Urea-formaldehyde resin for fireproof material
Through alkali-acid-base process and chemical graft coating modification of isocyanate acrylate, combined with tri(2-hydroxyethyl) isocyanurate triacrylate, the existing fire-retardant coatings are difficult to take into account both fire-retardant and water-retardant properties. The problem of this problem has achieved efficient fire and waterproofing effects, adapted to high-end market demand and reduced costs.
Patent Information
- Application Number
- CN202411177926.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult for existing fire-retardant coatings to take into account excellent fire resistance and waterproof performance. The water resistance and fire resistance of urea formaldehyde resin do not meet the requirements of the high-end market, and the cost after modification is high, which affects market competitiveness.
The modified urea-formaldehyde resin is prepared by alkali-acid-base process, and the chemical graft coating of isocyanate acrylate and acrylate is modified, combined with tri(2-hydroxyethyl) isocyanurate triacrylate to improve waterproof performance and Maintain the effect of foaming into carbon.
The excellent fire resistance and waterproof performance of modified urea formaldehyde resin in fire-resistant materials is achieved, which reduces costs, adapts to high-end market demands, and improves the stability and durability of the coating.
Abstract
Description
Technical Field
[0001] The invention relates to a urea-formaldehyde resin for fireproof materials, and further, the urea-formaldehyde resin is obtained by chemically coating and modifying melamine-modified urea-formaldehyde resin by using polyacrylate. Background Art
[0002] Intumescent fireproof materials are specifically composed of fireproof sealing strips, fireproof boards, and fireproof coatings. Taking fireproof coatings as an example, it is a fireproof coating made of water-based resin as a film-forming material and a compound intumescent flame retardant that can form a coating with the film-forming material. It is usually used in ancient buildings, wooden villas, high-end wood products, steel structure projects and other places. This kind of coating is both decorative and fireproof. When exposed to fire, the coating can expand to more than dozens of times its original thickness, forming a porous carbonized layer to protect the substrate from burning and has a heat-insulating effect.
[0003] General intumescent flame retardants are usually mixed with catalysts composed of phosphorus-containing substances (phosphorus sources), carbon-forming agents composed of polyhydroxy organic substances (carbon sources), and foaming agents composed of nitrogen-containing organic substances (nitrogen sources), and are added to resins in large quantities. Amino resins (urea-formaldehyde resins, melamine formaldehyde resins, melamine urea-formaldehyde resins) contain rich carbon and nitrogen sources, and are both carbon-forming agents and foaming agents, which can reduce the amount of added flame retardants. Fire-retardant coatings prepared with amino resins as film-forming materials have good foaming properties.
[0004] The amino resin itself is a multi-functional structure. The cross-linking density of the coating after room temperature curing is large. The coating is hard and brittle, and the flexibility is poor. The cured coating is prone to cracking after being placed for a short time. In order to solve the above technical problems, CN114250023A discloses a fire retardant coating and a preparation method. The mass fractions of the components taken are: 60% to 70% of water-based amino resin, 20% to 30% of expansion flame retardant and 5% to 10% of self-repairing microcapsules; a film-forming aid corresponding to the capsule core of the self-repairing microcapsule is also added; the water-based amino resin is selected from one or more combinations of urea-formaldehyde resin, melamine formaldehyde resin, and melamine urea-formaldehyde resin; the expansion flame retardant is a mixed or reactive expansion flame retardant; the wall material of the self-repairing microcapsule is melamine urea-formaldehyde resin or urea-formaldehyde resin, and the capsule core is a water-based room temperature self-crosslinking resin. However, the preparation process of this coating is relatively complicated and has poor waterproofness.
[0005] Prior art CN114213912A discloses a multifunctional water-based paint and a preparation method thereof. Wherein, taking the total mass of the multifunctional water-based paint as 100%, the multifunctional water-based paint includes the following raw material components: 10-30% of vinyl acetate-ethylene copolymer emulsion, 10-30% of elastic emulsion, 2-5% of anti-rust pigment, 1-2% of anti-flash rust agent, 0.3-1% of mildew and preservative, 0.5-1.5% of silane coupling agent, 30-40% of flame retardant pigment and filler, 1-10% of auxiliary additive, and the balance of water. The multifunctional water-based paint provided in this application enables the water-based paint to have fireproofing, waterproofing and anti-corrosion properties at the same time. The applicant used the patent formula and found that in order to overcome the problem of weak waterproofness of the vinyl acetate-ethylene copolymer film-forming material, a large amount of elastic emulsion was added to the formula. Although elastic emulsions can improve waterproof performance, their role in promoting foam formation and maintaining foam stability and integrity is much inferior to that of VAE emulsions and urea-formaldehyde resins, which means that the fire resistance of the coating is reduced. Therefore, the formula needs to add up to 30-40% of flame retardant pigments and fillers composed of pentaerythritol, melamine, ammonium polyphosphate and titanium dioxide to ensure fire resistance. This greatly increases the cost of the coating and is not suitable for the current highly competitive coating market.
[0006] And general urea-formaldehyde resin, especially melamine-modified urea-formaldehyde resin (MUF), is widely used in wood manufacturing industry, for bonding wood or being applied to wood-based material production as adhesive, for example, in the production of particleboard, plywood and various fiberboards.Urea-formaldehyde resin is the reaction product of urea and formaldehyde.Due to the poor water resistance and strength of this urea-formaldehyde resin, urea-formaldehyde resin modifier is generally used to modify the urea-formaldehyde resin obtained, to obtain modified urea-formaldehyde resin such as commonly used melamine-modified urea-formaldehyde resin (MUF), the water resistance and strength of this urea-formaldehyde resin are significantly higher than unmodified conventional urea-formaldehyde resin.Described urea-formaldehyde resin modifier is generally melamine, phenol or resorcinol, acrylate copolymer solution, isocyanate, polyvinyl alcohol, lignin etc. For example, CN102898604A discloses a method for preparing a modified urea-formaldehyde resin with improved storage stability, which comprises: (1) subjecting the first batch of urea, a modifier and formaldehyde to a first contact reaction until the water miscibility is 0.4 to 1.5 times, and the molar ratio of formaldehyde to the total amount of the first batch of urea and the modifier is 1 to 1.7:1; (2) subjecting the obtained mixture to a second contact reaction with the second batch of urea at a temperature of 60±15°C for 1 to 30 minutes, and the molar ratio of formaldehyde to the total amount of the first batch of urea, the second batch of urea and the modifier is 0.6 to 1.25:1; (3) adjusting the pH value of the mixture obtained in step (2) to 8.5 to 10 and cooling to below 40°C. The modifier is at least one of melamine, phenol, resorcinol, isocyanate, polyvinyl alcohol and lignin. The above-mentioned urea-formaldehyde resin is mainly for improving storage stability and reducing formaldehyde release. The water resistance of the modified urea-formaldehyde resin is improved, but it is still not comparable to the water resistance of acrylic resin and cannot meet the water resistance requirements of fire retardant coatings.
[0007] In short, after actual market research, it is found that the fireproof materials used in the fireproof material industry, such as fireproof coatings and fireproof boards, mainly use vinyl acetate-ethylene copolymers, polyacrylic acid polymers, etc. as film-forming materials, while urea-formaldehyde resin can be both a carbon source and a nitrogen source, and is both a carbon former and a foaming agent. It is generally used as an auxiliary resin. This is because even the modified phenolic resin is not as waterproof as the acrylic resin, and its fireproof performance is slightly inferior to the Wacker 3066 emulsion used in the mainstream high-end fireproof material market. It can only be used as an auxiliary film-forming material, and the amount added cannot be too high. Even if melamine and or isocyanate-modified urea-formaldehyde resin is used, although it can increase the stability and other properties of fireproof coatings, the waterproofness still cannot meet the requirements of the high-end fireproof market. Even if the elastic emulsion with better waterproofness is used for modification, the waterproofness has improved, but the improvement of physical blending modification is limited. In addition, if the amount of elastic emulsion is too much, it will inhibit the generation of foam, thereby affecting the fireproof performance. It can be seen that the current urea-formaldehyde resins on the market are difficult to balance fire resistance and water resistance. Although polyacrylate elastic emulsions have good water resistance, they are not fire resistant. VAE emulsions represented by Wacker 3066 emulsions have excellent fire resistance, but poor water resistance. Even if the two are blended, the water resistance and fire resistance are reduced. In other words, the current intumescent fire retardant coatings that use vinyl acetate-ethylene copolymers, polyacrylate polymers and urea-formaldehyde resins as film-forming materials are difficult to have excellent fire resistance and water resistance at the same time. Summary of the invention
[0008] The purpose of the present application is to provide a modified urea-formaldehyde resin which is specially used for fireproof materials and has excellent fireproofing and waterproofing properties.
[0009] To achieve the above object, the present application provides a process for manufacturing urea-formaldehyde resin for fireproof materials, which is manufactured by alkali-acid-alkali process and comprises the following steps: (1) Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; (2) Adjust the pH to 5.0-5.5 with formic acid, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, and finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; (3) After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; (4) Adding the pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and reacting for 15-25 minutes; wherein the sum of the amounts of isocyanate acrylate and acrylate is 5-10 wt % based on the basic modified urea-formaldehyde resin.
[0010] (5) adding 5-10 wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture based on the basic modified urea-formaldehyde resin while stirring, the mass ratio of the two being (2-4):1; (6) Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.
[0011] In steps (1) to (3), the cumulative molar ratio of formaldehyde to (urea + melamine) is 1.05-1.15; In step (2), the reaction is continued at a temperature of 16 to 20 seconds (Tu-4 cup, 30°C test) and then the reactants are cooled to 65 to 75°C. The weight ratio of isocyanate acrylate to acrylate in step (4) is (3-5): 1 In step (4), the isocyanate acrylate may be ethyl isocyanate acrylate or ethyl isocyanate methacrylate; The ester solvent in step (4) includes one or more of ethyl acetate, octyl acetate, and n-butyl acetate.
[0012] In step (4), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (5), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (6), the initiator is one or more of sodium persulfate, azobisisobutyronitrile, dibenzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide; In summary, this application has the following beneficial effects: (1) While using isocyanate to modify urea-formaldehyde resin, polyacrylate was used as a functional linker to achieve chemical grafting and coating modification of urea-formaldehyde resin, thereby improving the waterproof performance.
[0013] (2) Among many types of acrylic ester monomers, tri(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) was finally selected after a large number of experiments. While achieving the waterproofing effect of acrylic polymer coating, it also has the effect of foaming into carbon. It is speculated that this may be due to its nitrogen-containing characteristics, which avoids the acrylic resin with too low nitrogen content outside the urea-formaldehyde resin from inhibiting foaming into carbon.
[0014] (3) In step (4), the mixture is prepared by using a mixture of isocyanate acrylate, acrylate and ester solvents. On the one hand, the slow side reaction of isocyanate acrylate with water is reduced. On the other hand, by dispersing the isocyanate acrylate in the acrylate and ester solvents, local high cross-linking between the isocyanate acrylate and the urea-formaldehyde resin is avoided, which is conducive to the uniform coating of the isocyanate acrylate. Finally, the acrylate added together as a dispersion medium also increases the reaction response speed of the subsequent free radical copolymerization of the acrylate and the acrylic functional group in the isocyanate.
[0015] (4) The outer coating uses a mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylates to avoid the high cross-linking of THEICTA due to its three functional groups, which will increase the decomposition temperature and thus mismatch the decomposition and dehydration temperature of the intumescent flame retardant in the fireproof material, and even inhibit the early dehydration and foaming. Some acrylates can significantly reduce the cross-linking density, and while improving the bonding performance of the film-forming material, the effect of improving the foaming performance can be maintained.
[0016] (5) The amount of isocyanate acrylate should be appropriate. If it is too little, the coating effect is poor, and the effect of improving the waterproof effect and fire resistance is insufficient. If it is too much, isocyanate will consume a large amount of amino groups and even hydroxyl groups inside the urea-formaldehyde resin, and the hydroxyl content determines the dehydration and foaming rate of the urea-formaldehyde resin. Therefore, the amount of isocyanate acrylate should be appropriate. Example
[0017] Example 1 Preparation of modified urea-formaldehyde resin A The modified urea-formaldehyde resin is produced by an alkali-acid-alkali process, which includes the following steps: (1) Add a certain mass of 4.05 kg (48.6 moles) of formaldehyde solution (36%) into the reactor, add a certain amount of deionized water, then adjust the pH to 8.0 with 30% sodium hydroxide aqueous solution, and heat to 50°C. Then, add the first batch of urea 0.8 kg and the first batch of melamine 0.315 kg under stirring conditions, raise the temperature to 95°C and keep the temperature for 30 minutes; (2) Adjust the pH to 5.0 with 10 wt% formic acid, raise the temperature to 95°C, and continue to keep the temperature to react until the system viscosity reaches 18s (apply 4 cups, test at 30°C). Finally, cool the reactants to 70°C, adjust the pH to 7.0 with sodium hydroxide aqueous solution, add 1.0 kg of the second batch of urea and 0.315 kg of the second batch of melamine, stir evenly, and keep the temperature to react for 30 minutes; (3) After cooling to a certain temperature, add 0.6 kg of the third batch of urea, keep the temperature at 70°C for 20 minutes, cool to 40°C, and then adjust the pH value to 8.0 to obtain a basic modified urea-formaldehyde resin; (4) Add 0.354 kg of a mixture of ethyl isocyanate acrylate and ethyl acrylate (5 wt % based on urea-formaldehyde resin) and 0.708 kg of ethyl acetate while stirring. The mass ratio of ethyl isocyanate acrylate to ethyl acrylate is 4:1.
[0018] (5) Add tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate (0.354 kg) in a mass ratio of 2:1. (6) Add initiator solution, raise the temperature to 70°C, and react for 2 hours to obtain modified urea-formaldehyde resin.
[0019] Example 2 Preparation of modified urea-formaldehyde resin B On the basis of Example 1, in step (5), the mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate in a mass ratio of 2:1 was completely replaced by ethyl acrylate, and the other preparation steps were the same to obtain a modified urea-formaldehyde resin B.
[0020] Example 3 Preparation of modified urea-formaldehyde resin C On the basis of Example 1, in step (5), the mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate in a mass ratio of 2:1 was completely replaced by THEICTA, and the other preparation steps were the same to obtain a modified urea-formaldehyde resin C.
[0021] Example 4 Preparation of modified urea-formaldehyde resin D On the basis of Example 1, in step (4), 0.354 kg of the mixture of isocyanate ethyl acrylate and ethyl acrylate and ethyl acetate were all replaced with 0.354 kg of isocyanate ethyl acrylate, and the other preparation steps were the same to obtain modified urea-formaldehyde resin D.
[0022] Example 5 Preparation of modified urea-formaldehyde resin E On the basis of Example 1, steps (4) to (6) were omitted. At the same time, 3.54 kg of acrylic resin elastic emulsion (solid content of 20%) was added to the basic modified urea-formaldehyde resin and stirred at high speed for 20 minutes to obtain modified urea-formaldehyde resin E. Example 6 Preparation of modified urea-formaldehyde resin F On the basis of Example 1, steps (4) to (6) are omitted to directly obtain the basic modified urea-formaldehyde resin F.
[0023] Example 7 Preparation of fire retardant coating According to weight percentage, 6% of expandable vermiculite, 12% of coating additives and fillers, 24% of intumescent flame retardant, 20% of vinyl acetate-ethylene copolymer (VAE) emulsion, 20% of modified urea-formaldehyde resin and 18% of tap water are stirred in a high-speed disperser at 1000 rpm to obtain a fire retardant coating, and fire retardant coatings A, B, C, D, E, F prepared by using Examples 1-6 are obtained. Among them, the VAE emulsion is EZ 3066, the defoamer is 0.4%, the leveling agent is 0.3%, the thickener is 0.3%, the dispersant is 0.5%, the preservative is 0.5%, and the titanium dioxide is 10%. The intumescent flame retardant includes 6% pentaerythritol, 12% ammonium polyphosphate, and 6% melamine.
[0024] Fire resistance test The water-based fire retardant coating for steel structure prepared in Example 7 was sprayed on the steel plate so that the thickness of the coating was 3±0.1 mm; after 12 hours of surface drying, the fire resistance limit of the coating was tested with reference to the test method for thermal insulation efficiency deviation described in GB14907-2018, and the fire resistance limit of the water-based fire retardant coating for steel structure prepared in Example 7 was tested, and the test results are shown in Table 1. The coating of this embodiment was tested according to the standard GB 14907-2018 "Fire Retardant Coating for Steel Structure", and the results are shown in Table 1.
[0025] Water resistance test According to GB14907-2018 standard, the edge of the specimen is sealed with a molten mixture of paraffin and rosin (mass ratio is 1:1), and the edge width shall not be less than 5mm. After the mixture is completely solidified, it shall continue to be cured for 24 hours; during the test, all the specimens shall be immersed in a container filled with tap water. During the experiment, the appearance of the fire retardant coating on the surface of the specimen should be observed and recorded until the specified test time (24h) is reached. At the same time, in order to compare the differences in water resistance of different coatings, the time when the coating appears to be delaminated, foamed, and detached is recorded.
[0026] Table 1 Fire resistance and water resistance test of fire retardant coating coating Refractory time / min Water resistance (》24h water immersion test with no peeling, bubbling or shedding of the coating) Evaluation of strength, uniformity and adhesion of carbon foam layer Fire retardant coating A 152 Qualified (28 hours) High strength and uniformity Fire retardant coating B 122 Qualified (28 hours) High strength and uniformity Fire retardant coating C 131 Qualified (28 hours) High strength and uniformity Fire retardant coating D 135 Qualified (27h) High strength and uniformity Fire retardant coating E 102 24h coating starts to fall off (12 hours) Average strength, uneven, easy to fall off Fire retardant coating F 121 24h coating peeling off (8 hours) Average strength, uneven, easy to fall off It can be seen from Table 1 that the water-based ultra-thin intumescent steel structure fire retardant coating of the present invention has good fire resistance and water resistance.
Claims
1. A process for producing urea-formaldehyde resin for fireproof materials, using an alkali-acid-alkali process, characterized in that: The steps include: (1) Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; (2) Adjust the pH to 5.0-5.5 with formic acid, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, and finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; (3) After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; (4) adding a pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and reacting for 15-25 minutes; wherein the sum of the amounts of isocyanate acrylate and acrylate is 5-10wt% based on the basic modified urea-formaldehyde resin; (5) adding 5-10 wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture based on the basic modified urea-formaldehyde resin while stirring, the mass ratio of the two being (2-4):1; (6) Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.
2. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: In steps (1) to (3), the cumulative molar ratio of formaldehyde / (urea+melamine) is 1.05-1.
15.
3. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: In step (2), the reaction was continued at a temperature of 16 to 20 seconds until the viscosity of the system reached 16 to 20 seconds, and then the reactants were cooled to 65 to 75°C. The test conditions were 30°C and the coating-4 cup test was used.
4. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: In step (4), the weight ratio of isocyanate acrylate to acrylate is (3-5):
1.
5. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: The isocyanate acrylate is isocyanate ethyl acrylate or isocyanate ethyl methacrylate.
6. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: The ester solvent in step (4) includes one or more of ethyl acetate, octyl acetate, and n-butyl acetate.
7. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: The acrylic acid ester in step (4) can be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate.
8. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: The acrylate in step (5) can be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate.
9. The process for producing urea-formaldehyde resin for fireproof materials according to claim 1, characterized in that: In step (6), the initiator is one or more of sodium persulfate, azobisisobutyronitrile, dibenzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide.
10. A fire-resistant urea-formaldehyde resin prepared according to the manufacturing process of urea-formaldehyde resin for fire-proof materials according to claims 1-9.
Citation Information
Patent Citations
Preparation method of modified urea-formaldehyde resin with improved storage stability
CN102898604A
Multifunctional water-based paint and preparation method thereof
CN114213912A
Room-temperature self-repairing water-based transparent expansion fireproof coating and preparation method thereof