Pyrene and imidazole blue luminescent material based on 1, 8-bit modification

By developing 1,8-bit modified pyrene-imidazole materials, the problem of slow development of blue light materials in the existing technology is solved, and blue luminescent materials with good transmission functions and high performance are realized, which improves the performance of organic electroluminescent devices. .

CN118930489APending Publication Date: 2024-11-12NANJING TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410978733.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Among the existing organic electroluminescence technology, the development of blue light materials is relatively slow, mainly because the band gap of blue light organic semiconductor materials is wide and the electron energy level is poorly matched with other functional layers, which affects the transmission of carriers and leads to efficiency and stability. It is difficult to achieve the effect of green and red light in color purity.

Method used

A new type of blue luminescent material-1,8-position modified pyrene-imidazole material was developed, which was prepared by synthesis, separation and purification processes. The imidazole intermediate was used to react Suzuki with boric acid derivatives to form hole and electron transport functions. pyrene-imidazole material is used as a luminescent material to expand the types of organic light emitting devices.

Benefits of technology

The prepared 1,8-position modified pyrene-imidazole material has good solubility, thermal stability and film formation. It is suitable for spin coating or vacuum evaporation preparation. It has good hole and electron transport functions and shows that it is The potential of a luminescent body or a guest improves the performance of organic electroluminescent devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930489A_ABST
    Figure CN118930489A_ABST
Patent Text Reader

Abstract

The invention discloses a 1, 8-bit modification-based pyrene and imidazole blue light-emitting material, a preparation method and an application of the 1, 8-bit modification-based pyrene and imidazole blue light-emitting material. The 1, 8-bit modified pyrene and imidazole blue light-emitting material molecule is composed of an electron donor and an acceptor, and has good hole and electron transmission performance; the material has high thermal stability, can be dissolved in a conventional organic solvent, and is suitable for preparing a film by a spin coating method or a vacuum evaporation method; compared with the prior art, the blue organic light-emitting material provided by the invention has good photophysical properties and stable oxidation-reduction performance, can be used for preparing a non-doped light-emitting functional layer, can be used as a guest material to prepare a doped light-emitting functional layer through co-evaporation with a proper host material, and shows that the material has a wide application prospect in blue organic light-emitting devices. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic electroluminescence, and specifically relates to a 1,8-modified pyrene imidazole blue luminescent material, a preparation method and the application of the luminescent material in the field of electroluminescence. Background Art

[0002] Organic light-emitting diodes (OLEDs) have the advantages of low power consumption, fast response, wide viewing angle, transparent display, and foldability. They have become one of the most promising display technologies in applications such as televisions, smart phones, auto shows, laptops, and wearable devices. In 1987, Tang et al. from Kodak Company in the United States used 8-hydroxyquinoline aluminum as the luminescent material, indium tin oxide ITO conductive film as the anode, and magnesium silver alloy as the cathode to prepare an organic electroluminescent device with excellent performance. The device adopts a double-layer film sandwich structure and uses aromatic diamine materials as the hole transport layer. The maximum brightness can reach 1000 cd cm -2 , luminous efficiency is 1.5lmW -1 , the driving voltage is less than 10V, and the life span is more than 100 hours. This result is of epoch-making significance in the history of organic electroluminescence, making it possible to apply organic electroluminescence in real life.

[0003] At present, the typical structure of an OLED device includes a cathode, an anode, and a functional layer located between the two electrodes. The functional layer includes one or more of an electron injection layer, an electron transport layer, a hole blocking layer, an organic light-emitting layer, an electron blocking layer, a hole transport layer, and a hole injection layer.

[0004] Among them, the luminescent material is the core functional layer of OLED. Among the three primary color luminescent materials, the development of blue light materials is relatively slow compared with green and red light materials. The main reason is that the blue light organic semiconductor material has a wide bandgap, and the electronic energy level is poorly matched with the electronic energy level of other functional layers, which affects the transmission of carriers, making it difficult to achieve the same effect as green and red light in terms of efficiency, stability and color purity. Therefore, the exploration and development of new blue light materials is a necessary condition for the development of organic electroluminescent devices.

[0005] Both pyrene and imidazole are classic structural units of organic electroluminescent materials. Their modifiability and unique structure can well regulate the luminescence and energy level of the materials. As a new emerging structure, pyrene imidazole combines the advantages of pyrene and imidazole while retaining good electron transport properties, becoming a novel organic electroluminescent material. However, pyrene imidazole materials based on 1,8-position modification have never been reported before, which is a problem that needs to be explored and solved in this field. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a new type of blue light-emitting material - 1,8-modified pyrene imidazole material, the material molecule is composed of electron donor and acceptor units, has hole and electron transport functions, can be used as a light-emitting material, and expands the types of organic compounds that can be used to prepare organic light-emitting devices.

[0007] The 1,8-modified pyrenoimidazole of the present invention has the following general chemical structure:

[0008]

[0009] Ar1 is any of the following structural units:

[0010]

[0011] Ar2 is any of the following structural units:

[0012]

[0013] Preferably, the 1,8-modified pyrene imidazole blue light-emitting material is selected from any one of the following structures:

[0014]

[0015] The present invention also provides a method for preparing the 1,8-modified pyrenoimidazole material, which comprises the following steps: synthesis, separation and purification.

[0016] The synthesis steps include: (1) preparation of imidazole intermediate: taking 1,8-dibromopyrenequinone, benzaldehyde, aniline (or 4-tert-butylaniline) and ammonium acetate, heating them in glacial acetic acid, and detecting the completion of the reaction; stopping heating to obtain the imidazole intermediate; (2) CC coupling: the imidazole intermediate and the boronic acid derivative undergo Suzuki reaction to obtain the final product.

[0017] The separation step comprises: (1) cooling the reaction to room temperature and filtering to obtain residual solid; (2) drying the reaction solution by spin drying, extracting with dichloromethane solvent, washing with ultrapure water, collecting the dichloromethane organic phase, drying, and spin drying.

[0018] The purification step includes: using dichloromethane and petroleum ether as eluents and SiO2 column chromatography to obtain the 1,8-dibromo-modified pyrene imidazole material as described above.

[0019] The present invention also provides an electroluminescent device, comprising a substrate layer, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer and a cathode layer.

[0020] The 1,8-modified pyrenoimidazole material prepared by the present invention has the following advantages and beneficial effects:

[0021] (1) The 1,8-modified pyrenoimidazole material prepared by the present invention has good solubility in solvents such as dimethyl sulfoxide, N,N′-dimethylformamide, toluene, chlorobenzene, and dichloromethane;

[0022] (2) The raw materials used in the 1,8-modified pyrene imidazole material prepared by the present invention are low in cost and the preparation process is simple;

[0023] (3) The 1,8-position modified pyrene imidazole material prepared by the present invention has high thermal stability and good film-forming properties, and is suitable for preparing thin films by spin coating or vacuum evaporation;

[0024] (4) The 1,8-modified pyrene imidazole material prepared by the present invention has good hole and electron transport functions;

[0025] (5) The 1,8-modified pyrene imidazole material prepared by the present invention has the potential to be a light-emitting host or guest. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They explain the present invention together with the examples of the present invention and do not constitute a limitation of the present invention.

[0027] Figure 1 Tetrahydrofuran dilute solution (10 -5 mol / L) UV absorption spectrum and fluorescence emission spectrum

[0028] Figure 2 Fluorescence emission spectra of spin-coated films

[0029] Figure 3 Material electrochemical performance test

[0030] Figure 4 Schematic diagram of the structure and energy level of non-doped OLED devices

[0031] Figure 5 EL spectrum of non-doped OLED device

[0032] Figure 6 Schematic diagram of doped OLED device structure and energy levels

[0033] Figure 7 EL spectrum of doped OLED devices Specific embodiments

[0034] The present invention is further described below by means of specific embodiments in combination with the accompanying drawings, but the specific embodiments herein are only used to explain the present invention and are not used to limit the present invention. Any modifications, equivalent substitutions and improvements made within the principles of the present invention should be included in the present invention and the described technical features or combinations of technical features should not be considered isolated, and they can be combined and combined with each other to achieve better technical effects.

[0035] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods. Unless otherwise specified, the materials and reagents used are all commercially available.

[0036] Example 1: Chemical synthesis of materials

[0037] The synthetic route of material 1 is as follows:

[0038]

[0039] 0.39 g of 1,8-dibromopyrenequinone, 0.1 mL of benzaldehyde, 0.5 mL of aniline and 0.5 g of ammonium acetate were heated to 120°C in 10 mL of glacial acetic acid and refluxed for 2 hours, then the heating was stopped. After cooling to room temperature, the solid was filtered to obtain a green solid. The light green intermediate A was purified by SiO2 column separation method with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) as the eluent, with a yield of 43.5%. 0.6 g of intermediate A, 0.4 g of 4-fluorophenylboric acid, 0.8 g of potassium carbonate, and 0.15 g of tetrakis-(triphenylphosphine)palladium were refluxed at 90°C in a mixed solvent of 20 mL of toluene, 10 mL of water, and 10 mL of ethanol for 12 hours; heating was stopped, and the mixture was cooled to room temperature and then evaporated under reduced pressure to obtain a yellow solid, which was separated by a SiO2 column and eluted with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 3:1) to obtain a light yellow target product 1 with a yield of 60.0%. 1 H NMR (400MHz, CHLOROFORM-D) δ9.21, 9.19, 8.12, 8.11, 8.10, 8.09, 8.05, 8.02, 7.69, 7.67, 7.64, 7.62, 7.60, 7.51, 7.49, 7.48, 7.47, 7.45, 7.36, 7.34, 7.24, 7.22, 7.21, 7.19, 7.17.

[0040] The synthetic route of material 2 is as follows:

[0041]

[0042] 0.39 g of 1,8-dibromopyrenequinone, 0.1 mL of benzaldehyde, 0.5 mL of aniline and 0.5 g of ammonium acetate were heated to 120 ° C in 10 mL of glacial acetic acid and refluxed for 2 hours, then the heating was stopped; after cooling to room temperature, it was filtered to obtain a green solid, which was separated by SiO2 column using a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) as eluent to obtain a light green intermediate A with a yield of 43.5%. Intermediate A 0.6 g, 4-methoxyphenylboronic acid 0.4 g, potassium carbonate 0.8 g, tetrakis-(triphenylphosphine)palladium 0.15 g were refluxed at 90 ° C for 12 hours in a mixed solvent of 20 mL toluene, 10 mL water and 10 mL ethanol. The heating was stopped, and the mixture was cooled to room temperature and then evaporated under reduced pressure to obtain a light yellow solid. The solid was separated by SiO2 column and eluted with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 3:1) to obtain a light yellow target product 2 with a yield of 65.0%. 1 H NMR (400MHz, CHLOROFORM-D) δ8.19, 8.17, 8.11, 7.69, 7.64, 7.60, 7.58, 7.48, 7.45, 7.43, 7.35, 7.10, 7.08, 7.05, 7.02, 3.93, 3.90.

[0043] The synthetic route of material 3 is as follows:

[0044]

[0045] 0.39 g of 1,8-dibromopyrenequinone, 0.1 mL of benzaldehyde, 0.5 mL of aniline and 0.5 g of ammonium acetate were heated to 120°C in 10 mL of glacial acetic acid and refluxed for 2 hours, then the heating was stopped; after cooling to room temperature, it was filtered to obtain a green solid, which was separated by SiO2 column and eluted with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) to obtain a light green intermediate A with a yield of 43.5%. 0.6 g of intermediate A, 0.5 g of 3,5-dimethoxyphenylboronic acid, 0.8 g of potassium carbonate, and 0.15 g of tetrakis-(triphenylphosphine)palladium were refluxed at 90°C in a mixed solvent of 20 mL of toluene, 10 mL of water, and 10 mL of ethanol for 12 hours. The heating was stopped, and the mixture was cooled to room temperature and then evaporated under reduced pressure to obtain a light yellow solid. The solid was separated by a SiO2 column and eluted with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 3:1) to obtain the yellow target product 3 with a yield of 63.0%. 1 H NMR (400MHz, CHLOROFORM-D) δ8.24, 8.21, 8.15, 8.13, 7.70, 7.68, 7.64, 7.46, 7.44, 7.36, 7.34, 6.81, 6.80, 6.68, 6.67, 6.59, 6.55, 3.88, 3.83.

[0046] The synthetic route of material 4 is as follows:

[0047]

[0048] 0.39 g of 1,8-dibromopyrenequinone, 0.1 mL of benzaldehyde, 0.5 mL of aniline and 0.5 g of ammonium acetate were heated to 120 ° C in 10 mL of glacial acetic acid and refluxed for 2 hours. The heating was stopped, and the solid was cooled to room temperature and filtered to obtain a green solid. The solid was separated by SiO2 column and a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) was used as the eluent to purify the light green intermediate A with a yield of 43.5%. Intermediate A 0.6 g, 4-cyanophenylboronic acid 0.4 g, potassium carbonate 0.8 g, tetrakis-(triphenylphosphine)palladium 0.15 g were refluxed at 90 ° C for 12 hours in a mixed solvent of 20 mL toluene, 10 mL water and 10 ml ethanol. After stopping heating and cooling to room temperature, vacuum rotary evaporation was performed to obtain a light yellow solid. The solid was separated by SiO2 column and purified with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) as eluent to obtain a light yellow target product 4 with a yield of 70.0%. 1 H NMR (400MHz, CHLOROFORM-D) δ8.13, 8.11, 8.09, 8.07, 8.02, 7.99, 7.86, 7.84, 7.81, 7.79, 7.77, 7.69, 7.68, 7.67, 7.65, 7.64, 7.62, 7.53, 7.51, 7.37, 7.35.

[0049] The synthetic route of material 5 is as follows:

[0050]

[0051] 0.39 g of 1,8-dibromopyrenequinone, 0.1 mL of benzaldehyde, 0.6 g of 4-tert-butylaniline and 0.5 g of ammonium acetate were heated to 120 ° C in 10 mL of glacial acetic acid and refluxed for 2 hours. The heating was stopped, and the solid was cooled to room temperature and filtered to obtain a green solid. The solid was separated by SiO2 column and a mixed solvent of dichloromethane and petroleum ether (volume ratio of 3:1) was used as the eluent to purify the light green intermediate B with a yield of 40.0%. Intermediate B 0.6 g, 4-fluorophenylboric acid 0.4 g, potassium carbonate 0.8 g, tetrakistriphenylphosphine palladium 0.15 g were refluxed at 90 ° C for 12 hours in a mixed solvent of 20 mL toluene, 10 mL water and 10 mL ethanol. The heating was stopped, and the mixture was cooled to room temperature and then evaporated under reduced pressure to obtain a light yellow solid. The solid was separated by SiO2 column and eluted with a mixed solvent of dichloromethane and petroleum ether (volume ratio of 4:1) to obtain a light yellow target product 5 with a yield of 55.0%. 1H NMR (400MHz, CHLOROFORM-D) δ8.12, 8.10, 8.05, 8.02, 7.73, 7.72, 7.67, 7.65, 7.64, 7.63, 7.62, 7.60, 7.59, 7.56, 7.53, 7.51, 7.49, 7.49, 7.47, 7.47, 7.45, 7.37, 7.36, 7.24, 7.22, 7.21, 7.19, 7.16, 1.47.

[0052] Example 2: Photophysical and electrochemical properties of materials

[0053] The photophysical characterization of the material was carried out, and the absorption, emission, fluorescence quantum yield of the THF solution and the emission of the spin-coated film were tested. Figure 1 and 2 The redox properties of the material were studied by electrochemical testing. Figure 3 , determine the highest occupied molecular orbital HOMO and the lowest unoccupied molecular orbital LUMO, and calculate the energy level difference E g The performance parameters are shown in Table 1.

[0054] Table 1: Photophysical properties and energy level parameters of materials

[0055]

[0056] ( 1 For 10 -5 mol / L tetrahydrofuran solution, 2 The spin-coated film was 40 nm thick. With platinum wire as the auxiliary electrode, glassy carbon disk as the working electrode, and Ag / Ag+ as the reference electrode, cyclic voltammetry (CV) scanning of CHI 660E A14297 was performed in tetra-n-butylammonium hexafluorophosphate (Bu4NPF6) (0.1 M) dichloromethane solvent at a scan rate of 100 mV s -1 . Ionization potential (IP CV )=[E ox -E 1 / 2 (Fc / Fc + )+4.8]eV, electron affinity (EACv) = [E red -E 1 / 2 (Fc / Fc + )+4.8]eV, where E ox and E red Respectively relative to Fc / Fc + (4.8 eV) initial oxidation potential and reduction potential, E 1 / 2 (Fc / Fc + ) indicates the calibration value obtained.

[0057] Example 3: Organic electroluminescent performance

[0058] Preparation of undoped organic light-emitting diodes (OLEDs): device structure and energy level diagram Figure 4 .

[0059] (1) Cleaning: First, the ITO glass substrate was ultrasonically cleaned with acetone, deionized water and ethanol for 15 minutes in sequence, and then the residual solvent on the surface of the ITO was blown dry with an N2 air gun, and then oxygen plasma treatment was performed for 10 minutes. Subsequently, the ITO glass substrate was transferred to an N2 glove box and a vacuum evaporation chamber to prepare the functional layer;

[0060] (2) Preparation of hole injection layer: In a N2 glove box, polystyrene sulfonate (PEDOT:PSS) (~40 nm) was spin-coated on ITO;

[0061] (3) Preparation of hole transport layer: NPB (~40 nm) was evaporated on the hole injection layer in a vacuum evaporation chamber;

[0062] (4) Preparation of the light-emitting layer: The above-mentioned materials were evaporated in a vacuum evaporation chamber to a thickness of 20 nm on the hole transport layer;

[0063] (5) Preparation of electron transport layer: TPBi (~40 nm) was evaporated on the organic light-emitting layer in a vacuum evaporation chamber;

[0064] (6) Preparation of electrodes: In a vacuum evaporation chamber, lithium fluoride (~1 nm) and aluminum (~100 nm) are evaporated on the electron transport layer to obtain the desired electroluminescent device.

[0065] Undoped OLED shows sky blue luminescence, EL spectrum see Figure 5 The electroluminescent performance parameters are shown in Table 2.

[0066] Table 2: Non-doped OLED performance parameters

[0067]

[0068] Doped OLED device production steps: device structure and energy level diagram Figure 6 .

[0069] (1) Cleaning: First, the ITO glass substrate was ultrasonically cleaned with acetone, deionized water and ethanol for 15 minutes in sequence, and then the residual solvent on the surface of the ITO was blown dry with a N2 air gun, and then oxygen plasma treatment was performed for 10 minutes. Subsequently, the ITO glass substrate was transferred to a vacuum evaporation chamber to prepare the functional layer;

[0070] (2) Preparation of hole injection layer: MoO3 (~6 nm) was evaporated on ITO in a vacuum evaporation chamber;

[0071] (3) Preparation of hole transport layer: NPB (~30 nm) was evaporated on the hole injection layer in a vacuum evaporation chamber;

[0072] (4) Preparation of electron blocking layer: TCTA (~10 nm) was evaporated on the hole transport layer in a vacuum evaporation chamber;

[0073] (5) Preparation of the light-emitting functional layer: The light-emitting material and the doping host mCP mentioned above are co-evaporated in a vacuum evaporation chamber at a ratio of 10% to deposit 20 nm on the barrier layer;

[0074] (6) Preparation of electron transport layer: TmPyPB was evaporated in a vacuum evaporation chamber to a thickness of 40 nm on the organic light-emitting functional layer;

[0075] (7) Preparation of electrodes: In a vacuum evaporation chamber, lithium fluoride (~1 nm) and aluminum (~100 nm) are evaporated on the electron transport layer to obtain the desired electroluminescent device.

[0076] The material was used as the guest and mCP as the host to prepare the doped OLED device to show blue luminescence. The EL spectrum is shown in Figure 7 The electroluminescent performance parameters are shown in Table 3.

[0077] Table 3: Doped OLED performance parameters

[0078]

[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes, replacements or simple modifications that can be easily thought of by any technician familiar with the technical field within the technical scope of the present invention should be covered within the protection scope of the present invention.

Claims

1. A type of 1,8-modified pyrene imidazole blue luminescent material, characterized in that: Ar1 is any of the following structural units: Ar2 is any of the following structural units:

2. The 1,8-modified pyrene imidazole blue luminescent material according to claim 1, characterized in that: Its chemical structure is any of the following structures:

3. A method for preparing the 1,8-modified pyrene imidazole blue luminescent material according to claim 1 or 2, characterized in that: The synthesis steps of the conjugated polyelectrolyte are as follows: Take 1,8-dibromopyrenequinone, benzaldehyde, aniline (or 4-tert-butylaniline) and ammonium acetate, heat them in glacial acetic acid, monitor the reaction until it is complete, stop heating and then treat to obtain an imidazole intermediate; the intermediate is subjected to Suzuki reaction with a corresponding boronic acid derivative; after the reaction is completed, the crude product obtained by extraction is purified by chromatographic column separation and recrystallization to obtain the target product.

4. Use of the 1,8-modified pyrenoimidazole material according to claim 1 or 2 as a luminescent material in an organic electroluminescent device.

5. The use of the 1,8-modified pyrenoimidazole material according to claim 4 as a luminescent material in an organic electroluminescent device, characterized in that: By vacuum thermal evaporation deposition, the non-doped single device is used as the light-emitting functional layer; the structure of the organic electroluminescent device is: ITO / PEDOT:PSS / NPB / light-emitting functional layer / TPBi / LiF / Al, wherein the thickness of PEDOT:PSS is 40nm, the thickness of the hole transport layer NPB is 40nm, the thickness of the light-emitting functional layer is 20nm, the thickness of the electron transport layer TPBi is 40nm, and the thicknesses of the electrode lithium fluoride and aluminum are 1nm and 100nm respectively.

6. The use of the 1,8-modified pyrenoimidazole material according to claim 4 as a light-emitting material in an organic electroluminescent device, characterized in that: By vacuum thermal evaporation deposition, the guest material is co-evaporated with a suitable host material to form a device light-emitting functional layer; the structure of the organic electroluminescent device is: ITO / MoO3 / NPB / TCTA / light-emitting functional layer / TmPyPB / LiF / Al, wherein the thickness of MoO3 is 6nm, the thickness of the hole transport layer NPB is 30nm, the thickness of the electron blocking layer TCTA is 10nm, the thickness of the light-emitting functional layer is 20nm, the thickness of the electron transport layer TmPyPB is 40nm, and the thicknesses of the electrode lithium fluoride and aluminum are 1nm and 100nm respectively.

Citation Information

Patent Citations

  • Pyrene derivatives and organic electronic device using pyrene derivatives

    CN101080478A

  • Organic thin film transistor

    CN101107716A

  • Pyrene-imidazole derivative and application thereof as electroluminescent material

    CN103772362A

  • Pyroimidazole derivative, preparation method thereof and electroluminescent device

    CN104592125A