Preparation method of novel efficient chlorinated polyethylene wax

By using the polar functional groups of oxidized polyethylene wax to react with the chlorinated agent at normal pressure and temperature, the preparation of high-efficiency chlorinated polyethylene wax is solved, and the problems of complex high-temperature and high-pressure processes and low chlorination rate in the existing technology are solved, and the problems of high-temperature and high-pressure processes and low chlorination rate are improved. Product performance and market application.

CN118930692APending Publication Date: 2024-11-12JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227596.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing preparation methods of chlorinated polyethylene wax require high temperature and high pressure conditions, the process is complex and the chlorination rate is low, resulting in unsatisfactory product performance, tight market and expensive prices.

Method used

Polar oxidized polyethylene wax is used as raw material, and high-efficiency chlorination is achieved at normal pressure and temperature through oxidation, chlorination, physical adsorption and decolorization and precipitation steps to achieve efficient chlorination at normal pressure and temperature to prepare high-bright chlorinated polyethylene wax.

Benefits of technology

The preparation process is simplified, high temperature carbonization is avoided, the chlorination rate is improved, the product is white powdery, suitable for large-scale production, broadening the scope of application, alleviating the problems of market shortage and expensive prices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930692A_ABST
    Figure CN118930692A_ABST
Patent Text Reader

Abstract

The invention discloses a novel high-efficiency chlorinated polyethylene wax preparation method, which comprises: carrying out an oxidation reaction on polyethylene wax to produce hydroxyl, carboxyl and other groups, carrying out a chlorination reaction on the oxidized polyethylene wax to convert hydroxyl, carboxyl and the like on the carbon chain of the oxidized polyethylene wax into chlorinated hydrocarbon, acyl chloride and other groups, and carrying out physical adsorption decolorization; and carrying out precipitation to obtain the chlorinated polyethylene wax. The chlorinated polyethylene wax prepared by the invention shows pure white granular appearance, the preparation process is simple, the cost is low, the chlorination efficiency is high, the chlorine content is 3.5-8.8 wt%, harsh process conditions such as high temperature and high pressure are not needed, and the application of the chlorinated polyethylene wax in the aspects of flame retardance, impact resistance modifiers and the like can be greatly expanded; the problems of market shortage and high price of chlorinated polyethylene wax are relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyethylene wax modification, in particular to a method for preparing a novel high-efficiency chlorinated polyethylene wax. Background Art

[0002] Polyethylene wax is a widely used polymer material with many excellent properties. In the plastic processing industry, polyethylene wax, as a lubricant and release agent, can effectively reduce the viscosity of plastic melt, reduce friction, and improve the surface finish and demolding performance of plastic products, thereby improving production efficiency and product quality. In the field of coatings and inks, polyethylene wax can improve the rheology, scratch resistance and wear resistance of coatings and inks, enhance the adhesion and gloss of coatings, and improve the performance and quality of coatings and inks. In addition, polyethylene wax also plays an important role in rubber processing, textile, papermaking and other industries.

[0003] However, in practical applications, polyethylene wax also has certain defects, such as limited dispersibility. In some applications, polyethylene wax may have uneven dispersion, which may affect its performance, especially in systems with high dispersibility requirements; relatively poor thermal stability. Compared with some other high-performance materials, polyethylene wax has slightly insufficient thermal stability. Under high temperature conditions, it may decompose or degrade to a certain extent; low strength and hardness. The mechanical properties of polyethylene wax are relatively weak, and its strength and hardness are not as good as some other engineering plastics or reinforced materials; limited chemical corrosion resistance. When facing some highly corrosive chemicals, it may corrode and impair performance. Therefore, the modification of polyethylene wax has always been an important topic in academia and enterprises.

[0004] Generally speaking, the modification of polyethylene wax includes oxidation, maleic anhydride grafting and chlorination. Among them, the oxidation method and maleic anhydride grafting modification method are relatively mature, but the preparation method of chlorinated polyethylene wax is very simple. The common preparation of chlorinated polyethylene wax is anaerobic pyrolysis, that is, polyethylene and anhydrous ferric chloride are reacted under high temperature and high pressure. However, this method is completed under high temperature and high pressure conditions, so there is a problem of polyethylene carbonization, and the chlorination rate is low. Even if the carbonization phenomenon is reduced by adding catalysts such as solid acid catalysts or the chlorination rate is increased by increasing the amount of ferric chloride, the effect is not ideal, but the process complexity and cost are increased. The market for chlorinated polyethylene wax is tight and expensive, and there are very few reports on related preparation methods.

[0005] Chinese patent CN202410571589.4 proposes a method for preparing chlorinated polyethylene wax, which prepares a catalyst, fixes the catalyst, and then adds high-density polyethylene, ferric chloride, a catalyst, etc. to a high-pressure reactor to react and prepare chlorinated polyethylene wax. Although this method reduces the problem of polyethylene carbonization to a certain extent, the catalyst preparation process is complicated, and it still needs to be reacted at a high temperature of more than 300 degrees Celsius and a high pressure of 0.9MPa. There are still excessive cracking and carbon deposition phenomena, and the chlorine content is only about 1%. Chinese patent CN201710578346.3 proposes a method for preparing chlorinated polyethylene wax, which adds polyethylene wax to water, and then passes chlorine or oxidized chlorination gas to react and prepare at 140-180°C. Although the modified method can prepare a certain amount of chlorinated polyethylene wax, polyethylene wax is a non-polar substance, which cannot be dissolved in water by itself, and the structure is CC bonds and CH bonds. This structure is difficult to undergo chlorination reaction under the conditions of lack of catalyst and high temperature and high pressure, so the chlorination rate is low and the performance is not ideal.

[0006] Therefore, a method for improving the chlorination rate of polyethylene wax is urgently needed. Summary of the invention

[0007] The purpose of the present invention is to provide a novel method for preparing a high-efficiency chlorinated polyethylene wax, so as to solve the problems of the above-mentioned chlorinated polyethylene wax preparation process, which is complicated, requires a high-temperature and high-pressure environment, and has a low chlorination rate. The present invention uses polar oxidized polyethylene wax as a raw material, and utilizes its inherent polar functional groups such as carboxyl and hydroxyl groups and chlorination reagents to achieve high-efficiency chlorination under mild conditions of normal pressure and temperature, and can prepare high-brightness chlorinated polyethylene wax through physical adsorption decolorization and precipitation crystallization, which is of great significance for broadening the application of chlorinated polyethylene wax.

[0008] To achieve the above object, the first aspect of the present invention provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, comprising the following steps:

[0009] S1: Oxidation reaction: Place the polyethylene wax in a solvent and dissolve and stir at 90-150°C for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-12 hours, and then add deionized water for washing;

[0010] S2: Chlorination reaction: dissolve the oxidized polyethylene wax solution obtained in step S1 above at 60-120°C and stir for 2-4 hours, then add a chlorinating agent to carry out chlorination reaction for 4-8 hours, and then add deionized water for washing;

[0011] S3: Physical adsorption decolorization: add an adsorbent to the chlorinated polyethylene wax mixture obtained in step S2 above, stir and react at 60-120°C for 1-3 hours, and then filter and recover the adsorbent;

[0012] S4: Precipitation: The chlorinated polyethylene wax mixture obtained in the above step S3 is stirred and reacted at 90-120° C. for 1-3 hours, then the temperature is lowered to 40-60° C., and a precipitant is slowly added to crystallize the chlorinated polyethylene wax to prepare a high-brightness white chlorinated polyethylene wax.

[0013] Preferably, the solvent in step S1 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, tetrahydrofuran, and dioxane.

[0014] Preferably, in step S1, the mass volume ratio of the polyethylene wax to the solvent is 0.1-1 g / mL.

[0015] Preferably, the oxidant in step S1 is one or more of air, oxygen, hydrogen peroxide, sodium hypochlorite, and nitric acid.

[0016] The oxidant of the present invention comprises a gaseous oxidant, a liquid oxidant and a solid oxidant, wherein the gas flow rate of the gaseous oxidant is 25-100 mL / min, and the mass ratio of the added amount of the liquid oxidant or the solid oxidant to the polyethylene wax is (0.05-0.2):1.

[0017] Preferably, the temperature of the oxidation reaction in step S1 is 90-150°C.

[0018] During the oxidation process, the present invention can generate polar groups such as hydroxyl groups and carboxyl groups in the carbon chain of the polyethylene wax, thereby forming oxidized polyethylene wax, which is convenient for subsequent reaction with a chlorinating agent at normal temperature and pressure.

[0019] Preferably, the acid value of the polyethylene wax after being treated with the oxidant is 14-24.

[0020] Preferably, the chlorinating agent in step S2 is one or more of thionyl chloride, thionyl chloride, hydrogen chloride, phosphorus trichloride, N-chloroamide, and trimethylchlorosilane.

[0021] Preferably, in step S2, the mass ratio of the chlorinating agent to the polyethylene wax is (0.01-0.1):1.

[0022] Preferably, the temperature of the chlorination reaction in step S2 is 60-120°C.

[0023] During the chlorination reaction of the present invention, polar groups such as hydroxyl groups and carboxyl groups in the carbon chain of the oxidized polyethylene wax can undergo chlorination reaction to generate corresponding chlorinated hydrocarbons, acyl chlorides and other groups, thereby introducing chlorine elements into the carbon chain to form chlorinated polyethylene wax.

[0024] Among the chlorinating agents, thionyl chloride, thionyl chloride, phosphorus trichloride, and trimethylsilyl chloride are liquid reagents with high selectivity, and can efficiently react hydroxyl and carboxyl groups to generate corresponding chlorohydrocarbons and acyl chlorides; hydrogen chloride is a gaseous reagent with high selectivity and high reaction yield, and can efficiently and quickly react hydroxyl and carboxyl groups to generate corresponding chlorohydrocarbons and acyl chlorides, and is cheap, easy to remove, and has a clean reaction without impurities; N-chloroamide is a solid reagent with safe and convenient operation, high selectivity, and can efficiently react hydroxyl groups to generate corresponding chlorides.

[0025] Preferably, the adsorbent in step S3 is one or more of activated carbon, alumina, zeolite molecular sieve, diatomaceous earth, and polyacrylamide.

[0026] Preferably, in step S3, the mass ratio of the adsorbent to the oxidized polyethylene wax is (0.02-0.1):1.

[0027] The present invention uses physical adsorption decolorization to completely remove metal elements, solid impurities and the like remaining in the chlorinated polyethylene wax.

[0028] Preferably, the precipitant in step S4 is one or more of methanol, ethanol, isopropanol, n-butanol, and N,N-dimethylformamide.

[0029] Preferably, in step S4, the mass volume ratio of the precipitant to the polyethylene wax is 0.5-4 g / mL.

[0030] Preferably, the crystallization temperature in step S4 is 40-60°C.

[0031] In the present invention, when the solvent fully dissolves the chlorinated polyethylene wax, the temperature is slowly lowered to allow partial crystals to precipitate, and then a suitable precipitant is used to slowly crystallize the polyethylene wax from the solution, so that the chlorinated polyethylene wax with high brightness and high chlorination rate can be prepared.

[0032] The second aspect of the present invention provides a chlorinated polyethylene wax prepared by the above-mentioned preparation method.

[0033] Preferably, the chlorine content of the chlorinated polyethylene wax is 3.5-8.8%.

[0034] The polyethylene wax prepared by the invention presents a bright white appearance, a high chlorination rate, and a chlorine content exceeding 3wt%.

[0035] The third aspect of the present invention provides an application of chlorinated polyethylene wax, which is used in masterbatches, coatings, inks, plastic processing, printing, hot melt adhesives, floor waxes, and waterproof materials.

[0036] Therefore, the present invention adopts a novel method for preparing a high-efficiency chlorinated polyethylene wax of the above structure, which has the following beneficial effects:

[0037] (1) The present invention uses polyethylene wax as a raw material, and can prepare high-brightness white powdered chlorinated polyethylene wax through the steps of oxidation, chlorination, physical adsorption decolorization, precipitation and the like. The preparation process is simple, and can be prepared through a solvation reaction at a temperature not exceeding 120° C., without the need for high temperature and high pressure reaction conditions, with high safety, good repeatability, and suitable for large-scale production.

[0038] (2) The preparation method of the present invention is different from the conventional anaerobic pyrolysis method. It does not require polyethylene and anhydrous ferric chloride to react at high temperature, but uses the inherent polar functional groups of polyethylene wax such as carboxyl and hydroxyl to react with the chlorinating agent at room temperature. The selected chlorinating agents can undergo chlorination reaction at normal pressure and temperature, and have the advantages of high selectivity and high chlorination rate. The hydroxyl and carboxyl groups can be efficiently reacted to generate corresponding chlorinated products and acyl chloride structures. The higher the hydroxyl and carboxyl groups contained in the polyethylene wax, the higher the chlorination rate. This chlorination method avoids the defect of high-temperature carbonization of polyethylene wax in the conventional pyrolysis method.

[0039] (3) The chlorinated polyethylene wax prepared by the present invention has a white powdery appearance, a high chlorination rate, and a chlorine content of more than 3wt%, which can effectively broaden the market application of chlorinated polyethylene wax and alleviate the problem of tight market and high price of chlorinated polyethylene wax.

[0040] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a process flow chart of the method for preparing chlorinated polyethylene wax in the present invention;

[0042] Figure 2 This is a picture of the appearance of the chlorinated polyethylene wax prepared in Example 1;

[0043] Figure 3 This is a scanning electron microscope image of the chlorinated polyethylene wax prepared in Example 1;

[0044] Figure 4 This is a transmission electron microscope image of the chlorinated polyethylene wax prepared in Example 1. DETAILED DESCRIPTION

[0045] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.

[0046] Example 1

[0047] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0048] (1) Oxidation reaction

[0049] Polyethylene wax (500 g) was placed in petroleum ether (3500 mL) and tetrahydrofuran (1500 mL), and stirred at 90°C for 2 hours. Air was then continuously introduced into the reaction solution (25 mL / min), and then stirred vigorously for 4 hours. Deionized water was then added to wash and remove impurities.

[0050] (2) Chlorination reaction

[0051] The oxidized polyethylene wax solution obtained in the above step (1) was stirred at 60° C. for 2 hours, and then thionyl chloride (5 g) was added to the reaction solution, and then stirred for 4 hours, and deionized water was added for washing to remove impurities.

[0052] (3) Physical adsorption decolorization

[0053] Activated carbon (10 g) was added to the reaction solution obtained in the above step (2), and then heated to 60° C. and stirred for reaction for 1 hour, followed by filtration to recover the activated carbon.

[0054] (4) Precipitation

[0055] The reaction solution obtained in the above step (3) was stirred at 90° C. for 1 hour, then cooled to room temperature, and then methanol (1000 mL) was used as a precipitant to slowly crystallize the chlorinated polyethylene wax.

[0056] Example 2

[0057] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0058] (1) Oxidation reaction

[0059] Polyethylene wax (500 g) was placed in n-hexane (2000 mL) and dichloromethane (500 mL), and stirred at 100°C for 3 hours. Then, oxygen was continuously introduced into the reaction solution (50 mL / min), and then stirred vigorously for 6 hours. Deionized water was added to wash and remove impurities.

[0060] (2) Chlorination reaction

[0061] The oxidized polyethylene wax solution obtained in the above step (1) was stirred and reacted at 80° C. for 3 hours, and then thionyl chloride (10 g) was added to the reaction solution, and then stirred and reacted for 5 hours, and deionized water was added for washing to remove impurities.

[0062] (3) Physical adsorption decolorization

[0063] Alumina (20 g) was added to the reaction solution in the above step (2), and then heated to 80°C and stirred for reaction for 2 hours, followed by filtration to recover the alumina.

[0064] (4) Precipitation

[0065] The reaction solution in the above step (3) was stirred at 100° C. for 1 hour, then cooled to room temperature, and then ethanol (500 mL) was used as a precipitant to slowly crystallize the chlorinated polyethylene wax.

[0066] Example 3

[0067] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0068] (1) Oxidation reaction

[0069] Polyethylene wax (500 g) was placed in n-hexane (2000 mL) and chloroform (500 mL), and stirred at 110°C for 4 hours. Then, hydrogen peroxide (25 g) was added to the reaction solution, and then stirred vigorously for 8 hours. Deionized water was added to wash and remove impurities.

[0070] (2) Chlorination reaction

[0071] The oxidized polyethylene wax solution obtained in the above step (1) was stirred and reacted at 100° C. for 4 hours, and then hydrogen chloride (20 g) was added to the reaction solution, and then the stirring reaction was continued for 6 hours, and deionized water was added for washing to remove impurities.

[0072] (3) Physical adsorption decolorization

[0073] Zeolite molecular sieve (30 g) was added to the reaction solution obtained in the above step (2), and then heated to 100° C. and stirred for reaction for 3 hours, followed by filtration to recover the zeolite molecular sieve.

[0074] (4) Precipitation

[0075] The reaction solution obtained in the above step (3) was stirred at 120° C. for 3 hours, then cooled to room temperature, and then ethanol (200 mL) and isopropanol (100 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0076] Example 4

[0077] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0078] (1) Oxidation reaction

[0079] Polyethylene wax (500 g) was placed in n-heptane (1000 mL) and toluene (200 mL), and stirred at 110°C for 2 hours. Then, sodium hypochlorite (50 g) was added to the reaction solution, and then stirred vigorously for 12 hours. Deionized water was added to wash and remove impurities.

[0080] (2) Chlorination reaction

[0081] The oxidized polyethylene wax solution obtained in the above step (1) was stirred and reacted at 120° C. for 2 hours, and then phosphorus trichloride (30 g) was added to the reaction solution, and then stirred and reacted for 6 hours, and deionized water was added for washing to remove impurities.

[0082] (3) Physical adsorption decolorization

[0083] To the reaction solution obtained in the above step (2), diatomaceous earth (40 g) was added, and then heated to 120° C. and stirred for reaction for 3 hours, and then the diatomaceous earth was recovered by filtration.

[0084] (4) Precipitation

[0085] The reaction solution obtained in the above step (3) was stirred at 120° C. for 3 hours, then cooled to room temperature, and then ethanol (200 mL) and n-butanol (50 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0086] Example 5

[0087] This embodiment provides a novel and efficient method for preparing chlorinated polyethylene wax, and the reaction steps are as follows:

[0088] (1) Oxidation reaction

[0089] Polyethylene wax (500 g) was placed in n-heptane (800 mL) and xylene (100 mL), and stirred at 120°C for 2 hours. Then, nitric acid (50 g) was added to the reaction solution, and then stirred vigorously for 8 hours. Deionized water was added to wash and remove impurities.

[0090] (2) Chlorination reaction

[0091] The oxidized polyethylene wax solution obtained in the above step (1) was stirred at 100° C. for 3 hours, and then N-chloroamide (40 g) was added to the reaction solution, and then the stirring reaction was continued for 8 hours, and deionized water was added for washing to remove impurities.

[0092] (3) Physical adsorption decolorization

[0093] Polyacrylamide (50 g) was added to the reaction solution obtained in the above step (2), and then heated to 100° C. and stirred for reaction for 3 hours, followed by filtration to recover the polyacrylamide.

[0094] (4) Precipitation

[0095] The reaction solution obtained in the above step (3) was stirred at 100° C. for 2 hours, then cooled to room temperature, and then ethanol (100 mL) and N,N-dimethylformamide (25 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0096] Example 6

[0097] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0098] (1) Oxidation reaction

[0099] Polyethylene wax (500 g) was placed in dichloromethane (600 mL) and dioxane (200 mL), and stirred at 120 ° C for 2 hours. Then, oxygen was continuously introduced into the reaction solution (100 mL / min), and then stirred vigorously for 8 hours. Deionized water was added to wash and remove impurities.

[0100] (2) Chlorination reaction

[0101] The oxidized polyethylene wax solution obtained in the above step (2) was stirred at 80° C. for 3 hours, and then trimethylsilyl chloride (40 g) was added to the reaction solution, and then the stirring reaction was continued for 8 hours, and deionized water was added for washing.

[0102] (3) Physical adsorption decolorization

[0103] Activated carbon (30 g) was added to the reaction solution obtained in the above step (2), and then heated to 80° C. and stirred for reaction for 3 hours, followed by filtration to recover the activated carbon.

[0104] (4) Precipitation

[0105] The reaction solution obtained in the above step (3) was stirred at 100° C. for 2 hours, then cooled to room temperature, and then ethanol (200 mL) and dimethyl sulfoxide (25 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0106] Example 7

[0107] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0108] (1) Oxidation reaction

[0109] Polyethylene wax (500 g) was placed in petroleum ether (400 mL) and toluene (100 mL), stirred at 120 ° C for 2 hours, and then air was continuously introduced into the reaction solution (100 mL / min), and then vigorously stirred for 8 hours, and then deionized water was added to wash to remove impurities.

[0110] (2) Chlorination reaction

[0111] The oxidized polyethylene wax solution obtained in the above step (1) was stirred and reacted at 100° C. for 3 hours, and then thionyl chloride (50 g) was added to the reaction solution, and then the stirring reaction was continued for 8 hours, and deionized water was added for washing to remove impurities.

[0112] (3) Physical adsorption decolorization

[0113] Zeolite molecular sieve (20 g) was added to the reaction solution obtained in the above step (2), and then heated to 100° C. and stirred for reaction for 2 hours, followed by filtration to recover the zeolite molecular sieve.

[0114] (4) Precipitation

[0115] The reaction solution obtained in the above step (3) was stirred at 100° C. for 2 hours, then cooled to room temperature, and then methanol (200 mL) and ethanol (200 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0116] Example 8

[0117] This embodiment provides a method for preparing a novel high-efficiency chlorinated polyethylene wax, and the reaction steps are as follows:

[0118] (1) Oxidation reaction

[0119] Polyethylene wax (500 g) was placed in petroleum ether (800 mL) and dioxane (200 mL), and stirred at 130 ° C for 2 hours. Then, oxygen was continuously introduced into the reaction solution (50 mL / min), and then stirred vigorously for 12 hours. Deionized water was added to wash and remove impurities.

[0120] (2) Chlorination reaction

[0121] The oxidized polyethylene wax solution obtained in the above step (1) was stirred and reacted at 100° C. for 3 hours, and then hydrogen chloride (30 g) was added to the reaction solution, and then stirred and reacted for 6 hours, and deionized water was added for washing to remove impurities.

[0122] (3) Physical adsorption decolorization

[0123] To the reaction solution obtained in the above step (2), diatomaceous earth (40 g) was added, and then heated to 100° C. and stirred for reaction for 2 hours, and then the diatomaceous earth was recovered by filtration.

[0124] (4) Precipitation

[0125] The reaction solution obtained in the above step (3) was stirred at 100° C. for 2 hours, then cooled to room temperature, and then methanol (200 mL) and isopropanol (100 mL) were used as precipitants to slowly crystallize the chlorinated polyethylene wax.

[0126] Comparative Example 1

[0127] The difference from Example 7 is that chlorinated polyethylene wax is prepared by reacting directly purchased oxidized polyethylene wax with a chlorinating agent. The acid value of the oxidized polyethylene wax is 7-13, purchased from Lianyungang Youdao New Material Technology Co., Ltd., model 0A-103.

[0128] Comparative Example 2

[0129] The difference from Example 7 is that oxidized polyethylene wax with a higher acid value is used to react with a chlorinating agent to prepare chlorinated polyethylene wax. The acid value of the oxidized polyethylene wax is 30-33, purchased from Lianyungang Youdao New Material Technology Co., Ltd., model 0A-330.

[0130] Example 9

[0131] The chlorinated polyethylene wax prepared in Examples 1-8 and Comparative Examples 1-2 were used as samples for whiteness value test. Referring to GB2913-82 plastic whiteness test method, the whiteness was measured using a whiteness meter WSB-2. Examples 1-8 and Comparative Examples 1-2 were evenly placed in a sample pool, respectively, and the surface of the sample was covered with a smooth glass plate. The sample was pressed, and then the glass plate was carefully removed to keep the surface of the sample smooth and free of scattered particles. The pressed sample was placed in the sample stage of the instrument, and its whiteness value was measured to 0.1%.

[0132] Referring to the detection method of chlorine content in chlorinated paraffin, the chlorine content in the chlorinated polyethylene wax prepared in Examples 1-8 and Comparative Examples 1-2 was measured.

[0133]

[0134] As can be seen from the above table, the chlorinated polyethylene wax prepared based on Examples 1-8 has a very ideal whiteness value, all exceeding 85, and the appearance presents a white micro-granular morphology, which has a good driving effect on the application expansion of chlorinated polyethylene wax. The chlorine content of the chlorinated polyethylene wax prepared based on Examples 1-8 is between 3.5-8.8wt%. This high chlorine content shows that the method can successfully produce chlorine elements on the carbon chain of polyethylene wax, and also shows that the chlorination reaction by utilizing the inherent polar groups such as carboxyl and hydroxyl groups on the carbon chain of polyethylene wax and the chlorinating agent is very successful, and the chlorine content can actually be changed by adjusting the content of hydroxyl and carboxyl groups in the polyethylene wax carbon chain and the amount of chlorinating agent added. It can also be seen from the above table that the whiteness value and chlorine content of Comparative Example 1-2 are significantly less than those of Example 7, indicating that the limitation of the acid value of oxidized polyethylene wax in the present invention plays a very important role.

[0135] Figure 2 This is a picture of the appearance of the chlorinated polyethylene wax prepared in Example 1, and it can be clearly seen that the micro-particles are white in color. The bright white color of the prepared chlorinated polyethylene wax is one of the most important indicators, which avoids uneven color or the appearance of impurities, improves the visual quality of the product, and improves the color compatibility of the product. For products that require color matching, such as coatings, inks, etc., white chlorinated polyethylene wax will not interfere with the color, which is conducive to accurately matching the required color and ensuring the color consistency and accuracy of the product. The scope of application has been broadened. In some specific application fields, such as plastic products and rubber products that have strict requirements on color, white chlorinated polyethylene wax can better meet the needs of these industries and expand its scope of application. At the same time, when consumers choose products, they often have a higher preference for products with neat appearance and pure color.

[0136] Figure 3 This is a scanning electron microscope image of the chlorinated polyethylene wax prepared in Example 1. It can be seen that it is composed of very smooth and delicate tiny particles. Figure 4The transmission electron microscope image also shows that the prepared chlorinated polyethylene wax is a waxy structure composed of many extremely tiny transparent flakes or particles. This structural feature plays a very important role. It can improve dispersibility and compatibility. The structure of tiny particles enables chlorinated polyethylene wax to be better dispersed in various matrices and improve compatibility with other materials; improve surface properties. Smooth and delicate particles can provide better surface lubricity and wear resistance. When applied to products such as coatings, inks or plastics, it can increase the smoothness of the surface, reduce friction, and improve the service life and appearance quality of the product; enhance the filling effect. These tiny particles can fill the tiny gaps and defects in the material, enhance the structural integrity of the material, and help improve the mechanical properties of the material, such as strength and toughness; improve stability. The uniform tiny particle structure can make chlorinated polyethylene wax more stable during storage and use, reduce the occurrence of agglomeration and precipitation, and ensure the consistency of product performance; improve multifunctional application. This structure allows chlorinated polyethylene wax to play multiple functions in different fields. It can be used as a lubricant and release agent in plastics, and can improve scratch resistance and weather resistance in coatings.

[0137] In summary, the present invention provides a novel method for preparing a high-efficiency chlorinated polyethylene wax, which has a simple process and does not require polyethylene and anhydrous ferric chloride to react at a high temperature, thereby avoiding the defect of high-temperature carbonization of polyethylene wax. Furthermore, the higher the content of hydroxyl groups, carboxyl groups, etc. on the carbon chain of the polyethylene wax, the higher the chlorination rate will be. This method can effectively broaden the market application of chlorinated polyethylene wax, alleviate the problem of tight market and high price of chlorinated polyethylene wax, and enhance its application in flame retardant, impact modifier, etc.

[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a novel high-efficiency chlorinated polyethylene wax, characterized in that: The following steps are involved: S1: Oxidation reaction: Place the polyethylene wax in a solvent and dissolve and stir at 90-150°C for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-12 hours, and then add deionized water for washing; S2: Chlorination reaction: dissolve the oxidized polyethylene wax solution obtained in step S1 above at 60-120°C and stir for 2-4 hours, then add a chlorinating agent to carry out chlorination reaction for 4-8 hours, and then add deionized water for washing; S3: Physical adsorption decolorization: add an adsorbent to the chlorinated polyethylene wax mixture obtained in step S2 above, stir and react at 60-120°C for 1-3 hours, and then filter and recover the adsorbent; S4: Precipitation: The chlorinated polyethylene wax mixture obtained in the above step S3 is stirred and reacted at 90-120° C. for 1-3 hours, then the temperature is lowered to 40-60° C., and a precipitant is slowly added to crystallize the chlorinated polyethylene wax to prepare a high-brightness white chlorinated polyethylene wax.

2. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The solvent in step S1 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, tetrahydrofuran, and dioxane.

3. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The oxidant in step S1 is one or more of air, oxygen, hydrogen peroxide, sodium hypochlorite, and nitric acid.

4. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The chlorinating agent in step S2 is one or more of thionyl chloride, thionyl chloride, hydrogen chloride, phosphorus trichloride, N-chloroamide, and trimethylchlorosilane.

5. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The adsorbent in step S3 is one or more of activated carbon, alumina, zeolite molecular sieve, diatomaceous earth, and polyacrylamide.

6. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The precipitant in step S4 is one or more of methanol, ethanol, isopropanol, n-butanol, and N,N-dimethylformamide.

7. The method for preparing a novel high-efficiency chlorinated polyethylene wax according to claim 1, characterized in that: The temperature of crystallization in step S4 is 40-60°C.

8. A chlorinated polyethylene wax, characterized in that Prepared by the preparation method according to any one of claims 1 to 7.

9. A chlorinated polyethylene wax according to claim 8, characterized in that: The chlorine content of chlorinated polyethylene wax is 3.5-8.8%.

10. The use of a chlorinated polyethylene wax according to claim 9, characterized in that: Chlorinated polyethylene wax is used in masterbatch, coatings, inks, plastic processing, printing, hot melt adhesives, floor wax, and waterproof materials.