Semi-hydrogenated bio-based terpene and conjugated diene multi-element random copolymerized elastomer as well as preparation method and application thereof

Through the preparation of semi-hydrogenated bio-based terpenes and conjugated diene polyvarious random interpolymers, the problem of insufficient research on bio-based polymer materials in the existing hydrogenation research system was solved, and a semi-based with high wet resistance and excellent mechanical properties was obtained. Hydrogenated elastomers are suitable for industrial production and have promoted the development of polymer materials.

CN118930736AActive Publication Date: 2024-11-12QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411002686.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing hydrogenation research system has insufficient research on bio-based polymer materials, resulting in the lack of hydrogenated elastomers with high wet resistance and excellent mechanical properties.

Method used

The semihydrogenated bio-based terpene and conjugated diene polyvariate random interpolymer is used to copolymerize the conjugated diene monomer and the bio-based terpene monomer and undergo hydrogenation treatment to prepare a semihydrogenation elasticity with a hydrogenation degree of 30-60%. The hydrogenation reaction conditions are controlled to obtain materials with excellent mechanical properties in combination with Ziegler-Natta hydrogenation reaction system or metallocene hydrogenation reaction system.

Benefits of technology

It has achieved the preparation of semi-hydrogenated elastomers with excellent mechanical properties, anti-slip properties and non-deformation, which is suitable for industrial production, and fills the gap in research on bio-based hydrogenated elastomers, and promotes the development of polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930736A_ABST
    Figure CN118930736A_ABST
Patent Text Reader

Abstract

The invention discloses a semi-hydrogenated bio-based terpene and conjugated diene multi-element random copolymerized elastomer as well as a preparation method and application thereof. The invention belongs to the field of olefin catalytic polymerization and hydrogenation. The invention aims to solve the technical problem that the existing hydrogenated rubber material generally does not have good skid resistance and mechanical properties. The elastomer is formed by copolymerization and hydrogenation of at least one of conjugated diene monomers and at least one of bio-based terpene monomers, and the hydrogenation degree is 40-55%. According to the invention, bio-based terpene and conjugated diene monomers are copolymerized and then hydrotreated, and the hydrogenation process is controlled, so that the bio-based semi-hydrogenated elastomer with only a half of hydrogenation degree is finally obtained, and the elastomer has all properties of elastomers and plastics due to long side chains and only a half of hydrogenation degree; the elastomer has excellent mechanical properties, weather resistance and skid resistance, the whole preparation process is simple, the yield is high, and the elastomer is very suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of olefin catalytic polymerization and hydrogenation, and specifically relates to a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer and a preparation method and application thereof. Background Art

[0002] The rapid development of industrialization and motorization has led to an increase in demand for fossil fuels such as oil, while the consumption of fossil energy has brought more greenhouse gas emissions. Traditional fossil energy seems to be insufficient in the face of the growing needs of national defense and people's livelihood. Countries around the world are in urgent need of seeking more efficient, low-cost and sustainable alternative resources. Biomass energy is currently believed to be able to replace fossil energy to a certain extent. It mainly converts solar energy, carbon dioxide and water into corresponding bio-based compounds through plant photosynthesis. This bio-based compound will emit water and carbon dioxide during use, forming a theoretically zero carbon dioxide emission and recyclable process. Therefore, bio-based compounds are also recognized as the only solar energy that can be stored, and it is also an environmentally friendly renewable energy that is economically feasible and effectively solves global environmental pollution and other problems. This type of bio-based energy has great potential to replace fossil energy to a certain extent.

[0003] Countries around the world are now actively implementing policies to use biomass resources to refine and produce bio-based fuels and chemicals, and some bio-based polymer materials have been used in production and life, such as in medical and packaging materials. A relatively saturated elastomer can be obtained by special hydrogenation treatment of bio-based polymer materials such as terpenes myrcene and farnesene. Because the polymer chain structure has a certain degree of saturation, the hydrogenated rubber material has good oil resistance (good resistance to fuel oil, lubricating oil, and aromatic solvents); and this saturated structure also makes the rubber material have excellent heat resistance, chemical corrosion resistance (good resistance to acid and alkali Freon), ozone resistance, compression permanent deformation resistance, etc.; at the same time, because bio-based terpenes such as β-myrcene and β-farnesene have longer side chains, they have better anti-slip properties. However, the current research and development of hydrogenated rubber materials is limited to polymer materials based on fossil energy, and there is almost no research on bio-based polymers. Therefore, the exploration of hydrogenation of bio-based polymer materials is of great scientific significance and industrial value. Summary of the invention

[0004] The purpose of the present invention is to solve the problem of insufficient research in the existing hydrogenation research system, to provide a semi-hydrogenated elastomer with high anti-skid property and excellent mechanical properties, and finally to propose a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer and its preparation method and application.

[0005] The technical solution of the present invention is as follows:

[0006] One of the purposes of the present invention is to provide a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, wherein the elastomer is copolymerized and hydrogenated by at least one of the conjugated diene monomers and at least one of the bio-based terpene monomers, has a hydrogenation degree of 30 to 60%, a number average molecular weight of 10,000 to 500,000 g / mol, a molecular weight distribution of 1.0 to 5.0, a molar content of conjugated diene polymerized units of 5 to 95%, and a molar mass of bio-based terpene polymerized units of 5 to 95%.

[0007] Preferably, the conjugated diene monomers include 1,3-butadiene, isoprene, 1,5-hexadiene, 1,7-octadiene, and the bio-based terpene monomers are monoterpene and / or sesquiterpene.

[0008] More preferably, the conjugated diene monomer is 1,3-butadiene or isoprene.

[0009] Further preferably, the monoterpene is geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral or menthol, and the sesquiterpene is cadinene, α-farnesene, β-farnesene, cedrene or caryophyllene.

[0010] Most preferably, the monoterpene is β-myrcene and the sesquiterpene is β-farnesene.

[0011] Preferably, the degree of hydrogenation is 45-52%, the molecular weight distribution is 1.9-3.2, the molar content of the conjugated diene polymerized units is 10-90%, and the molar mass of the bio-based terpene polymerized units is 10-90%.

[0012] Preferably, the glass transition temperature range is -80 to 0°C, the tanδ value at 0°C is 0.7 to 1.3, the tear strength is >28N / mm, the elongation at break is >520%, the Shore hardness A is >40, the heat deformation temperature is >80°C, and the brittle temperature is <-35°C.

[0013] Further preferably, the glass transition temperature range is -55 to -19°C, the tanδ value at 0°C is 0.96 to 1.21, the tear strength is >32N / mm, the elongation at break is >560%, the Shore hardness A is >51, the heat deformation temperature is >96°C, and the brittle temperature is <-43°C.

[0014] The second object of the present invention is to provide a method for preparing a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, the method being carried out according to the following steps:

[0015] (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer;

[0016] (2) dissolving the multi-component random copolymer in a solvent to obtain a copolymer solution, using a Ziegler-Natta hydrogenation reaction system, in an argon atmosphere, sequentially adding the copolymer solution, a catalyst and a co-catalyst into a dry high-temperature reactor, replacing the gas in the reactor three times with hydrogen, reacting for 1 to 3 hours at a reactor speed of 100 to 1000 rpm, a hydrogenation reaction pressure of 1 to 3 MPa, and a temperature of 10° C. to 40° C., to obtain a semi-hydrogenated bio-based terpene and conjugated diene multi-component random copolymer;

[0017] Alternatively, a metallocene hydrogenation reaction system is used, and in an argon atmosphere, a copolymer solution and a bis(titanate)-alkylaluminum / lithium-based metal compound composite catalyst are sequentially added to a dry high-temperature reactor, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100 to 1500 rpm, the hydrogenation reaction pressure is 0.1 to 1.5 MPa, the temperature is increased to 10°C to 60°C, and the reaction is carried out for 1 to 2 hours to obtain a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer.

[0018] Preferably, the copolymerization in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization.

[0019] Preferably, the specific process of anionic polymerization is adopted:

[0020] Under anhydrous and oxygen-free conditions, the copolymerization is initiated under the conditions of an organic alkali metal as an initiator and / or an organic aluminum compound as a co-catalyst. Further preferably, the organic alkali metal is one or more of n-butyl lithium, sec-butyl lithium, tert-butyl lithium, lithium tert-butoxide, methyl lithium, ethyl lithium, n-propyl lithium, isopropyl lithium, phenyl lithium, benzyl lithium, and naphthalene lithium, and the organic aluminum compound is abbreviated as AB, wherein A represents one or more of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, or sesquiethyl aluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol, or 2,6-di-tert-butyl-4-ethylphenol, and the reaction temperature is -50°C to 70°C, and the reaction time is 10min to 360min. More preferably, the reaction temperature is 30°C to 50°C, and the reaction time is 30min to 120min.

[0021] Preferably, the coordination polymerization method includes iron coordination polymerization, Zignata-type catalyst system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalyst polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, and cobalt catalyst system polymerization.

[0022] Further preferably, the specific process of using the iron coordination polymerization method is:

[0023] Under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent are added to a reactor, and the polymerization reaction is stirred at -30 to 100°C for 10 to 120 minutes. More preferably, the reaction temperature is -20°C to 30°C, and the reaction time is 30 minutes. The iron catalyst is any one of the following structural formulas:

[0024]

[0025] Preferably, the concentration of the copolymer solution in step (2) is 10 wt %, and the solvent of the copolymer solution is one or more of toluene, xylene, n-hexane, and cyclohexane.

[0026] Preferably, the catalyst in the Ziegler-Natta hydrogenation reaction system is one or more of palladium dichloride, platinum dichloride, platinum tetrachloride, vanadium trichloride, cobalt chloride, titanium tetrachloride, nickel chloride, and nickel naphthenate. More preferably, the catalyst is nickel naphthenate.

[0027] Preferably, the cocatalyst is an organometallic compound of a metal from Group IA to Group IIIA. Further preferably, the cocatalyst is one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, aluminum tert-butoxide, aluminum nitrate, dimethylaluminum chloride, diisobutylaluminum hydride, and methylaluminoxane.

[0028] Preferably, the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-500):1, and the molar ratio of the catalyst to the co-catalyst is 1:(1-9).

[0029] Preferably, the dititanium ocene in the metallocene hydrogenation reaction system includes dichlorotitanium ocene, and the alkyl aluminum is one or more of trimethyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, triethyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, and diisobutyl aluminum hydride. More preferably, the alkyl aluminum is triisobutyl aluminum. The lithium metal compound is one or more of lithium hydride, lithium isopropoxide, ethyl lithium, isopropyl lithium, lithium carbonate, lithium amide, lithium sulfate, and lithium aluminum hydroxide. More preferably, the lithium metal compound is lithium hydride.

[0030] Preferably, the mass ratio of the copolymer to the bis(trifluoromethyl)titanium in the copolymer solution is (1-6000):1, the molar ratio of the bis(trifluoromethyl)titanium to the alkylaluminum compound is 1:(1-9), and the molar ratio of the bis(trifluoromethyl)titanium to the lithium metal compound is 1:(1-10).

[0031] The third object of the present invention is to provide an elastomer having high mechanical-anti-slip properties and low deformation resistance, which is obtained by vulcanizing the above-mentioned semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer.

[0032] Preferably, the elastomer having high mechanical-anti-slip-resistant properties and low deformation resistance has a Shore A hardness of >40, a rebound elastic modulus of >20%, a breaking elongation of >300%, and a tear strength of >20 N / mm.

[0033] A fourth object of the present invention is to provide a method for preparing an elastomer having high mechanical-anti-slip properties and low deformation resistance, the method comprising:

[0034] 100 parts of semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, 5 to 70 parts of carbon black, 1 to 4 parts of vulcanization accelerator, 0.1 to 10 parts of sulfur, 1 to 8 parts of zinc oxide, 1 to 10 parts of zinc stearate, 0.5 to 5 parts of antioxidant and 1 to 20 parts of filler oil are weighed by mass, mixed, kneaded and vulcanized.

[0035] Preferably, the carbon black is one or more of N324, N110, and N320; the vulcanization accelerator is one or more of NS, NA-22, NOBS, CZ, and DCBS; the antioxidant is one or more of quinoline, p-phenylenediamine, or naphthylamine; and the filler oil is one or more of paraffin oil, cyclohexane oil, or aromatic oil.

[0036] A fifth object of the present invention is to provide an elastomer having high mechanical-anti-slip properties and low deformation resistance for use in the fields of industrial materials, building materials, and daily necessities.

[0037] Compared with the prior art, the present invention has the following advantages:

[0038] The present invention first copolymerizes bio-based terpene monomers with conjugated diene monomers to obtain a multi-component random copolymer, and then hydrogenates the copolymer to finally obtain a bio-based semi-hydrogenated elastomer with only half the degree of hydrogenation. Because the elastomer has a longer side chain and only half the degree of hydrogenation, it has all the properties of an elastomer and a plastic, and has excellent mechanical properties, anti-slip properties, and is not easy to deform. The overall preparation process is simple and the yield is high, and it is very suitable for industrial production. At present, research on bio-based hydrogenated elastomers is basically blank, so the present invention has a high degree of creativity and effectively promotes the development of my country's polymer material field. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The two-component copolymer obtained in Example 1 1 H NMR spectrum;

[0040] Figure 2 The hydrogenated two-component copolymer obtained in Example 1 1 H NMR spectrum;

[0041] Figure 3 This is the GPC spectrum of the hydrogenated two-component copolymer obtained in Example 1;

[0042] Figure 4 The DSC spectrum of the hydrogenated two-component copolymer obtained in Example 1 is shown in FIG. DETAILED DESCRIPTION

[0043] As used in the present invention, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0044] When equivalent, concentration or other value or parameter is represented by range, preferred range or a series of upper preferred value and lower preferred value in the invention, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the range is disclosed separately. For example, when the range "1 to 5" is disclosed, the described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range. In the present application specification and claims, range limits can be combined and / or interchanged, and if these ranges are not otherwise stated, all sub-ranges contained therein are included.

[0045] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0046] The "one embodiment" or "embodiment" of the present invention refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.

[0047] The endpoints and any values ​​of the ranges disclosed in the invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article.

[0048] The present invention provides a semi-hydrogenated bio-based terpene and conjugated diene multi-component random copolymer elastomer. The elastomer is copolymerized and hydrogenated by at least one conjugated diene monomer and at least one bio-based terpene monomer, has a hydrogenation degree of 30-60%, a number average molecular weight of 10,000-500,000 g / mol, a molecular weight distribution of 1.0-5.0, a molar content of conjugated diene polymerized units of 5-95%, and a molar mass of bio-based terpene polymerized units of 5-95%.

[0049] In an optional embodiment, the conjugated diene monomer includes 1,3-butadiene, isoprene, 1,5-hexadiene, 1,7-octadiene. More preferably, the conjugated diene monomer is 1,3-butadiene or isoprene.

[0050] In an optional embodiment, the bio-based terpene monomer is a monoterpene and / or a sesquiterpene. Further preferably, the monoterpene is geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral or menthol, and the sesquiterpene is cadinene, α-farnesene, β-farnesene, cedrene or caryophyllene. Most preferably, the monoterpene is β-myrcene and the sesquiterpene is β-farnesene.

[0051] In an optional embodiment, the degree of hydrogenation is 45-52%, the molecular weight distribution is 1.9-3.2, the molar content of the conjugated diene polymerized units is 10-90%, and the molar mass of the bio-based terpene polymerized units is 10-90%.

[0052] In an optional embodiment, the glass transition temperature range is -80 to 0°C, the tanδ value at 0°C is 0.7 to 1.3, the tear strength is >28N / mm, the elongation at break is >520%, the Shore hardness A is >40, the heat deformation temperature is >80°C, and the brittle temperature is <-35°C.

[0053] In an optional embodiment, the glass transition temperature range is -55 to -19°C, the tanδ value at 0°C is 0.96 to 1.21, the tear strength is >32N / mm, the elongation at break is >560%, the Shore hardness A is >51, the heat deformation temperature is >96°C, and the brittle temperature is <-43°C.

[0054] The present invention also provides a method for preparing a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, which is carried out according to the following steps:

[0055] (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer;

[0056] (2) The multi-component random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated by a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a semi-hydrogenated bio-based terpene and conjugated diene multi-component random copolymer elastomer.

[0057] In an optional embodiment, the preparation of the multi-component random copolymer in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization. More preferably, it is coordination polymerization, anionic polymerization or free radical polymerization. More preferably, it is coordination polymerization or anionic polymerization.

[0058] In an optional embodiment, the coordination polymerization method includes iron coordination polymerization, Zignata-type catalyst system polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, cobalt catalyst system polymerization. Further preferred are iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, cobalt catalyst system polymerization. More preferably, it is iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization. Most preferably, it is iron coordination polymerization.

[0059] In an optional embodiment, when the preparation of the multi-random copolymer adopts the iron coordination polymerization method, the specific steps are: under anhydrous and oxygen-free conditions, add an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent into a reactor, stir the polymerization reaction at -30°C to 100°C for 10min to 120min, add a quencher and an antioxidant after the reaction, wash and vacuum dry to constant weight to obtain a multi-random copolymer of conjugated diene and bio-based terpene.

[0060] In an optional embodiment, the reaction temperature is -20°C to 30°C, more preferably 0°C to 30°C; and the reaction time is 30 min.

[0061] In an optional embodiment, when the iron coordination polymerization method is adopted, the iron catalyst is any one of the following structural formulas:

[0062]

[0063] In an optional embodiment, the solvent is one or more of cyclohexane, n-hexane, petroleum ether, toluene, and xylene, and the ratio of the solvent to the total volume of the comonomer is (1-50):1, more preferably (7-20):1; the molar ratio of the total molar amount of the comonomer to the iron element in the iron catalyst is (100-50000):1, more preferably (150-5000):1.

[0064] In an optional embodiment, the co-catalyst is a single component or a two-component. When the co-catalyst is a single component, the co-catalyst is selected from one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), and modified methylaluminoxane (MMAO). The molar ratio of the aluminum element in the co-catalyst to the iron element in the iron catalyst is (100-1500):1, more preferably 500:1; when the co-catalyst is a two-component, component A is selected from one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, diisobutylaluminum hydride, sesquiethylaluminum chloride, or The present invention relates to a catalyst comprising a plurality of catalysts, wherein the component B is one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), modified methylaluminoxane (MMAO), N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, 4-isopropyl-4'-methyldiphenyl iodide tetrakis(pentafluorophenyl)borate, triphenylphosphine oxide, tris(pentafluorophenyl)phosphine, and triphenylphosphine, the molar ratio of the aluminum element in the component A to the iron element in the iron catalyst is (1-100):1, more preferably 40:1, and the molar ratio of the aluminum, boron or phosphine element in the component B to the iron element in the iron catalyst is (1-20):1, more preferably 1:1.

[0065] In an optional embodiment, when the preparation of the multi-component random copolymer adopts anionic polymerization, the specific steps are: under anhydrous and oxygen-free conditions, using an organic alkali metal as an initiator to initiate copolymerization of a conjugated diene monomer and a bio-based terpene monomer, reacting at a certain temperature for a certain time, adding ethanol to quench the reaction and obtain a polymer product;

[0066] Alternatively, under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator and an organic aluminum compound is used as a co-catalyst to initiate the copolymerization of a conjugated diene monomer and a bio-based terpene monomer. After reacting at a certain temperature for a certain time, ethanol is added to quench the reaction and obtain a polymerization product.

[0067] In an optional embodiment, the organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; further preferably, it is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, and n-propyllithium.

[0068] In an optional embodiment, the reaction temperature is -50°C to 70°C, and the reaction time is 10 min to 360 min; more preferably, the reaction temperature is 30°C to 50°C, and the reaction time is 30 min to 120 min.

[0069] In an optional embodiment, the solvent is one or more of THF, toluene, ethylbenzene, xylene, n-hexane, cyclohexane, dichloromethane, chloroform, ethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and methyl tert-butyl ether; further preferably, the solvent is one or more of THF, toluene, ethylbenzene, n-hexane, cyclohexane, ethylene glycol dimethyl ether, and methyl tert-butyl ether.

[0070] In an optional embodiment, the organoaluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride or sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol or 2,6-di-tert-butyl-4-ethylphenol, and the molar ratio of A to B is (0.1 to 2):1.

[0071] In an optional embodiment, the ratio of the total volume of the solvent to the comonomer is (1-50):1, more preferably 3:1; the molar ratio of the total molar amount of the comonomer to the lithium element in the initiator is (100-50000):1, more preferably 1556:1; the molar ratio of the total molar amount of the comonomer to the aluminum element in the co-catalyst is (13-6250):1, more preferably 195:1.

[0072] In an optional embodiment, when the preparation of the multi-component random copolymer adopts a free radical polymerization method, examples include: hydrogen peroxide polymerization, emulsion polymerization, nitroxide free radical polymerization (NMP), reversible addition chain transfer polymerization (RAFT), etc. Among these methods, nitroxide free radical polymerization (NMP) and reversible addition chain transfer free radical polymerization are preferred; the most preferred is reversible addition chain transfer free radical polymerization, and the initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, azobisisoheptanenitrile, azobishydroxyvaleric acid, dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, and azoisobutylcyanoformamide.

[0073] In an optional embodiment, when the preparation of the multi-component random copolymer adopts a cationic polymerization method, examples thereof include: cationic polymerization of β-myrcene using a dispersible Lewis acid surfactant combination catalyst (LASC) prepared from ytterbium chloride and sodium alkylbenzene sulfonate surfactant; trifluoromethanesulfonate initiation system, boron trifluoride ether initiation system, etc. Among these methods, the LASC polymerization method is preferred.

[0074] In an optional embodiment, the polymerization reaction can be quenched by adding a protic compound such as methanol, a methanol solution of acetic acid, a methanol solution of hydrochloric acid, or an aqueous solution of acetic acid or hydrochloric acid to the reaction solution.

[0075] In an optional embodiment, the concentration of the copolymer solution in step (2) is 10 wt %.

[0076] In an optional embodiment, the solvent of the copolymer solution in step (2) is one or more of toluene, xylene, n-hexane, and cyclohexane.

[0077] In an optional embodiment, when the Ziegler-Natta hydrogenation reaction system is used in step (2), the specific process of hydrogenation is:

[0078] In an argon atmosphere, the copolymer solution, catalyst and co-catalyst are added to a dry high-temperature reactor in sequence, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100-1000rpm, the hydrogenation reaction pressure is 1-3MPa, the temperature is raised to 10℃-40℃, and the reaction is carried out for 1-3h. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer.

[0079] In an optional embodiment, the catalyst is one or more of palladium dichloride, platinum dichloride, platinum tetrachloride, vanadium trichloride, cobalt chloride, titanium tetrachloride, nickel chloride, and nickel cyclohexane, and nickel cyclohexane is most preferred; the co-catalyst is an organic metal compound of a metal from Group IA to Group IIIA, and more preferably one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, aluminum tert-butoxide, aluminum nitrate, dimethylaluminum chloride, diisobutylaluminum hydride, and methylaluminoxane, and most preferably methylaluminoxane.

[0080] In an optional embodiment, the mass ratio of the copolymer and the catalyst in the copolymer solution is (1-500):1, more preferably 350:1; the molar ratio of the catalyst and the co-catalyst is 1:(1-9), more preferably 1:6; the hydrogenation reaction temperature is preferably 25°C; the hydrogenation reaction pressure is preferably 3MPa; the rotation speed of the hydrogenation reactor is preferably 500rpm; and the hydrogenation reaction time is preferably 1.5h.

[0081] In an optional embodiment, the metallocene hydrogenation reaction system in step (2) includes a bis(titaniacin) / lithium hydride / aromatic ester system, a bis(titaniacin) or mono(titaniacin) / triphenyllithium system, a bis(titaniacin) / alkylaluminum / silicate system or a bis(titaniacin) / alkylaluminum / lithium-based metal compound system.

[0082] In an optional embodiment, the specific process of hydrogenation using the bis(triocene)titanium / alkylaluminum / lithium metal compound system is as follows:

[0083] In an argon atmosphere, a copolymer solution and a diocene / alkyl aluminum / lithium metal compound composite catalyst are sequentially added to a dry high-temperature reactor, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100-1500 rpm, the hydrogenation reaction pressure is 0.1-1.5 MPa, the temperature is raised to 10°C-60°C, and the reaction is carried out for 1-2 hours. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer.

[0084] In an optional embodiment, the catalyst dititanocene includes dititanocene dichloride; the co-catalyst alkyl aluminum is one or more of trimethyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, triethyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, and diisobutyl aluminum hydride, more preferably triisobutyl aluminum; the lithium-based metal compound is one or more of lithium hydride, lithium isopropoxide, ethyl lithium, isopropyl lithium, lithium carbonate, lithium amide, lithium sulfate, and lithium aluminum hydroxide, more preferably lithium hydride.

[0085] In an optional embodiment, the mass ratio of the copolymer and the bis(trifluoromethyl)-titanate in the copolymer solution is (1-6000):1, more preferably 4500:1; the molar ratio of the bis(trifluoromethyl)-titanate and the alkylaluminum compound is 1:(1-9), more preferably 1:5; the molar ratio of the bis(trifluoromethyl)-titanate and the lithium metal compound is 1:(1-10), more preferably 1:6; the hydrogenation reaction temperature is preferably 40°C; the hydrogenation reaction pressure is preferably 1MPa; the rotation speed of the hydrogenation reactor is preferably 650rpm; and the hydrogenation reaction time is preferably 1h.

[0086] The present invention first copolymerizes bio-based terpene monomers with conjugated diene monomers to obtain a multi-component random copolymer, and then hydrogenates the copolymer to finally obtain a bio-based semi-hydrogenated elastomer with only half the degree of hydrogenation. Because the elastomer has a longer side chain and only half the degree of hydrogenation, it has all the properties of an elastomer and a plastic, and has excellent mechanical properties, anti-slip properties, and is not easy to deform. The overall preparation process is simple and the yield is high, and it is very suitable for industrial production. At present, research on bio-based hydrogenated elastomers is basically blank, so the present invention has a high degree of creativity and effectively promotes the development of my country's polymer material field.

[0087] The present invention also provides an elastomer with high mechanical-anti-slip properties and low deformation resistance. The elastomer with high mechanical-anti-slip properties and low deformation resistance is vulcanized from the aforementioned semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer.

[0088] In an optional embodiment, after vulcanization, the elastomer has a Shore A hardness greater than 40, a rebound elastic modulus greater than 20%, an elongation at break greater than 300%, and a tear strength greater than 20 N / mm.

[0089] The present invention also provides a method for preparing an elastomer having high mechanical-anti-slip properties and low deformation resistance, the method comprising:

[0090] 100 parts of semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, 5 to 70 parts of carbon black, 1 to 4 parts of vulcanization accelerator, 0.1 to 10 parts of sulfur, 1 to 8 parts of zinc oxide, 1 to 10 parts of zinc stearate, 0.5 to 5 parts of antioxidant and 1 to 20 parts of filler oil are weighed by mass, mixed, kneaded and vulcanized.

[0091] In an optional embodiment, the carbon black is one or more of N324, N110, and N320.

[0092] In an optional embodiment, the vulcanization accelerator is one or more of NS, NA-22, NOBS, CZ, and DCBS.

[0093] In an optional embodiment, the antioxidant is one or more of quinolines, p-phenylenediamines or naphthylamines.

[0094] In an optional embodiment, the extender oil is one or more of paraffin oil, naphthenic oil or aromatic oil.

[0095] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0096] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0097] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0098] When equivalent, concentration or other value or parameter are represented with scope, preferred range or a series of upper preferred value and lower preferred value limit scope in the following examples, this should be understood as specifically disclosing all scopes formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, and no matter whether the scope is disclosed separately. For example, when disclosing scope "1 to 5", described scope should be interpreted as including scope "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, scope limitation can be combined and / or interchanged, and if these scopes are not otherwise stated, all sub-ranges contained therein are included.

[0099] In the following embodiments, the indefinite articles "a" and "an" before the elements or components have no restrictions on the quantity requirements (i.e., the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number obviously refers to the singular form only.

[0100] The "one embodiment" or "embodiment" described in the following embodiments refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.

[0101] The endpoints and any values ​​of the ranges disclosed in the following examples are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article.

[0102] The mechanical properties test standard in the following embodiments is GB / T 589-2009;

[0103] Thermal deformation temperature detection standard: refer to GB / T1634-2019;

[0104] Brittle temperature test standard: Refer to GB / T 5470-2008

[0105] Example 1: The steps of preparing an elastomer having high mechanical-anti-slip properties and low deformation resistance in this example are as follows:

[0106] (1) Polymerization: In an argon atmosphere, anhydrous toluene (120 mL), β-myrcene (0.26 mL, 1.6 mmol, 156 equiv.), isoprene (1.4 mL, 14 mmol, 1400 equiv.), MAO reagent (5.0 mmol, 500 equiv.), and catalyst 5 (1.0 ml, 10 μmol, 1 equiv.) were added to a 250 mL Schlenk tube in sequence, and the polymerization was carried out at 30° C. for 30 min, and then the reaction was terminated with 25 mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1 mL of an antioxidant. After the clear liquid was discarded, the polymer was washed three times with ethanol, and the obtained polymer was placed at 40° C. and vacuum dried to constant weight to obtain an elastomeric polymer.

[0107] (2) Hydrogenation: A n-hexane mother solution (10 wt%) of the copolymer was prepared in a 500 mL Schlenk tube. Catalyst nickel cyclohexane (14.3 mg, 35.6 μmol, 1 equiv.) and co-catalyst methylaluminoxane (18 mL, 1.8 mmol, 6 equiv.) were added to the Schlenk tube in sequence under an argon atmosphere, and the mixture was stirred for 20 mins. The reactor was dried, and 200.0 mL of n-hexane mother solution (10 wt%) of the copolymer and a mixed solution system of the catalyst and co-catalyst were added under an argon atmosphere. The gas was replaced with H2 three times, and the pressure in the reactor was 3 MPa after stamping. Stirring was started, the hydrogenation temperature was 25 ° C, the hydrogenation time was 1.5 h, and the rotation speed was 500 rpm. After the reaction, the hydrogenation reactor was cooled to room temperature, and after the pressure was released, the reactor was opened for 30 mins, and anhydrous ethanol was added and stirred to obtain a hydrogenated white elastomer. The performance test results are shown in Table 1.

[0108] (3) Mixing and vulcanization: 100 parts of the hydrogenated white elastomer prepared in step (2), 45 parts of N220, 2.5 parts of a vulcanizing agent CZ, 2.5 parts of sulfur, 2.5 parts of zinc oxide, 1.5 parts of zinc stearate, 2 parts of an ethoxyquinoline antioxidant (Bermuda Biotechnology Co., Ltd.), and 15 parts of an aromatic oil vulcanization composition were weighed by mass, and finally after mixing and vulcanization, a reinforced semi-hydrogenated β-myrcene-isoprene binary random copolymer composite material was obtained. The mechanical properties test results are shown in Table 2.

[0109] Example 2: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: in step (1), the bio-based terpene monomer is replaced with β-farnesene, the amount of β-farnesene added is (0.04 mL, 0.16 mmol, 15.6 equiv.), the amount of isoprene added is (0.14 mL, 1.4 mmol, 140 equiv.), the amount of anhydrous toluene added as the reaction solvent is (1.8 mL), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0110] Example 3: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: the conjugated diene monomer in step (1) is replaced with 1,3-butadiene, and the amount of 1,3-butadiene added is (1.16 mL, 14 mmol, 1400 equiv.), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before vulcanization are shown in Table 1. The mechanical performance test results of the product after vulcanization are shown in Table 2.

[0111] Example 4: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: the monomer molar ratio in step (1) is changed to: β-myrcene: isoprene = 1:1; β-myrcene (4.2 mL, 25.0 mmol, 2500 equiv.) and isoprene (2.5 mL, 25.0 mmol, 2500 equiv.), the amount of anhydrous toluene added as the reaction solvent is (65 mL), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0112] Example 5: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: the monomer molar ratio in step (1) is changed to β-myrcene:isoprene=9:1; β-myrcene (2.4 mL, 14.0 mmol, 1400 equiv.) and isoprene (0.17 mL, 1.56 mmol, 156 equiv.), the amount of anhydrous toluene added as the reaction solvent is (25.7 mL) and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0113] Example 6: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that anhydrous toluene (70 mL), isoprene (3.5 mL, 35.0 mmol, 3500 equiv.), β-myrcene (1.3 mL, 7.5 mmol, 750 equiv.) and β-farnesene (2.1 mL, 7.5 mmol, 750 equiv.) are used in step (1), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0114] Example 7: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that anhydrous toluene (70 mL), 1,3-butadiene (2.9 mL, 35.0 mmol, 3500 equiv.), β-myrcene (1.3 mL, 7.5 mmol, 750 equiv.) and β-farnesene (2.1 mL, 7.5 mmol, 750 equiv.) are used in step (1), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0115] Example 8: The preparation method of the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: in step (1), anhydrous toluene (124 mL), isoprene (1.75 mL, 17.5 mmol, 1750 equiv.), 1,3-butadiene (1.45 mL, 17.5 mmol, 1750 equiv.), β-myrcene (1.25 mL, 7.5 mmol, 750 equiv.) and β-farnesene (2.05 mL, 7.5 mmol, 750 equiv.) are used, and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0116] Example 9: The method for preparing an elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that the amount of anhydrous toluene added in step (1) is (36 mL), and the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before vulcanization are shown in Table 1. The mechanical performance test results of the product after vulcanization are shown in Table 2.

[0117] Example 10: The method for preparing an elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that: in step (1), the iron catalyst is replaced with No. 1, the addition amount is (1.0 ml, 10 μmol, 1 equiv.), and the reaction temperature is -20°C; the other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0118] Example 11: The method for preparing the elastomer with high mechanical-anti-slip properties and low deformation resistance in this example is different from that in Example 1 in that anionic polymerization is used in step (1), and the other steps and parameters are the same as those in Example 1.

[0119] (1) Polymerization: In an argon atmosphere, anhydrous toluene (5 mL), i-BuAl(BHT) and 1.9 (5mL, 1.6mmol, 8equiv.) aluminum reagent, initiator sec-butyl lithium (0.15mL, 0.2mmol, 1equiv.), β-myrcene (0.26mL, 1.6mmol, 156equiv.) and isoprene (1.4mL, 14mmol, 1400equiv.), polymerized at 25°C for 30min, and then terminated with 5mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1mL of an antioxidant. After pouring off the clear liquid, the polymer was washed three times with ethanol, and the obtained polymer was placed at 40°C and dried in vacuum to constant weight to obtain an elastomeric polymer. The performance test results of the hydrogenated product before vulcanization are shown in Table 1. The mechanical properties test results of the product after vulcanization are shown in Table 2.

[0120] Example 12: The preparation method of the elastomer with high mechanical-anti-slip properties and non-deformability in this example is different from that in Example 1 in that the hydrogenation reaction system in step (2) is replaced with a dipentadienyl titanocene / alkyl aluminum / lithium metal compound hydrogenation system, and the other steps and parameters are the same as in Example 1.

[0121] (2) The hydrogenation process is as follows: a xylene mother solution (10 wt%) of the copolymer is prepared in a 500 mL Schlenk tube. The reactor is dried and heated to 40° C., and 200.0 mL of the xylene mother solution (10 wt%) of the copolymer and a catalyst, dichlorotantalum (4.4 mg, 17.7 μmol, 1 equiv.), and a co-catalyst, triisobutylaluminum (0.08 mL, 88.5 μmol, 5 equiv.), and lithium hydride (0.84 mg, 106.2 μmol, 6 equiv.) are added successively under an argon atmosphere, and the reaction is stirred at 600 rpm for 20 min. H2 is used to replace the gas three times, and the pressure in the reactor is 1 MPa after stamping. Stirring is turned on, the hydrogenation temperature is 40° C., the hydrogenation time is 1 h, and the rotation speed is 650 rpm. After the reaction is completed, the hydrogenation reactor is cooled to room temperature, and after the pressure is released, the reactor is left to stand for 30.0 min, and anhydrous ethanol is added and stirred to obtain a hydrogenated white elastomer. The other steps and parameters are the same as those in Example 1. The performance test results of the hydrogenated product before sulfurization are shown in Table 1. The mechanical performance test results of the product after sulfurization are shown in Table 2.

[0122] Table 1 Physical property test data of semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer before vulcanization

[0123]

[0124]

[0125] Table 2 Mechanical properties test data of the vulcanized products of semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer

[0126]

[0127] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, characterized in that: The elastomer is formed by copolymerizing and hydrogenating at least one of the conjugated diene monomers and at least one of the bio-based terpene monomers, with a hydrogenation degree of 30 to 60%, a number average molecular weight of 10,000 to 500,000 g / mol, a molecular weight distribution of 1.0 to 5.0, a molar content of conjugated diene polymer units of 5 to 95%, and a molar mass of bio-based terpene polymer units of 5 to 95%.

2. The elastic body according to claim 1, characterized in that The conjugated diene monomers include 1,3-butadiene, isoprene, 1,5-hexadiene, and 1,7-octadiene, and the bio-based terpene monomers are monoterpenes and / or sesquiterpenes; wherein the monoterpenes are geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral or menthol, and the sesquiterpenes are cadinene, α-farnesene, β-farnesene, cedrene or caryophyllene.

3. The elastic body according to claim 2, characterized in that The conjugated diene monomer is isoprene or 1,3-butadiene, and the bio-based terpene monomer is β-myrcene or β-farnesene.

4. The elastic body according to claim 1, characterized in that The degree of hydrogenation is 45-52%, the molecular weight distribution is 1.9-3.2, the molar content of the conjugated diene polymerized units is 10-90%, and the molar mass of the bio-based terpene polymerized units is 10-90%.

5. The elastic body according to claim 1, characterized in that The glass transition temperature range is -80 to 0°C, the tanδ value at 0°C is 0.7 to 1.3, the tear strength is >28N / mm, the elongation at break is >520%, the Shore hardness A is >40, the heat deformation temperature is >80°C, and the brittle temperature is <-35°C.

6. The elastic body according to claim 5, characterized in that The glass transition temperature range is -55 to -19°C, the tanδ value at 0°C is 0.96 to 1.21, the tear strength is >32N / mm, the elongation at break is >560%, the Shore hardness A is >51, the heat deformation temperature is >96°C, and the brittle temperature is <-43°C.

7. The method for preparing an elastomer according to any one of claims 1 to 6, characterized in that: The method: (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer; (2) dissolving the multi-component random copolymer in a solvent to obtain a copolymer solution, using a Ziegler-Natta hydrogenation reaction system, in an argon atmosphere, sequentially adding the copolymer solution, a catalyst and a co-catalyst into a dry high-temperature reactor, replacing the gas in the reactor three times with hydrogen, reacting for 1 to 3 hours at a reactor speed of 100 to 1000 rpm, a hydrogenation reaction pressure of 1 to 3 MPa, and a temperature of 10 to 40° C., to obtain a semi-hydrogenated bio-based terpene and conjugated diene multi-component random copolymer; Alternatively, a metallocene hydrogenation reaction system is used, and in an argon atmosphere, a copolymer solution and a di-titanate / alkylaluminum / lithium-based metal compound composite catalyst are added in sequence to a dry high-temperature reactor, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100 to 1500 rpm, the hydrogenation reaction pressure is 0.1 to 1.5 MPa, the temperature is increased to 10 to 60°C, and the reaction is carried out for 1 to 2 hours to obtain a semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer.

8. The method according to claim 7, characterized in that The copolymerization in step (1) adopts anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization.

9. The method according to claim 8, characterized in that The specific process of anionic polymerization is as follows: The copolymerization is initiated under anhydrous and oxygen-free conditions with an organic alkali metal as an initiator and / or an organic aluminum compound as a co-catalyst.

10. The method according to claim 9, characterized in that The organic alkali metal is one or more of n-butyl lithium, sec-butyl lithium, tert-butyl lithium, lithium tert-butoxide, methyl lithium, ethyl lithium, n-propyl lithium, isopropyl lithium, phenyl lithium, benzyl lithium, and naphthalene lithium. The organic aluminum compound is abbreviated as AB, wherein A represents one or more of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, or sesquiethyl aluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol, or 2,6-di-tert-butyl-4-ethylphenol. The reaction temperature is -50 to 70° C., and the reaction time is 10 to 360 min.

11. The method according to claim 10, characterized in that The reaction temperature is 30-50°C, and the reaction time is 30-120 minutes.

12. The method according to claim 8, characterized in that Coordination polymerization methods include iron coordination polymerization, Zignata-type catalytic system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half-sandwich scandium complex polymerization, and cobalt catalytic system polymerization.

13. The method according to claim 12, characterized in that The specific process of using iron coordination polymerization method: Under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent are added into a reactor, and a polymerization reaction is carried out at -30 to 100° C. with stirring for 10 to 120 minutes.

14. The method according to claim 13, characterized in that The reaction temperature is -20 to 30°C and the reaction time is 30 minutes.

15. The method according to claim 13, characterized in that The iron catalyst is any one of the following structural formulas:

16. The method according to claim 7, characterized in that The concentration of the copolymer solution in step (2) is 10 wt %, and the solvent of the copolymer solution is one or more of toluene, xylene, n-hexane, and cyclohexane.

17. The method according to claim 7, characterized in that The catalyst in the Ziegler-Natta hydrogenation reaction system is one or more of palladium dichloride, platinum dichloride, platinum tetrachloride, vanadium trichloride, cobalt chloride, titanium tetrachloride, nickel chloride, and nickel cyclohexaneate; the cocatalyst is an organic metal compound of metals from Group IA to Group IIIA; the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-500):1; and the molar ratio of the catalyst to the cocatalyst is 1:(1-9).

18. The method according to claim 17, characterized in that The catalyst is nickel cyclohexaneate, and the co-catalyst is one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, aluminum tert-butoxide, aluminum nitrate, dimethylaluminum chloride, diisobutylaluminum hydride, and methylaluminoxane.

19. The method according to claim 7, characterized in that The bis-titanocene in the metallocene hydrogenation reaction system includes dichlorobis-titanocene, the alkyl aluminum is one or more of trimethyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, triethyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, and diisobutyl aluminum hydride, the lithium metal compound is one or more of lithium hydride, lithium isopropoxide, ethyl lithium, isopropyl lithium, lithium carbonate, lithium amide, lithium sulfate, and lithium aluminum hydroxide, the mass ratio of the copolymer and the bis-titanocene in the copolymer solution is (1-6000):1, the molar ratio of the bis-titanocene and the alkyl aluminum compound is 1:(1-9), and the molar ratio of the bis-titanocene and the lithium metal compound is 1:(1-10).

20. The method according to claim 19, characterized in that The alkyl aluminum is triisobutyl aluminum, and the lithium metal compound is lithium hydride.

21. An elastomer having high mechanical-anti-slip properties and low deformation resistance, characterized in that: The elastomer described in any one of claims 1 to 6 is vulcanized.

22. The elastic body with high mechanical-anti-slip properties and low deformation resistance according to claim 21, characterized in that: After vulcanization, the Shore A hardness of the elastomer is greater than 40, the rebound elastic modulus is greater than 20%, the elongation at break is greater than 300%, and the tear strength is greater than 20N / mm.

23. The method for preparing an elastomer according to claim 21 or 22, characterized in that: The method: 100 parts of semi-hydrogenated bio-based terpene and conjugated diene multi-random copolymer elastomer, 5 to 70 parts of carbon black, 1 to 4 parts of vulcanization accelerator, 0.1 to 10 parts of sulfur, 1 to 8 parts of zinc oxide, 1 to 10 parts of zinc stearate, 0.5 to 5 parts of antioxidant and 1 to 20 parts of filler oil are weighed by mass, mixed, kneaded and vulcanized.

24. The method according to claim 23, characterized in that The carbon black is one or more of N324, N110, and N320; the vulcanization accelerator is one or more of NS, NA-22, NOBS, CZ, and DCBS; the antioxidant is one or more of quinoline, p-phenylenediamine, or naphthylamine; and the filler oil is one or more of paraffin oil, cyclohexane oil, or aromatic oil.

25. Use of the elastomer according to claim 21 or 22 in the fields of industrial materials, building materials and daily necessities.

Citation Information

Patent Citations

  • Partially hydrogenated styrene-b-conjugated diene / divinyl benzene random copolymer as well as preparation and application thereof

    CN111718454A

  • High-molecular-weight iron-based bio-based rubber, preparation method and application thereof, and rubber composition based on high-molecular-weight iron-based bio-based rubber

    CN115073666A

  • Process for preparing partially hydrogenated butadiene polymers

    US20030092851A1