or special environments.

[0053] Sintering aid: Select sintering aids that can reduce the sintering temperature and promote grain growth and densification during the sintering process. These additives help improve the sintering performance of the pellets and the performance of the final product. The sintering aid is selected from at least one of magnesium oxide, aluminum oxide, and calcium oxide.

[0054] Dispersant: When it is necessary to improve the fluidity of the powder, an appropriate dispersant can be selected. The dispersant can reduce the agglomeration force between the powder particles, making it easier to mix and shape. At least one of sodium dodecyl sulfate (SDS), sodium polyacrylate (PAAS), methyl amyl alcohol, cellulose derivatives and triethylhexyl phosphoric acid (TEHP) can be selected.

[0055] Additive introduction method:

[0056] Dry mixing method: Place the selected additives and powder in a certain proportion into a mixing device such as a blender or ball mill.

[0057] During the mixing process, ensure that the speed and time of the mixing equipment are appropriate so that the additives and powders are fully in contact and evenly mixed.

[0058] Check the mixing effect regularly to ensure that the additives are evenly distributed in the powder and there is no local concentration that is too high or too low.

[0059] Wet mixing method: Mix the additive with an appropriate amount of solvent (such as water or organic solvent) to form a slurry.

[0060] The slurry and the powder can be mixed by stirring, kneading, etc.

[0061] During the wet mixing process, pay attention to controlling the amount of solvent and mixing time to ensure that the additives and powders are fully mixed, while avoiding problems in the pelletization process caused by excessive solvent.

[0062] Whether dry mixing or wet mixing, the dosage and mixing conditions of additives need to be strictly controlled to ensure that the additives can be evenly distributed in the powder and play the expected effect. At the same time, attention should be paid to the compatibility and safety of additives and powders to avoid the introduction of impurities or components that have a negative impact on the pelletization process or the performance of the final product.

[0063] In the process of selecting and introducing additives, multiple tests and adjustments may be required to obtain the best type and dosage of additives, as well as the best way of introduction. This requires researchers or production personnel to have rich professional knowledge and practical experience to ensure the smooth progress of the pelletization process and the high-quality performance of the final product.

[0064] 3. Specific operations of mixing and granulation:

[0065] Mixing process:

[0066] Prepare equipment: First, make sure the mixing equipment, such as agitators or ball mills, is in good working condition. Check the cleanliness of the equipment to avoid impurities that may affect the mixing effect.

[0067] Add powder and additives: Add the pre-treated powder and selected additives into the mixing equipment in a certain proportion. Pay attention to the order and proportion of addition to ensure that each ingredient is evenly distributed.

[0068] Start mixing: Start the mixing equipment and start stirring or ball milling. During this process, make sure that the speed of the agitator or ball mill is moderate so that the powder and additives can fully contact and mix evenly.

[0069] Check the mixing effect: During the mixing process, check the uniformity of the mixture regularly. You can ensure that the mixing effect meets the requirements by sampling and observation or performing chemical composition analysis.

[0070] Adjust parameters: According to the mixing effect, adjust the speed, mixing time and other parameters of the mixing equipment in time to obtain the best mixing effect.

[0071] Granulation method:

[0072] Depending on product requirements and production scale, choose spray drying or extrusion granulation. The following are the specific operations of these two granulation methods:

[0073] Spray drying method:

[0074] Prepare solution: send the evenly mixed powder and additive solution into the atomizer through a high-pressure pump.

[0075] Spray drying: Use an atomizer to spray the solution into mist, which is in direct contact with hot air for heat exchange, and quickly dried to obtain spherical powder particles.

[0076] Adjustment parameters: During the granulation process, according to the product requirements, adjust the atomizer pressure, solution flow rate, hot air temperature and other parameters to obtain the ideal pellet size and shape.

[0077] Extrusion granulation method:

[0078] Prepare equipment: Make sure the extrusion granulator and its ancillary equipment (such as feeding system, mold, etc.) are in good condition.

[0079] Add the mixture: Add the evenly mixed powder and additives into the feeding system of the extrusion granulator.

[0080] Start extrusion: start the extrusion granulator, adjust the speed and pressure of the extrusion screw, so that the mixture passes through the die to form pellets; the average particle size of the raw material powder is 1.2-1.5 microns; the specific surface area is 2.3-2.9m2 / g; the oxygen content is 0.85%;

[0081] Granulation index: Particle size: ≤80 mesh accounts for 100%, 80-200 mesh accounts for 30%; 200-325 mesh accounts for 10%; 325-400 mesh accounts for 15%; ≤400 mesh accounts for 30-35%;

[0082] The powder is set as pseudo-granules to increase fluidity, which is conducive to molding and pressing. Stirring granulation, air flow granulation, screening granulation, winnowing granulation and rolling granulation can be used.

[0083] Adjustment parameters: According to the size and shape requirements of the pellets, timely adjust the extrusion screw speed, pressure, mold shape and other parameters.

[0084] Collect pellets: Collect the pellets from the discharge port of the granulator and perform necessary subsequent processing (such as drying, screening, etc.).

[0085] 4. Pelletization treatment: the specific operation of pre-sintering the pellets after granulation and then performing the main sintering:

[0086] Pre-burning treatment:

[0087] Preparation of pellets: First, the pellets obtained after granulation are subjected to necessary inspection and screening to ensure that the size, shape and quality of the pellets meet the requirements of pre-burning treatment.

[0088] Set up pre-burning equipment: Place the pellets into the pre-burning equipment, ensure that the inside of the equipment is clean and free of impurities, and adjust the temperature and atmosphere control system of the equipment.

[0089] Removal of residual moisture and organic additives: Start the pre-burning equipment and gradually heat up to the preset temperature. In this process, the residual moisture and organic additives in the pellets will be gradually removed, and the pellet structure will become more compact.

[0090] Controlling the pre-firing temperature and time: The selection of the pre-firing temperature and time should be adjusted according to the characteristics of the powder and the type of additives. Generally speaking, it is necessary to ensure that the temperature is high enough to remove the residues, but not too high to avoid the destruction of the pellet structure. The pre-firing time should also be moderate to ensure that the residues are completely removed.

[0091] Cooling and inspection: After pre-burning, let the pellets cool naturally to room temperature in the equipment. Then take out the pellets for inspection to ensure that they are tight and free of defects such as cracks.

[0092] Main sintering:

[0093] Prepare sintering equipment: Place the pre-burned pellets into the sintering equipment and set up the temperature, atmosphere and pressure control systems of the equipment.

[0094] Controlled atmosphere: Select the appropriate sintering atmosphere according to product requirements and material properties. For silicon nitride / aluminum nitride ceramics, commonly used sintering atmospheres include nitrogen or inert gas.

[0095] Heating and densification: Gradually increase the temperature to the main sintering temperature and maintain it for a period of time. During this process, the pellets will be further densified, improving their strength and stability.

[0096] Optimize sintering parameters: Sintering temperature, time and atmosphere parameters have an important influence on the performance of pellets. They need to be optimized according to specific conditions to obtain the best sintering effect.

[0097] Cooling and post-processing: After sintering, let the pellets cool naturally to room temperature in the equipment. Then take out the pellets for necessary post-processing, such as cleaning, drying and packaging.

[0098] 5. Subsequent processing and testing: Specific operations for performance testing of the sintered pellets after cooling and crushing:

[0099] Cooling and breaking:

[0100] Cooling treatment: Take the sintered pellets out of the sintering equipment and place them in a well-ventilated place for natural cooling, or use special cooling equipment for rapid cooling.

[0101] During the cooling process, it is necessary to ensure that the pellets dissipate heat evenly to avoid thermal stress that may cause cracking or deformation.

[0102] Crushing and grinding: After the pellets are cooled to room temperature, they are crushed or ground as needed to adjust the particle size distribution of the pellets.

[0103] Select appropriate crushing equipment (such as crusher, ball mill, etc.), and control the crushing force and particle size range to ensure that the pellet size that meets the requirements is obtained.

[0104] During the crushing process, the particle size distribution of the pellets should be checked regularly and adjusted as needed to obtain the ideal particle size distribution.

[0105] Performance testing:

[0106] Density test: Measure the density of the pellets using methods such as a densitometer or water immersion method.

[0107] Compare the measured results with the design requirements or standard values ​​to ensure that the density of the pellets meets the requirements.

[0108] Hardness and compressive strength test: Use a hardness tester to measure the hardness of the pellets, such as Vickers hardness, Rockwell hardness, etc.

[0109] To conduct a compressive strength test, place the pellet on a pressure testing machine, apply gradually increasing pressure, and record the maximum pressure value when the pellet breaks.

[0110] The hardness and compressive strength of the pellets are evaluated based on the test results to ensure that they meet the requirements for use.

[0111] Chemical composition analysis: Chemical analysis or spectral analysis is used to detect the chemical composition of the pellets.

[0112] Compare the test results with the expected values ​​or standard values ​​to ensure that the chemical composition of the pellets meets the requirements.

[0113] Microstructure observation: Use optical microscope or electron microscope to observe the microstructure of the pellet.

[0114] The grain size, shape and distribution of the pellets are analyzed to evaluate their sintering quality and density.

[0115] Handling and improvement of defective products:

[0116] Cause analysis of defective products: For pellets that do not meet the requirements in performance testing, conduct cause analysis.

[0117] Check factors such as raw material quality, type and amount of additives, sintering process parameters, etc. to find out the possible reasons why the pellet performance does not meet the standards.

[0118] Take corrective measures: Take corresponding corrective measures based on the analysis results of the causes of non-conforming products.

[0119] It may involve adjusting the raw material ratio, replacing additives, optimizing sintering process parameters, etc.

[0120] The pellets were re-prepared and performance tests were conducted to verify the effectiveness of the improvement measures.

[0121] Embodiment 2

[0122] Based on Example 1, taking silicon nitride as an example, a detailed preparation process of silicon nitride ceramic pellets is proposed:

[0123] 1. Raw materials and additives

[0124] Silicon nitride powder: Use silicon nitride powder with a purity of ≥99.9%, an average particle size of 1.2 microns, and a specific surface area of ​​2.3m 2 / g, and the oxygen content is controlled below 0.85%.

[0125] Alumina / yttrium oxide additives (Al2O3 / Y2O3): purity requirement ≥99.5%, added amount is 5% (mass percentage) of the total amount of silicon nitride powder. The role of the alumina additive is to act as a sintering aid to improve the sintering quality and mechanical strength of silicon nitride ceramic balls.

[0126] 2. Powder Preparation

[0127] Silicon nitride powder and additives such as aluminum oxide / yttrium oxide are weighed according to a predetermined ratio and placed in a ball mill.

[0128] An appropriate amount of anhydrous ethanol was added as a ball milling medium for wet ball milling. The ball milling time was 12 hours, and the ball mill speed was controlled at 300 rpm.

[0129] After the ball milling, the mixed powder was dried at a temperature of 100° C. for 4 hours.

[0130] The dried powder was sieved through a 200-mesh sieve to ensure uniform particle size.

[0131] 3. Molding

[0132] The prepared silicon nitride mixed powder is placed in an isostatic pressing machine for molding.

[0133] The molding pressure was controlled to be 30 MPa and the holding time was 5 minutes.

[0134] The green silicon nitride ceramic ball after molding needs to be demolded and checked to see if its shape and size meet the requirements.

[0135] 4. Sintering

[0136] The formed silicon nitride ceramic ball green body is placed in a high-temperature sintering furnace for sintering.

[0137] The sintering temperature was set to 1700°C, the heating rate was 5°C / min, and the holding time was 4 hours.

[0138] During the sintering process, a nitrogen atmosphere is maintained inside the furnace to prevent the silicon nitride ceramic balls from oxidation at high temperatures.

[0139] 5. Performance testing

[0140] Density: Use a densitometer to measure the density of silicon nitride ceramic balls, which is required to reach 3.2g / cm 3 above.

[0141] Hardness: Use Vickers hardness tester to measure the hardness of silicon nitride ceramic ball, the result should be greater than 2,200Hv.

[0142] Compressive strength: Use a pressure testing machine to test the compressive strength, and the result should be greater than 2000Mpa.

[0143] Embodiment 3

[0144] Based on Example 1, a detailed preparation process of aluminum nitride ceramic powder pellets is proposed:

[0145] 1. Raw materials and additives

[0146] Aluminum nitride powder: purity ≥99.8%, average particle size 1.4 microns, specific surface area 2.6m 2 / g

[0147] Boron nitride additive (BN): purity ≥ 99.0%, added in an amount of 3% (mass percentage) of aluminum nitride powder, used to improve thermal conductivity and thermal shock resistance

[0148] 2. Powder Preparation

[0149] Aluminum nitride powder and boron nitride additive are added into a ball mill in a certain proportion, mixed and ball milled together with the ball milling medium.

[0150] The ball mill speed was set to 250 rpm and the mixing time was set to 60 minutes to obtain aluminum nitride mixed powder meeting certain fineness requirements.

[0151] 3. Molding

[0152] The mixed aluminum nitride powder is granulated by a spray drying method.

[0153] The atomizer pressure was set to 2.0 MPa, the solution flow rate was set to 10 L / h, and the hot air temperature was set to 500 °C.

[0154] The spray drying parameters are controlled to obtain aluminum nitride pellets with uniform particle size distribution.

[0155] 4. Sintering

[0156] The formed aluminum nitride pellets are placed in a high temperature furnace for sintering.

[0157] The sintering temperature was set to 1,800°C, the sintering time was set to 3 hours, and the sintering atmosphere was set to nitrogen.

[0158] 5. Performance testing

[0159] Density: measured with a density meter, the result is 3.3g / cm 3 .

[0160] Hardness: Measured using a Vickers hardness tester, the result is 2,100 Hv.

[0161] Thermal conductivity: measured using a thermal conductivity tester, the result is 25W / (m·K).

[0162] Embodiment 4

[0163] Based on Example 1, a detailed preparation process of alumina ceramic pellets is proposed.

[0164] 1. Raw materials and additives

[0165] Alumina powder: purity ≥99.7%, average particle size 1.5 microns, specific surface area 2.9m 2 / g

[0166] Zirconia additive (ZrO2): Purity ≥ 99.0%, added in an amount of 2% (mass percentage) of alumina powder, used to improve thermal shock resistance and wear resistance

[0167] 2. Powder Preparation

[0168] Alumina powder and zirconium oxide additive are added into the ball mill in a certain proportion, mixed and ball milled together with the ball milling media.

[0169] The ball mill speed was set to 280 rpm and the mixing time was set to 45 minutes to obtain the alumina mixed powder meeting certain fineness requirements.

[0170] 3. Molding

[0171] The mixed alumina powder was granulated by air flow granulation.

[0172] Set the gas flow rate to 15m 3 / h, and the nozzle diameter is 0.5mm to obtain alumina pellets with uniform particle size distribution.

[0173] 4. Sintering

[0174] The formed alumina pellets are placed in a high temperature furnace for sintering.

[0175] The sintering temperature was set to 1,600° C., the sintering time was set to 5 hours, and the sintering atmosphere was set to air.

[0176] 5. Performance Testing

[0177] Density: measured with a density meter, the result is 3.9g / cm 3 .

[0178] Hardness: Measured using a Vickers hardness tester, the result is 2,400 Hv.

[0179] Examples 2 to 4 respectively introduce the detailed preparation processes of silicon nitride, aluminum nitride and alumina ceramic pellets. In terms of the selection of raw materials and additives, silicon nitride ceramic pellets focus on high-purity silicon nitride powder and alumina additives to improve sintering quality and mechanical strength; aluminum nitride ceramic pellets use aluminum nitride powder and boron nitride additives to optimize thermal conductivity and thermal shock resistance; and alumina ceramic pellets enhance thermal shock resistance and wear resistance by mixing alumina powder and zirconium oxide additives.

[0180] In the preparation process, the three embodiments all use a ball mill for powder preparation, but the rotation speed, mixing time and ball milling medium may vary depending on the material properties. In the molding stage, the silicon nitride ceramic pellets are formed by pressing, while the aluminum nitride and aluminum oxide ceramic pellets are formed by spray drying and airflow granulation, respectively, to obtain pellets with uniform particle size distribution.

[0181] During the sintering stage, silicon nitride and aluminum nitride ceramic pellets are sintered in a high-temperature nitrogen atmosphere, while alumina ceramic pellets are sintered in an air atmosphere. The sintering temperature and time settings vary depending on the material and are designed to optimize the performance of the ceramic pellets.

[0182] Finally, the three embodiments were subjected to performance testing, including the measurement of density, hardness and specific properties (such as compressive strength and thermal conductivity) to ensure that the prepared ceramic pellets met the predetermined performance requirements.

[0183] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for pelletizing silicon nitride or aluminum nitride ceramic powder, Features: The method comprises the following steps: Raw material selection and pretreatment, raw material selection and procurement, as well as drying and screening; Selection and introduction of additives, including selection of additive types and methods of additive introduction; Mixing and granulation; Pelletizing treatment, pre-burning the pellets after granulation and then main sintering; Subsequent processing and testing: After the sintered pellets are cooled and crushed, performance testing is carried out.

2. A method for pelletizing silicon nitride or aluminum nitride ceramic powder according to claim 1, Features: The specific operations of raw material selection and pretreatment include: Raw material selection and procurement: According to product performance and process requirements, high-purity silicon nitride or aluminum nitride ceramic powders with uniform particle size distribution are selected to ensure that the raw materials are free of impurities, agglomerates, and have good fluidity; Drying and screening: Dry the selected powder to remove moisture and volatile impurities. The drying temperature and time are adjusted according to the characteristics of the powder to avoid powder agglomeration or oxidation. After drying, use screening equipment to grade the powder to ensure that the powder size meets the pelletization requirements.

3. A method for pelletizing silicon nitride or aluminum nitride ceramic powder according to claim 1, Features: The specific operations of selecting and introducing the additives include: Selection of additives: According to the characteristics of the powder and the requirements of pelletization, select binders, sintering aids and dispersants to improve the fluidity of the powder, increase the strength of the pellets and promote densification during the sintering process; Additive introduction method: Additives are introduced into the powder by dry mixing or wet mixing. During the mixing process, it is necessary to ensure that the additives are evenly distributed in the powder to avoid local concentrations that are too high or too low.

4. The method for pelletizing silicon nitride or aluminum nitride ceramic powder according to claim 1, Features: The specific operations of mixing and granulating include: Mixing process: the pretreated powder is mixed with the additives evenly. During the mixing process, stirring and ball milling are used to ensure that the powder and the additives are fully contacted and mixed evenly; Granulation method: according to product requirements and production scale, one of the granulation methods of spray drying and extrusion granulation is selected. During the granulation process, the rotation speed, pressure and temperature parameters of the granulator are controlled to obtain pellets of uniform size and regular shape; the average particle size of the raw material powder is 1.2-1.5 microns; the specific surface area is 2.3-2.9m2 / g; and the oxygen content is 0.85%.

5. The method for pelletizing silicon nitride or aluminum nitride ceramic powder according to claim 1, Features: The specific operations of the pelletization process include: Pre-burning treatment: the pellets after granulation are pre-burned to remove residual moisture and organic additives in the pellets and make the pellet structure more compact. The pre-burning temperature and time are adjusted according to the characteristics of the powder and the type of additives; The main sintering is carried out in a controlled atmosphere, and the pellets are further densified by heating to improve their strength and stability. The sintering temperature, time and atmosphere parameters have an important influence on the performance of the pellets and should be optimized according to the specific situation.

6. A method for pelletizing silicon nitride or aluminum nitride ceramic powder according to claim 1, Features: The specific operations of the subsequent processing and detection include: Cooling and crushing: the sintered pellets are cooled, crushed or ground to adjust the particle size distribution of the pellets; during the crushing process, the crushing force and particle size range are controlled to obtain the pellet size that meets the requirements; Performance testing: density, hardness, and compressive strength tests are conducted on the pellets to ensure that they meet the use requirements; chemical composition analysis and microstructure observation and testing methods are conducted to fully understand the performance and quality status of the pellets. For unqualified pellets, the cause analysis is conducted and corresponding measures are taken to improve them.

Citation Information

Patent Citations