Liquid fluoroelastomer as well as preparation method and application thereof

By reacting the fluoroelastomer solution with magnesium oxide and alcohol amine, introducing pendant hydroxyl and terminal carboxylic functional groups, the problem of low functionalities of liquid fluoroelastomers is solved by oxidative degradation method, and high functionality and excellent mechanical properties are achieved. Suitable for a variety of applications.

CN118930707AActive Publication Date: 2024-11-12BEIJING UNIV OF CHEM TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411216425.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing oxidation and degradation methods have low functionalities, insufficient cross-linking reactivity and mechanical strength, and complex processes and safety hazards.

Method used

By mixing the fluoroelastomer solution with magnesium oxide and alcohol amine, the pendant hydroxyl and terminal carboxylic functional groups are introduced to improve the functionality of the liquid fluoroelastomer and react with the crosslinking agent to cure it to form a high-functional low-molecular-weight liquid fluorine with low molecular weight Elastomer.

Benefits of technology

It has achieved the preparation of high-functional liquid fluoroelastomers, with high cross-linking reactivity, excellent mechanical properties and stability, simple and safe process, and is suitable for the preparation of special adhesives, sealants and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930707A_ABST
    Figure CN118930707A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fluorine materials, and discloses a liquid fluoroelastomer as well as a preparation method and application thereof. And mixing the fluorine-containing elastomer solution, magnesium oxide and alcohol amine for reaction to obtain the liquid fluorine elastomer, wherein the fluorine-containing elastomer has no side hydroxyl group. The preparation method has the characteristics of few byproducts, simplicity, controllability, high yield and the like. The high-functionality low-molecular-weight liquid fluoroelastomer contains a side hydroxyl group, preferably can also contain a terminal carboxyl group or a terminal hydroxyl group, has high functionality and good reactivity, and is cured after being subjected to a cross-linking reaction with a polyisocyanate compound. The cured product has excellent mechanical properties and chemical medium resistance, and can be used for preparing special adhesives, sealants and coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine materials, and in particular to a liquid fluorine elastomer and a preparation method and application thereof. Background Art

[0002] Fluoroelastomer is a polymer material containing fluorine atoms in the main chain or side chain. It has good chemical stability and thermal stability. At the same time, it also has excellent solvent resistance and other properties. It is widely used in aerospace, petrochemical, automobile and other fields. However, traditional fluoroelastomers are solid at room temperature and need to be processed by solid rubber molding, so it is difficult to prepare products in the form of solvent-free adhesives, coatings, etc. Liquid fluoroelastomers have a certain fluidity and can be cured into the required shape by adding a suitable curing agent. It can also be cured and formed "in situ" on the spot. The cured product retains the excellent properties of solid fluoroelastomers, such as high temperature resistance and chemical resistance. There are two major categories of liquid fluoroelastomers: one has no reactive functional groups in its chemical structure, and the other contains reactive functional groups. This functional group can be located in the side chain or distributed at both ends of the molecular chain. "Active" liquid fluoroelastomers with reactive functional groups, especially liquid fluoroelastomers containing two or more active functional groups, have good reactivity and therefore have a wide range of application value.

[0003] The main methods for synthesizing active liquid fluoroelastomers are monomer polymerization and oxidative degradation. Due to the complex process, difficulty and low yield of the monomer polymerization method, the molecular weight of the obtained product is difficult to control, and the initiators and telogens used in the monomer polymerization method are usually high-priced and complex organic compounds. Foreign researchers began to study the preparation of liquid fluoroelastomers by oxidative degradation around 1950. After continuous development, oxidative degradation is generally used to prepare liquid fluoroelastomers in modern industrial production. The problem with preparing liquid fluoroelastomers by oxidative degradation is that the actual functionality is low. During the oxidative degradation process, the two ends of the broken chain cannot be completely converted into carboxyl groups. Even if they are all converted into carboxyl groups, their theoretical functionality is 2, the cross-linking reactivity is low, and the mechanical strength is low.

[0004] From the preparation of carboxyl-terminated liquid fluoroelastomers by oxidative degradation, we can learn that fluoroelastomers containing vinylidene fluoride units can undergo dehydrofluorination to generate double bonds in an alkaline environment, and the generated double bonds can also undergo addition reactions to introduce active groups. Currently, the common methods for introducing hydroxyl groups on double bonds include double bond epoxidation ring-opening reactions and thiol-double bond click reactions, but epoxidation reagents are mostly peroxides, and the more effective ring-opening reagent osmium tetroxide is a highly toxic compound. The commonly used hydroxylation reagent 2-mercaptoethanol also has certain toxicity, which poses safety issues.

[0005] Therefore, there is an urgent need to develop a low molecular weight liquid fluoroelastomer that has high functionality and is simple and safe to prepare. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a liquid fluoroelastomer and a preparation method and application thereof.

[0007] The present invention enables the liquid fluoroelastomer to have a side hydroxyl group, and the terminal group can also be a terminal carboxyl group or a terminal hydroxyl group. These reactive functional groups have good reactivity and react with a crosslinking agent to be cured. The cured product has good mechanical properties and stability.

[0008] In order to achieve the above object, the first aspect of the present invention provides a liquid fluoroelastomer, characterized in that the structural formula of the liquid fluoroelastomer is as shown in Formula I:

[0009]

[0010] Wherein, R1 is -NH(CH2) x OH, R2 is a non-reactive terminal group, a carboxyl group or a hydroxyl group;

[0011] x is 1-6;

[0012] The ratio between m and q is 4-25:1.

[0013] The second aspect of the present invention provides a method for preparing the liquid fluoroelastomer according to the first aspect, wherein the method comprises: mixing a fluoroelastomer solution, magnesium oxide and an alcohol amine to react to obtain the liquid fluoroelastomer;

[0014] Wherein, the fluorine-containing elastomer has no pendant hydroxyl groups.

[0015] The third aspect of the present invention provides a liquid fluoroelastomer prepared according to the method described in the second aspect.

[0016] The fourth aspect of the present invention provides use of the liquid fluoroelastomer according to the first aspect or the third aspect in the preparation of special adhesives, sealants and coatings.

[0017] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0018] (1) The high-functionality, low-molecular-weight liquid fluoroelastomer provided by the present invention introduces hydroxyl groups on the side groups. Compared with the terminal-active liquid fluoroelastomer, both the terminal groups and the side groups are reactive, which makes up for the defect of the terminal-active liquid fluoroelastomer with low functionality. In the cross-linking and curing process, it has more cross-linking sites, high cross-linking reactivity, high cross-linking density, and better mechanical properties after vulcanization.

[0019] (2) The present invention is the first to propose a method for preparing a high-functionality liquid fluoroelastomer. The raw material synthesis is relatively simple, and there is no need to use a fluorinated olefin copolymerization method. The synthesis process is simple and controllable. During the operation, few reactants are added, and no additional initiator or catalyst is required. Moreover, the unreacted raw materials added are easy to remove.

[0020] (3) The high-functionality liquid fluoroelastomer provided by the present invention is a viscous liquid or semi-solid at room temperature, and can react with carboxyl and hydroxyl crosslinking agents to undergo crosslinking and curing. The cured product has excellent mechanical properties, thermal stability and chemical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a graph showing the infrared spectrum (FT-IR) test results of the high-functionality, low-molecular-weight liquid fluoroelastomer prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0023] The first aspect of the present invention provides a liquid fluoroelastomer, wherein the structural formula of the liquid fluoroelastomer is as shown in Formula I:

[0024]

[0025] Wherein, R1 is -NH(CH2) x OH, R2 is a non-reactive terminal group, a carboxyl group or a hydroxyl group;

[0026] x is 1-6;

[0027] The ratio between m and q is 4.36-23.4:1.

[0028] In the present invention, x, m, n, p, r, and q are all integers. In some cases, n, p, and r are not all 0 at the same time, for example, p≠0.

[0029] The liquid fluoroelastomer provided by the present invention partially introduces R1 groups in a specific proportion on the vinylidene fluoride structural unit to achieve the purpose of introducing active groups on the side groups, thereby improving the functionality of the liquid fluoroelastomer and finally obtaining a vulcanized product with better mechanical properties.

[0030] In some embodiments of the present invention, x is 2-4, preferably 3.

[0031] In some embodiments of the present invention, the ratio of m to q is 4.36-23.4:1, for example, 4.36, 4.48, 4.66, 4.8, 4.9, 5.16, 8.21, 8.62, 8.84, 11.09, 11.11, 11.42, 12.34, 12.51, 13.18, 14.65, 16.44, 17.49, 19.34, 20.8, 21.6, 23.4, and any value within the range of any two of the above values, preferably 8.84-17.49:1, and more preferably 14.65-17.49:1.

[0032] In some embodiments of the present invention, the functionality of the liquid fluoroelastomer is above 2.5, for example, 2.5, 2.53, 2.58, 2.6, 2.63, 2.67, 2.7, 2.8, 3, 3.3, 3.45, 3.5, 3.54, 3.7, 3.75, 3.9, 4.03, 4.39, 4.6, 5.05, 6.2, and any value within the range of any two of the above values, preferably above 4, or 3.3-6.2.

[0033] In some embodiments of the present invention, the liquid fluoroelastomer is selected from at least one of a side hydroxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl-terminated hydroxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl-terminated carboxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl-terminated hydroxyl vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene terpolymer and a side hydroxyl-terminated carboxyl vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene terpolymer.

[0034] The second aspect of the present invention provides a method for preparing the liquid fluoroelastomer according to the first aspect, wherein the method comprises: mixing a fluoroelastomer solution, magnesium oxide and an alcohol amine to react to obtain the liquid fluoroelastomer;

[0035] Wherein, the fluorine-containing elastomer has no pendant hydroxyl groups.

[0036] Alcoholamine itself is a weak base, and there is no need to perform subsequent reactions after adding alkali to dehydrofluorinate. Liquid fluoroelastomer can directly dehydrofluorinate under the action of alcoholamine while alcoholamine acts as a nucleophilic agent to react with double bonds, and the method is simple and easy to operate. Therefore, the present invention introduces hydroxyl groups into liquid fluoroelastomer with inactive side groups through addition reaction with alcoholamine to prepare side hydroxyl liquid fluoroelastomer, and further, combines oxidation degradation method with side group introduction of hydroxyl groups to prepare liquid fluoroelastomer with active groups on both side groups and end groups.

[0037] In some embodiments of the present invention, the fluorine-containing elastomer is a binary, ternary or multi-polymer of vinylidene fluoride, preferably G-101 of Daikin Corporation of Japan, a carboxyl-terminated liquid fluorine elastomer or a hydroxyl-terminated liquid fluorine elastomer.

[0038] In some embodiments of the present invention, the solvent in the fluorine-containing elastomer solution is an organic solvent, preferably at least one selected from methyl isobutyl ketone, tetrahydrofuran and acetone.

[0039] In some embodiments of the present invention, the alcoholamine is selected from at least one of ethanolamine, 3-aminopropanol and 4-amino-1-butanol, preferably 3-aminopropanol.

[0040] In some embodiments of the present invention, the molar ratio of the alcohol amine to the vinylidene fluoride structural unit in the fluorine-containing elastomer is 0.5-4:4, preferably 1-3:4, more preferably 1.5-2:4, and most preferably 2:4.

[0041] In some embodiments of the present invention, the reaction time is 3-15h, preferably 8-12h;

[0042] In some embodiments of the present invention, the reaction temperature is 20-120°C, preferably 25-116°C, and more preferably 25°C, 60°C or 110°C.

[0043] In some embodiments of the present invention, after the reaction is completed, the system is cooled to room temperature, the inorganic salt and residual alcohol amine are extracted to remove, the solvent is removed by rotary evaporation, and the final product is obtained after drying.

[0044] The third aspect of the present invention provides a liquid fluoroelastomer prepared according to the method described in the second aspect.

[0045] The fourth aspect of the present invention provides use of the liquid fluoroelastomer according to the first aspect or the third aspect in the preparation of special adhesives, sealants and coatings.

[0046] The present invention will be described in detail below through examples.

[0047] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0048] In various embodiments of the present invention,

[0049] Low molecular weight liquid fluoroelastomer with inactive terminal groups, brand G-101, purchased from Daikin Corporation of Japan;

[0050] Carboxyl-terminated low molecular weight liquid fluoroelastomer, homemade;

[0051] Hydroxyl-terminated low molecular weight liquid fluoroelastomer, homemade;

[0052] Sodium borohydride, purchased from Tianjin Huadong Reagent Factory, CAS No. 16940-66-2;

[0053] Iodine, purchased from Fuchen Chemical, CAS No. 109-99-9;

[0054] Hydrochloric acid, purchased from Beijing Chemical Plant, CAS No. 16881-77-9;

[0055] Anhydrous sodium sulfite, purchased from Aladdin, CAS No. 7440-05-3;

[0056] Tetrahydrofuran, purchased from Fuchen Chemical, CAS No. 109-99-9;

[0057] HDI trimer curing agent, purchased from Covestro, CAS No. 3779-63-3;

[0058] Ethylene glycol, purchased from McLean, CAS No. 107-21-1;

[0059] Magnesium oxide, purchased from McLean, CAS No. 1309-48-4;

[0060] Methyl isobutyl ketone, purchased from Maclean, CAS number 108-10-1;

[0061] Ethanolamine, purchased from McLean, CAS No. 141-43-5;

[0062] 3-Aminopropanol, purchased from Maclean, CAS No. 156-87-6;

[0063] 4-Amino-1-butanol was purchased from Maclean with CAS number 13325-10-5.

[0064] The low molecular weight fluorine-containing elastomer used in Examples 1-11 is a vinylidene fluoride (VDF)-hexafluoropropylene (HFP) copolymer of Daikin Corporation of Japan, with a brand name of G-101, a copolymer composition with a VDF:HFP molar ratio of 80:20, and a number average molecular weight of 6200.

[0065] The low molecular weight fluorine-containing elastomer used in Examples 12-14 is a carboxyl-terminated liquid fluorocarbon elastomer A, which is a vinylidene fluoride (VDF)-hexafluoropropylene (HFP) binary copolymer, with a copolymer composition VDF:HFP molar ratio of 78:22, a carboxyl content of 3wt%, and a number average molecular weight of 2600, and is prepared by the following method:

[0066] 100 g of vinylidene fluoride (VDF)-hexafluoropropylene (HFP) copolymer elastomer (M) was added to a 2L glass reactor. n =296200,M w=335500, copolymer composition VDF:HFP molar ratio is 78:22) and 900g acetone, mechanically stirred until the solid elastomer is completely dissolved; 32g KOH and 39.8g deionized water are weighed in a 100mL beaker to prepare a 45% KOH aqueous solution; 60g of 30% hydrogen peroxide is weighed in another 100mL beaker; the material in the reactor is cooled to 10°C by a low-temperature coolant circulation pump, and then the hydrogen peroxide is dripped in 20min, and the KOH aqueous solution is dripped in 30min After the addition is completed, continue to react at 10°C for 5 hours; stop stirring, transfer the reaction solution to a 2L beaker, let it stand for 1 hour, transfer the upper clear liquid to another beaker, and discard the lower alkali solution; add dilute hydrochloric acid to the clear liquid to adjust the pH to 2, and then add 3 times the volume of deionized water under stirring. The viscous liquid condensed on the bottom and wall of the beaker is the crude product; the crude product is further dissolved in acetone and continues to condense in deionized water. The obtained product is dried in a vacuum oven to constant weight to obtain a refined product, a carboxyl-terminated low molecular weight liquid fluoroelastomer A, in the form of a colorless viscous liquid.

[0067] The low molecular weight fluorine-containing elastomer used in Examples 15-17 is a carboxyl-terminated liquid fluorocarbon elastomer B, which is a terpolymer of vinylidene fluoride (VDF)-hexafluoropropylene (HFP)-tetrafluoroethylene (TFE), with a copolymer composition of VDF:HFP:TFE in a molar ratio of 43:16:41, a carboxyl content of 4.2wt%, and a number average molecular weight of 1500, and is prepared by the following method:

[0068] 100 g of vinylidene fluoride (VDF)-hexafluoropropylene (HFP)-tetrafluoroethylene (TFE) ternary copolymer elastomer (M n =283300,M w=326100, copolymer composition VDF:HFP:TFE molar ratio = 43:16:41) and 900g of acetone, mechanically stirred until the solid elastomer is completely dissolved; 32g of KOH and 39.8g of deionized water are weighed in a 100mL beaker to prepare a 45% KOH aqueous solution; 60g of 30% hydrogen peroxide is weighed in another 100mL beaker; the material in the reactor is cooled to 10°C by a low-temperature coolant circulation pump, and then the hydrogen peroxide is dripped in 20min, and the KOH is dripped in 30min After the addition is completed, continue to react at 10°C for 5 hours; stop stirring, transfer the reaction solution to a 2L beaker, let it stand for 1 hour, transfer the upper clear liquid to another beaker, and discard the lower alkali solution; add dilute hydrochloric acid to the clear liquid to adjust the pH to 2, and then add 3 times the volume of deionized water under stirring, and the viscous liquid condensed on the bottom and wall of the beaker is the crude product; the crude product is further dissolved in acetone, and continues to condense in deionized water. The obtained product is dried in a vacuum oven to constant weight to obtain a refined product, a carboxyl-terminated low molecular weight liquid fluoroelastomer B, in the form of a colorless viscous liquid.

[0069] The low molecular weight fluorine-containing elastomer used in Examples 18-20 is a hydroxyl-terminated liquid fluorocarbon elastomer C, which is a vinylidene fluoride (VDF)-hexafluoropropylene (HFP) binary copolymer, with a copolymer composition VDF:HFP molar ratio of 78:22 and a number average molecular weight of 2600, and is prepared by the following method:

[0070] Weigh 50g of carboxyl-terminated liquid fluorocarbon elastomer A and dissolve it in 215g of tetrahydrofuran, stirring until it is completely dissolved into a homogeneous fluorocarbon elastomer solution; dissolve 12.68g (0.05mol) of iodine in 67g of tetrahydrofuran to prepare an iodine solution; place a 500mL three-necked flask in an ice-water bath, and add 37.8g of tetrahydrofuran and 3.78g (0.1mol) of sodium borohydride to the flask. After stirring for 5 minutes, add the fluorocarbon elastomer solution and iodine solution in the order of "first glue and then iodine". The specific operation is: slowly add the prepared fluorocarbon elastomer solution to the reaction flask, which takes about 1 hour; after stirring and reacting for 1 hour, continue to add the iodine solution, which takes about 1 hour. After continuing to stir and react for 1 hour, heat the system to the reflux temperature of 70°C and reflux for 5 hours. After the reaction is completed, the reaction is terminated, the system is cooled to room temperature, an appropriate amount of dilute hydrochloric acid is added to quench the residual sodium borohydride in the system, and an appropriate amount of sodium sulfite solution is added to remove the residual iodine, and the system is adjusted to neutral. Subsequently, 70-80% of the tetrahydrofuran solvent in the system is removed by rotary evaporation, the rotary evaporation temperature is 40°C, the speed is 30rpm, and the rotary evaporation time is 2h, and then 4-5 times the volume of deionized water is added for washing 3 times, and finally placed in a vacuum oven to dry to constant weight, to obtain a low molecular weight hydroxyl-terminated fluorocarbon elastomer C in the state of a colorless to light yellow viscous liquid.

[0071] The low molecular weight fluorine-containing elastomer used in Examples 21-23 is a hydroxyl-terminated liquid fluorocarbon elastomer, which is a terpolymer of vinylidene fluoride (VDF)-hexafluoropropylene (HFP)-tetrafluoroethylene (TFE), with a copolymer composition VDF:HFP:TFE molar ratio of 43:16:41 and a number average molecular weight of 1500, and is prepared by the following method:

[0072] Weigh 50g of carboxyl-terminated liquid fluorocarbon elastomer B and dissolve it in 215g of tetrahydrofuran, stirring until it is completely dissolved into a homogeneous fluorocarbon elastomer solution; dissolve 5.92g of iodine in 67g of tetrahydrofuran to prepare an iodine solution; place a 500mL three-necked flask in an ice-water bath, and add 37.8g of tetrahydrofuran and 5.29g of sodium borohydride to the flask. After stirring for 5 minutes, add the fluorocarbon elastomer solution and iodine solution in the order of "first glue and then iodine". The specific operation is: slowly add the prepared fluorocarbon elastomer solution to the reaction bottle, which takes about 1 hour; after stirring and reacting for 1 hour, continue to add the iodine solution, which takes about 1 hour. After continuing to stir and react for 1 hour, heat the system to the reflux temperature of 70°C and reflux for 5 hours. After the reaction is completed, the reaction is terminated, the system is cooled to room temperature, an appropriate amount of dilute hydrochloric acid is added to quench the residual sodium borohydride in the system, and an appropriate amount of sodium sulfite solution is added to remove the residual iodine, and the system is adjusted to neutral. Subsequently, 70-80% of the tetrahydrofuran solvent in the system is removed by rotary evaporation, the rotary evaporation temperature is 40°C, the speed is 30rpm, and the rotary evaporation time is 2h, and then 4-5 times the volume of deionized water is added for washing 3 times, and finally placed in a vacuum oven to dry to constant weight, to obtain a low molecular weight hydroxyl-terminated fluorocarbon elastomer D in the state of a colorless to light yellow viscous liquid.

[0073] Example 1

[0074] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0075] Introduce 10g G-101 and 90g methyl isobutyl ketone into a 250mL three-necked flask, stir and dissolve at room temperature to form a colorless transparent solution with a concentration of 10wt%, then add 0.985g magnesium oxide and 1.5g ethanolamine, wherein the molar ratio of ethanolamine to the vinylidene fluoride structural unit in G-101 is 1:4; react at 110°C for 12h to terminate the reaction. Add a small amount of deionized water to the reaction solution, let it stand for stratification, take the upper layer of liquid and wash it repeatedly three times, pour the obtained solution into a rotary evaporator, and rotary evaporate at 95°C. When the solvent in the solution is less, pour it into a 100mL beaker and place it in a vacuum oven to dry to constant weight to obtain a high-functionality liquid fluoroelastomer in a dark brown state.

[0076] Figure 1 The infrared spectrum (FT-IR) test results of the prepared high-functionality low-molecular-weight liquid fluoroelastomer are shown in Figure 2. Figure 1It can be seen that the side hydroxyl fluorocarbon oligomer and G-101 are both at 870-890 cm -1 1170~1200cm -1 1390~1400cm -1 The characteristic absorption peaks of fluorinated polymers appeared at 3344 cm -1 The stretching vibration peak of -OH appeared at , indicating that the double bond reacted with amino alcohol to introduce -OH on the side group, proving the synthesis of side hydroxyl fluorocarbon oligomer.

[0077] Example 2

[0078] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0079] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 1, except that the temperature of the reaction system is 25°C.

[0080] Example 3

[0081] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0082] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 1, except that the reaction system temperature is 60°C.

[0083] Example 4

[0084] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0085] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 1, except that 2.25 g of ethanolamine is added to the reaction, and the molar ratio of ethanolamine to the vinylidene fluoride structural unit in G-101 is 1.5:4.

[0086] Example 5

[0087] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0088] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 1, except that 3 g of ethanolamine is added to the reaction, and the molar ratio of ethanolamine to the vinylidene fluoride structural unit in G-101 is 2:4.

[0089] Example 6

[0090] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0091] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 1, except that the added alcohol amine is 3-aminopropanol with a mass of 1.87 g, and the molar ratio of 3-aminopropanol to the vinylidene fluoride structural unit in G-101 is 1:4.

[0092] Example 7

[0093] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0094] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 6, except that the mass of the added 3-aminopropanol is 2.81 g, and the molar ratio of 3-aminopropanol to the vinylidene fluoride structural unit in G-101 is 1.5:4.

[0095] Example 8

[0096] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0097] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is substantially the same as that of Example 6, except that the mass of the added 3-aminopropanol is 3.75 g, and the molar ratio of 3-aminopropanol to the vinylidene fluoride structural unit in G-101 is 2:4.

[0098] Example 9

[0099] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0100] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is basically the same as that of Example 1, except that the added alcohol amine is 4-amino-1-butanol with a mass of 2.18 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in G-101 is 1:4.

[0101] Example 10

[0102] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0103] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is basically the same as that of Example 9, except that the mass of the added 4-amino-1-butanol is 3.28 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in G-101 is 1.5:4.

[0104] Embodiment 11

[0105] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0106] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is basically the same as that of Example 9, except that the mass of the added 4-amino-1-butanol is 4.36 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in G-101 is 2:4.

[0107] Example 12

[0108] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0109] Introduce 10g of carboxyl-terminated liquid fluoroelastomer A and 90g of methyl isobutyl ketone into a 250mL three-necked flask, stir and dissolve at room temperature to form a colorless transparent solution with a concentration of 10wt%, then add 0.985g of magnesium oxide and 2.13g of 4-amino-1-butanol, wherein the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer A is 1:4; react at 110°C for 12h to terminate the reaction. Add a small amount of deionized water to the reaction solution, let it stand for stratification, take the upper layer of liquid and wash it repeatedly three times, pour the obtained solution into a rotary evaporator, and rotary evaporate at 95°C. When there is less solvent in the solution, pour it into a 100mL beaker and place it in a vacuum oven to dry to constant weight to obtain a high-functionality, low-molecular-weight liquid fluoroelastomer in a dark brown state.

[0110] Embodiment 13

[0111] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0112] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 12, except that the mass of the added 4-amino-1-butanol is 3.2 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer A is 1.5:4.

[0113] Embodiment 14

[0114] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0115] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 12, except that the mass of the added 4-amino-1-butanol is 4.25 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer A is 2:4.

[0116] Embodiment 15

[0117] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0118] Introduce 10g of carboxyl-terminated liquid fluoroelastomer B and 90g of methyl isobutyl ketone into a 250mL three-necked flask, stir and dissolve at room temperature to form a colorless transparent solution with a concentration of 10wt%, then add 0.985g of magnesium oxide and 1.17g of 4-amino-1-butanol, wherein the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer B is 1:4; react at 110°C for 12h to terminate the reaction. Add a small amount of deionized water to the reaction solution, let it stand for stratification, take the upper layer of liquid and wash it repeatedly three times, pour the obtained solution into a rotary evaporator, and rotary evaporate at 95°C. When there is less solvent in the solution, pour it into a 100mL beaker and place it in a vacuum oven to dry to constant weight to obtain a high-functionality liquid fluoroelastomer in a dark brown state.

[0119] Example 16

[0120] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0121] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 15, except that the mass of the added 4-amino-1-butanol is 1.76 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer B is 1.5:4.

[0122] Embodiment 17

[0123] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0124] The preparation method of the high-functionality low-molecular-weight liquid fluoroelastomer is basically the same as that of Example 15, except that the mass of the added 4-amino-1-butanol is 2.34 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer B is 2:4.

[0125] Embodiment 18

[0126] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0127] Introduce 10g of hydroxyl-terminated liquid fluoroelastomer C and 90g of methyl isobutyl ketone into a 250mL three-necked flask, stir and dissolve at room temperature to form a colorless transparent solution with a concentration of 10wt%, then add 0.985g of magnesium oxide and 2.13g of 4-amino-1-butanol, wherein the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer C is 1:4; react at 110°C for 12h to terminate the reaction. Add a small amount of deionized water to the reaction solution, let it stand for stratification, take the upper layer of liquid and wash it repeatedly three times, pour the obtained solution into a rotary evaporator, and rotary evaporate at 95°C. When there is less solvent in the solution, pour it into a 100mL beaker and place it in a vacuum oven to dry to constant weight to obtain a high-functionality liquid fluoroelastomer in a dark brown state.

[0128] Embodiment 19

[0129] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0130] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 18, except that the mass of the added 4-amino-1-butanol is 3.2 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the terminal carboxyl liquid fluoroelastomer C is 1.5:4.

[0131] Embodiment 20

[0132] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0133] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 18, except that the mass of the added 4-amino-1-butanol is 4.25 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the terminal carboxyl liquid fluoroelastomer C is 2:4.

[0134] Embodiment 21

[0135] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0136] Introduce 10g of hydroxyl-terminated liquid fluoroelastomer D and 90g of methyl isobutyl ketone into a 250mL three-necked flask, stir and dissolve at room temperature to form a colorless transparent solution with a concentration of 10wt%, then add 0.985g of magnesium oxide and 1.17g of 4-amino-1-butanol, wherein the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the carboxyl-terminated liquid fluoroelastomer D is 1:4; react at 110°C for 12h to terminate the reaction. Add a small amount of deionized water to the reaction solution, let it stand for stratification, take the upper layer of liquid and wash it repeatedly three times, pour the obtained solution into a rotary evaporator, and rotary evaporate at 95°C. When there is less solvent in the solution, pour it into a 100mL beaker and place it in a vacuum oven to dry to constant weight to obtain a high-functionality liquid fluoroelastomer in a dark brown state.

[0137] Embodiment 22

[0138] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0139] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 21, except that the mass of the added 4-amino-1-butanol is 1.76 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the terminal carboxyl liquid fluoroelastomer D is 1.5:4.

[0140] Embodiment 23

[0141] This example provides a method for preparing a high-functionality, low-molecular-weight liquid fluoroelastomer.

[0142] The preparation method of the high-functionality liquid fluoroelastomer is basically the same as that of Example 21, except that the mass of the added 4-amino-1-butanol is 2.34 g, and the molar ratio of 4-amino-1-butanol to the vinylidene fluoride structural unit in the terminal carboxyl liquid fluoroelastomer D is 2:4.

[0143] Comparative Example 1

[0144] G-101 from Japan's Daikin Corporation was used as a comparative example.

[0145] Comparative Example 2

[0146] Carboxyl-terminated liquid fluoroelastomer A was used as a comparative example.

[0147] Comparative Example 3

[0148] Carboxyl-terminated liquid fluoroelastomer B was used as a comparative example.

[0149] Comparative Example 4

[0150] The hydroxyl-terminated liquid fluoroelastomer C was used as a comparative example.

[0151] Comparative Example 5

[0152] The hydroxyl-terminated liquid fluoroelastomer D was used as a comparative example.

[0153] Effect Example 1

[0154] Yield:

[0155] Where m1 is the total mass of the reactants before the reaction; m2 is the mass of the products after the reaction.

[0156] Functionality f: f = f1 + f2

[0157] Side group functionality f1: x = m + n + p + r

[0158]

[0159] End group functionality f2:

[0160] (When the carboxyl-terminated liquid fluoroelastomer is reduced to the hydroxyl-terminated liquid fluoroelastomer, the functionality does not change)

[0161] Among them, M n is the number average molecular weight of the liquid fluoroelastomer raw material;

[0162] 64 is the molecular weight of the vinylidene fluoride structural unit;

[0163] 100 is the molecular weight of tetrafluoroethylene structural unit;

[0164] 150 is the molecular weight of the hexafluoropropylene structural unit;

[0165] 154 is the molecular weight of the perfluoromethyl vinyl ether structural unit;

[0166] 45 is the molecular weight of -COOH;

[0167] -COOH% is the carboxyl content;

[0168] The specific method for determining -COOH% is as follows: weigh 0.6g of sample and dissolve it in 30mL of acetone, prepare and calibrate KOH-C2H5OH solution as the titrant according to the content described in GB / T 601-2016, and titrate with bromocresol purple as the indicator. The end point of the titration is when the solution changes from yellow to light blue. The carboxyl content is calculated according to the following formula:

[0169] -COOH%=(V×C×45.02) / m

[0170] Where: V-volume of KOH-C2H5OH used for titration, mL;

[0171] Concentration of C-KOH-C2H5OH standard titration solution, mol / L;

[0172] m-mass of the test sample, mg.

[0173] m, n, p, r see formula I.

[0174] m / q: H NMR spectrum

[0175] Taking ethanolamine when x=2 as an example, the m / q calculation method is as follows

[0176]

[0177] Among them, ∫3.6~3.65ppm is the integral of -CH2 close to -OH in -NHCH2CH2OH in the side hydroxyl fluorocarbon oligomer, and ∫2.3~3.4ppm is the integral of the -CH2- structure in the main chain of the side hydroxyl fluorocarbon oligomer.

[0178] Table 1

[0179]

[0180]

[0181] It can be seen from the results in Table 1 that after the hydroxyl group is introduced into the side group, the functionality of the present invention is improved compared with the raw material, and the yield is above 70%.

[0182] Effect Example 2

[0183] The high-functionality, low-molecular-weight liquid fluoroelastomers of Examples 1-23 and the elastomers of Comparative Examples 1-4 were mixed with a chain extender, 1,4-butanediol, and a curing agent, HDI trimer (wherein the value of n(-NCO) / [n(-COOH)+n(-OH)] is 2, and n is the number of moles), and stirred evenly under an overhead mechanical stirrer. 1%wt of dibutyltin dilaurate was added dropwise, and the mixture was stirred evenly with planetary stirring and degassing for 3 minutes. The mixture was poured into a mold, cured at 100°C for 4 hours in a hot press, and then taken out to obtain a cured product.

[0184] The tensile properties were tested using a universal testing machine from Meters Industrial Systems (China) Co., Ltd. According to the provisions of GB / T528-2009, a type 3 dumbbell specimen standard was selected, the tensile rate was 200 mm / min, and the test environment was room temperature (25±2°C); according to the provisions of GB / T 531.1-2008, a Shore A durometer was used to test the hardness.

[0185] The test results are shown in Table 2.

[0186] Table 2

[0187]

[0188] It can be seen from the results in Table 2 that after the hydroxyl group is introduced into the side group of the present invention, due to the improvement of functionality, the number of cross-linking sites increases, and a more compact cross-linked network structure is formed after curing. Compared with the raw material liquid fluoroelastomer, the tensile strength is improved while the elongation at break does not decrease significantly. The high degree of cross-linking leads to a higher hardness.

[0189] Effect Example 3

[0190] The solvent immersion method was used to study the solvent resistance of the cured product, and whether its solvent resistance was excellent was examined based on the mass change rate of the cured product before and after immersion.

[0191] The formula for calculating the mass change rate is:

[0192]

[0193] Wherein, m1 is the mass of the cured product sample before immersion, g;

[0194] m2 is the mass of the cured product sample after immersion, g.

[0195] The mass change rate of the cured product after immersion in strong acid, strong base and polar solvent for 72 hours is shown in Table 3.

[0196] Table 3

[0197]

[0198]

[0199] It can be seen from the results in Table 3 that when the immersion time is as long as 72 hours, the mass change rate does not exceed 15%, and in alkaline solvents and polar solvents, the mass change rate does not exceed 5%, indicating that a stable three-dimensional network cross-linked structure is formed after curing, which can resist the attack of external atoms and has excellent solvent resistance.

[0200] Effect Example 4

[0201] The cured products of Examples 5, 8 and 11 were subjected to thermal gravimetric tests. 5% =370-385℃, T 10% =390-412℃, the residual carbon rate is 30-36.4% at 800℃.

[0202] G101 of Comparative Example 1: T 5% =318℃, T 10% =385℃, the residual carbon rate is 0 at 800℃.

[0203] Therefore, the cured products of the embodiments of the present invention have improved thermal stability.

[0204] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A liquid fluoroelastomer, characterized in that The structural formula of the liquid fluoroelastomer is shown in Formula I: Wherein, R1 is -NH(CH2) x OH, R2 is a non-reactive terminal group, a carboxyl group or a hydroxyl group; x is 1-6; The ratio between m and q is 4-25:

1.

2. The liquid fluoroelastomer according to claim 1, wherein x is 2-4, preferably 3; Preferably, the ratio between m and q is 4.36-23.4:1, preferably 8.84-17.49:1, and more preferably 14.65-17.49:

1.

3. The liquid fluoroelastomer according to claim 1 or 2, wherein The functionality of the liquid fluoroelastomer is above 2.5, preferably above 4.

4. The liquid fluoroelastomer according to any one of claims 1 to 3, wherein The liquid fluoroelastomer is selected from at least one of a side hydroxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl terminal hydroxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl terminal carboxyl vinylidene fluoride-hexafluoropropylene copolymer, a side hydroxyl terminal hydroxyl vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene terpolymer and a side hydroxyl terminal carboxyl vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene terpolymer.

5. A method for preparing a liquid fluoroelastomer according to any one of claims 1 to 4, characterized in that: The method comprises: mixing a fluorine-containing elastomer solution, magnesium oxide and an alcohol amine to react to obtain the liquid fluorine elastomer; Wherein, the fluorine-containing elastomer has no pendant hydroxyl groups.

6. The method according to claim 5, wherein: The fluorine-containing elastomer is a binary, ternary or multi-component copolymer of vinylidene fluoride, preferably G-101 of Daikin Corporation of Japan, a carboxyl-terminated liquid fluorine elastomer or a hydroxyl-terminated liquid fluorine elastomer; Preferably, the solvent in the fluorine-containing elastomer solution is an organic solvent, preferably at least one selected from methyl isobutyl ketone, tetrahydrofuran and acetone; Preferably, the alcoholamine is selected from at least one of ethanolamine, 3-aminopropanol and 4-amino-1-butanol, preferably 3-aminopropanol.

7. The method according to claim 5 or 6, wherein: The molar ratio of the alcohol amine to the vinylidene fluoride structural unit in the fluorine-containing elastomer is 0.5-4:4, preferably 1-3:4, more preferably 1.5-2:4, and most preferably 2:

4.

8. The method according to any one of claims 5 to 7, wherein: The reaction time is 3-15h, preferably 8-12h; Preferably, the reaction temperature is 20-120°C, preferably 25-116°C, and more preferably 25°C, 60°C or 110°C; Preferably, after the reaction is completed, the system is cooled to room temperature, the inorganic salt and residual alcohol amine are extracted to remove, the solvent is removed by rotary evaporation, and the final product is obtained after drying.

9. A liquid fluoroelastomer prepared according to the method of any one of claims 5 to 8.

10. Use of the liquid fluoroelastomer according to any one of claims 1 to 4 and 9 in the preparation of special adhesives, sealants and coatings.

Citation Information

Patent Citations

  • Preparation method of carboxyl-terminated liquid fluorine polymer

    CN101717464A

  • Laboratory-scale synthesizing and curing method of terminal carboxyl liquid fluorine elastomer

    CN105968247A

  • Fluororubber / polyhydroxy fluororubber-based polyurethane interpenetrating network reinforcing material and preparation method thereof

    CN111621107A

  • Wear-resistant oil-proof protective film and preparation method thereof

    CN115286834A

  • Preparation method of fluorine-containing pressure-sensitive silica gel

    CN117603648A