Fluorine-containing oil-proof agent and preparation method thereof
By using the mixed preparation of composite crosslinked monomers and fluorine-containing monomers, the problem of insufficient adhesion of fluorine-containing oil-resistant agents in the prior art is solved, and a stronger oil-resistant effect and simplified process are achieved, which is suitable for paper products. Waterproof and oil-proof applications.
Patent Information
- Application Number
- CN202411227466.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The existing fluorine-containing oil-resistant agents have insufficient adhesion on paper products, and the preparation process is complicated, making it difficult to achieve excellent waterproof and oil-proof performance.
Using composite crosslinked monomers, including allyl methacrylate phosphate, itaconic acid epoxy acrylic resin and melamine acrylate, is prepared by mixing with fluorine-containing monomers to form stronger coating crosslink density and density. Improve oil resistance.
It significantly improves oil resistance and coating adhesion, simplifies the preparation process, and shows excellent waterproof and oil resistance on paper products.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorine-containing oil-proofing agents, and in particular to a fluorine-containing oil-proofing agent and a preparation method thereof. Background Art
[0002] In recent years, environmental protection issues have become increasingly severe. Relevant departments attach great importance to environmental protection issues and have been committed to reducing the use of plastics. More and more products are required to reduce pollution or even no pollution. This has prompted non-degradable plastic products to be replaced by paper products. The amount and application range of paper products are constantly increasing. They are widely used in catering, food and other packaging fields. In these fields, paper products are usually required to have waterproof and oil-proof properties.
[0003] At present, fluorinated oil repellents mainly reduce the free energy of the material surface through their special chemical structure (such as the short bond length and high bond energy of the CF bond), thereby showing excellent waterproof, oil-proof and anti-fouling properties. This auxiliary agent is widely used in the fields of textiles, leather, coatings, etc., and can effectively improve the practicality and durability of the products, but the fluorinated oil repellent itself is mainly used to improve the waterproof, oil-proof and anti-fouling properties of the material. Since the fluorinated oil repellent itself has weak adhesion when coated on paper and other products, the current technology will first prepare a synergist during the preparation of the fluorinated oil repellent, and the synergist is combined with the fluorinated oil repellent, which increases the preparation steps and the process is still relatively complicated. Summary of the invention
[0004] The present invention aims at the deficiencies in the prior art and provides a fluorine-containing oil-proofing agent and a preparation method thereof. The fluorine-containing monomer is mixed with a composite cross-linking monomer for preparation. The composite cross-linking monomer adopts a composite cross-linking monomer of allyl methacrylate phosphate, itaconic acid epoxy acrylic resin and acrylic melamine to achieve a better oil-proofing effect.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A fluorine-containing oil-proofing agent comprises the following raw materials in parts by weight:
[0007] Fluorine-containing monomer: 60-70 parts by weight;
[0008] Acrylate monomer: 10-15 parts by weight;
[0009] Composite cross-linking monomer: 3-6 parts by weight, including 20-40% allyl methacrylate phosphate, 30-50% itaconic acid epoxy acrylic resin, and 20-40% acrylic melamine;
[0010] Solvent: 100-150 parts by weight;
[0011] Initiator: 0.3-0.5 parts by weight;
[0012] Molecular weight regulator: 0.01-0.03 parts by weight;
[0013] Neutralizer: content 1-3% (based on the weight of the emulsion);
[0014] Antifreeze: 3-5 parts by weight.
[0015] Preferably, the fluorine-containing monomer is one of CH2=CH-C(=O)-O-CH2CH2-C_6F13 or CH2=C(CH3)-C(=O)-O-CH2CH2-C6F13.
[0016] Preferably, the solvent is at least one of acetone, butanone, ethanol or isopropanol; the initiator is azobisisobutyronitrile; the molecular weight regulator is 3-mercaptopropionate; the neutralizer is phosphoric acid solution; and the antifreeze agent is methanol, ethylene glycol or propylene glycol.
[0017] Preferably, it further comprises 5-10 parts by weight of an antibacterial monomer, which is pre-treated by coating to improve its durability and stability.
[0018] Preferably, the coating pretreatment step comprises mixing the antibacterial monomer with the coating material monomer to form antibacterial agent microcapsules or nanoparticles through a prepolymerization reaction.
[0019] Preferably, the antibacterial monomer is a quaternary ammonium salt monomer, and the coating material monomer is polymethyl methacrylate or polyurethane.
[0020] Preferably, the coating material is modified by copolymerization of precursor monomers of polymethyl methacrylate or polyurethane with monomers containing fluorinated groups, thereby introducing fluorinated groups into the polymer chain to improve compatibility with fluorinated monomers.
[0021] Preferably, the invention further comprises a hydrophilic monomer: 5-15 parts by weight; the hydrophilic monomer is at least one of 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, hydroxyethyl methacrylate, vinyl pyrrolidone or pentaerythritol mono(meth)acrylate.
[0022] Preferably, the invention further comprises a retention aid: 4-6 parts by weight, wherein the retention aid is at least one of polyacrylamide, acrylamide or methyl methacrylate.
[0023] Preferably, the content of deionized water is 300 parts by weight.
[0024] A method for preparing a fluorine-containing oil-proofing agent comprises the following steps:
[0025] Pre-reaction: Mix the solvent, fluorinated monomer, acrylate monomer, hydrophilic monomer, initiator and part of deionized water at 70-75°C and stir for at least 1.5 hours;
[0026] Accelerating the reaction: heating the mixture to 80-85°C, adding the composite cross-linking monomer, molecular weight regulator and the remaining deionized water under accelerated stirring, continuing the reaction for 8-10 hours, and then heating to 90°C to evaporate the solvent to obtain an emulsion;
[0027] Neutralization: Add 1-3% neutralizer to the emulsion, mix well, and convert the emulsion into a solution;
[0028] Mixing aids: Add antifreeze agent and retention aid into the solution and mix well. Stir at a rate of 60-600r / min for at least 30 minutes during the mixing process.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present application provides a fluorine-containing oil-proofing agent and a preparation method thereof. In the preparation of the fluorine-containing oil-proofing agent, a composite cross-linking monomer is used. The composite cross-linking monomer includes allyl methacrylate phosphate, itaconic acid epoxy acrylic resin and acrylic melamine. To achieve a better oil-proofing effect, a composite cross-linking monomer is obtained by using allyl methacrylate phosphate, itaconic acid epoxy acrylic resin and acrylic melamine. The three cross-linking monomers have their own characteristics in structure. Through common cross-linking, complementary advantages can be formed at the molecular level. A complex network structure is formed during the polymerization process through a variety of cross-linking monomers. This network structure not only enhances the cross-linking density and hardness of the coating, but also improves the compactness and anti-permeability of the coating, thereby effectively preventing the invasion of oil stains and significantly improving the oil-proofing effect. The fluorine-containing oil-proofing agent has a good oil release effect, strong coating adhesion, is practical and convenient, and has a simpler preparation process.
[0031] In the present application, PMMA or PU monomers are copolymerized with fluorinated monomers to introduce fluorinated groups into the polymer chain. The fluorinated groups interact with other parts in the polymer chain and may form stronger intermolecular forces, such as hydrogen bonds or van der Waals forces, thereby enhancing the interaction between the polymer and the fluorinated monomer. DETAILED DESCRIPTION
[0032] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be used for other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0033] Those skilled in the art should understand that, in the disclosure of the present invention, the terms "longitudinal," "lateral," "up," "down," "left," "right," "front," "back," "vertical," "horizontal," "top," "bottom," "inside," "outside," etc., which indicate directions or positional relationships, are only for the convenience of describing the present invention in a simplified manner, and do not indicate or imply that the device or component referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the above terms should not be understood as limiting the present invention.
[0034] It is to be understood that the term "one" should be understood as "at least one" or "one or more," that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.
[0035] Embodiment 1:
[0036] This embodiment provides a fluorine-containing oil-proofing agent, comprising the following raw materials in parts by weight:
[0037] The fluorine-containing monomer is CH2=CH-C(=O)-O-CH2CH2-C_6F13: 60 parts by weight;
[0038] The acrylate monomer is methyl methacrylate: 10 parts by weight;
[0039] The composite cross-linking monomer includes 20% allyl methacrylate phosphate, 30% itaconic acid epoxy acrylic resin, and 20% acrylic melamine: 3 parts by weight;
[0040] The solvent is acetone: 100 parts by weight;
[0041] The initiator is azobisisobutyronitrile: 0.3 parts by weight;
[0042] Molecular weight regulator 3-mercaptopropionate: 0.01 parts by weight;
[0043] The neutralizing agent is phosphoric acid solution: content 1% (based on the weight of the emulsion);
[0044] The antifreeze agent is methanol: 3 parts by weight.
[0045] The hydrophilic monomer is 2-hydroxyethyl methacrylate: 5 parts by weight;
[0046] The retention aid is polyacrylamide: 4 parts by weight.
[0047] Deionized water: 300 parts by weight.
[0048] The preparation method of the fluorine-containing oil-proofing agent comprises:
[0049] 1) Pre-reaction: at 70° C., acetone, CH2=CH-C(=O)-O-CH2CH2-C_6F13, methyl methacrylate, hydrophilic monomer, azobisisobutyronitrile and 200 parts by weight of deionized water were mixed and stirred for 1.5 hours;
[0050] 2) Accelerating the reaction: heating the mixture to 80° C., adding allyl methacrylate phosphate, itaconic acid epoxy acrylic resin, a crosslinking monomer mixed in a predetermined ratio of acrylic melamine, 3-mercaptopropionic acid ester and the balance of deionized water under accelerated stirring, continuing the reaction for 8 hours, and then heating to 90° C. to evaporate the solvent to obtain an emulsion;
[0051] 3) Neutralization: Add 1% phosphoric acid solution to the emulsion, mix well, and convert the emulsion into a solution;
[0052] 4) Mixing aid: Add methanol and polyacrylamide into the solution and mix well. Stir at a rate of 600 r / min for 30 minutes during the mixing process.
[0053] Example 2
[0054] The present embodiment provides a fluorine oil-proofing agent, the raw materials, weight proportions thereof and the preparation method thereof are substantially the same as those in the embodiment 1, the only difference being that in the preparation in step 1) of the present embodiment, CH2=C(CH3)-C(=O)-O-CH2CH2-C6F13 is used as a fluorine-containing monomer.
[0055] Embodiment 3:
[0056] This embodiment provides a fluorine-containing oil-proofing agent, comprising the following raw materials in parts by weight:
[0057] The fluorine-containing monomer is CH2=CH-C(=O)-O-CH2CH2-C_6F13: 60 parts by weight;
[0058] The acrylate monomer is methyl methacrylate: 10 parts by weight;
[0059] The composite cross-linking monomer includes 20% allyl methacrylate phosphate, 30% itaconic acid epoxy acrylic resin, and 20% acrylic melamine: 3 parts by weight;
[0060] The solvent is acetone: 100 parts by weight;
[0061] The initiator is azobisisobutyronitrile: 0.3 parts by weight;
[0062] Molecular weight regulator 3-mercaptopropionate: 0.01 parts by weight;
[0063] The neutralizing agent is phosphoric acid solution: content 1% (based on the weight of the emulsion);
[0064] The antifreeze agent is methanol: 3 parts by weight.
[0065] The hydrophilic monomer is 2-hydroxyethyl methacrylate: 5 parts by weight;
[0066] The retention aid is polyacrylamide: 4 parts by weight.
[0067] Deionized water: 300 parts by weight;
[0068] The antibacterial monomer is a quaternary ammonium salt monomer: 5 parts by weight;
[0069] The coating material monomer is PMMA: 15 parts by weight.
[0070] The preparation method of the fluorine-containing oil-proofing agent comprises:
[0071] 1) Pretreatment of antibacterial monomers: quaternary ammonium salt monomers are mixed with a small amount of PMMA to form antibacterial agent microcapsules or nanoparticles through prepolymerization, and the antibacterial monomers are wrapped inside the coating material to form a stable coating structure;
[0072] Solvent, fluorinated monomer, acrylate monomer, hydrophilic monomer, initiator, pre-treated antimicrobial agent microcapsules (or nanoparticles) and part of deionized water are mixed.
[0073] 2) Pre-reaction: at 70° C., acetone, CH2=CH-C(=O)-O-CH2CH2-C_6F13, methyl methacrylate, azobisisobutyronitrile, pretreated antibacterial agent microcapsules (or nanoparticles) and 200 parts by weight of deionized water were mixed and stirred for 1.5 hours;
[0074] 3) Accelerating the reaction: heating the mixture to 80° C., adding allyl methacrylate phosphate, itaconic acid epoxy acrylic resin, a crosslinking monomer mixed in a predetermined ratio of acrylic melamine, 3-mercaptopropionic acid ester and the balance of deionized water under accelerated stirring, continuing the reaction for 8 hours, and then heating to 90° C. to evaporate the solvent to obtain an emulsion;
[0075] 4) Evaporation of solvent and neutralization: heating to 90°C to evaporate the solvent to obtain an emulsion; then adding 1% phosphoric acid solution as a neutralizing agent to the emulsion, mixing well, and converting the emulsion into a solution;
[0076] 5) Mixing aid: Add methanol, polyacrylamide, etc. to the solution and mix well. Stir at a speed of 600 r / min for 30 minutes during the mixing process.
[0077] Embodiment 4:
[0078] This embodiment provides a fluorine-containing oil-proofing agent, comprising the following raw materials in parts by weight:
[0079] The fluorine-containing monomer is CH2=CH-C(=O)-O-CH2CH2-C_6F13: 70 parts by weight;
[0080] The acrylate monomer is methyl methacrylate: 15 parts by weight;
[0081] The composite cross-linking monomer includes 20% allyl methacrylate phosphate, 30% itaconic acid epoxy acrylic resin, and 20% acrylic melamine: 5 parts by weight;
[0082] The solvent is acetone: 150 parts by weight;
[0083] The initiator is azobisisobutyronitrile: 0.5 parts by weight;
[0084] Molecular weight regulator 3-mercaptopropionate: 0.03 parts by weight;
[0085] The neutralizing agent is phosphoric acid solution: content 3% (based on the weight of the emulsion);
[0086] The antifreeze agent is methanol: 5 parts by weight.
[0087] The hydrophilic monomer is 2-hydroxyethyl methacrylate: 15 parts by weight;
[0088] The retention aid is polyacrylamide: 6 parts by weight.
[0089] Deionized water: 300 parts by weight;
[0090] The antibacterial monomer is a quaternary ammonium salt monomer: 10 parts by weight;
[0091] The coating material monomer is PMMA: 25 parts by weight.
[0092] The preparation method of the fluorine-containing oil-proofing agent comprises:
[0093] 1) Pretreatment of antibacterial monomers: quaternary ammonium salt monomers are mixed with a small amount of PMMA to form antibacterial agent microcapsules or nanoparticles through prepolymerization, and the antibacterial monomers are wrapped inside the coating material to form a stable coating structure;
[0094] Solvent, fluorinated monomer, acrylate monomer, hydrophilic monomer, initiator, pre-treated antimicrobial agent microcapsules (or nanoparticles) and part of deionized water are mixed.
[0095] 2) Pre-reaction: at 75° C., acetone, CH2=CH-C(=O)-O-CH2CH2-C_6F13, methyl methacrylate, azobisisobutyronitrile, pretreated antibacterial agent microcapsules (or nanoparticles) and 200 parts by weight of deionized water were mixed and stirred for 1.5 hours;
[0096] 3) Accelerating the reaction: heating the mixture to 85° C., adding allyl methacrylate phosphate, itaconic acid epoxy acrylic resin, a crosslinking monomer mixed in a predetermined ratio of acrylic melamine, 3-mercaptopropionic acid ester and the balance of deionized water under accelerated stirring, continuing the reaction for 10 hours, and then heating to 90° C. to evaporate the solvent to obtain an emulsion;
[0097] 4) Neutralization: Add 3% phosphoric acid solution as a neutralizing agent to the emulsion, mix well, and convert the emulsion into a solution;
[0098] 5) Mixing aid: Add methanol, polyacrylamide, etc. to the solution and mix well. Stir at a speed of 600 r / min for 30 minutes during the mixing process.
[0099] Example 5
[0100] The present embodiment provides a fluorine oil-proofing agent, the raw materials, weight proportions thereof and the preparation method thereof are substantially the same as those of the embodiment 3, the only difference being that in the preparation in step 2) of the present embodiment, CH2=C(CH3)-C(=O)-O-CH2CH2-C6F13 is used as a fluorine-containing monomer.
[0101] Example 6
[0102] This embodiment provides a fluorine oil-proofing agent, whose raw materials, weight parts and preparation method are basically the same as those in Example 3, and the only difference is that in step 1) of this embodiment, PU monomer is used as the coating material monomer.
[0103] Example 7
[0104] The present embodiment provides a fluorine oil-proofing agent, the raw materials, weight proportions thereof and the preparation method thereof are substantially the same as those of the embodiment 4, the only difference being that in the preparation in step 2) of the present embodiment, CH2=C(CH3)-C(=O)-O-CH2CH2-C6F13 is used as a fluorine-containing monomer.
[0105] Example 8
[0106] This embodiment provides a fluorine oil-proofing agent, whose raw materials, weight parts and preparation method are basically the same as those in Example 4, and the only difference is that in step 1) of this embodiment, PU monomer is used as the coating material monomer.
[0107] In the above embodiment, the solvent may also be at least one of butanone, ethanol or isopropanol.
[0108] In the above embodiment, the antifreeze agent may also be ethylene glycol or propylene glycol.
[0109] It should be noted that PMMA is polymethyl methacrylate and PU is polyurethane; the coating material is modified by copolymerization of precursor monomers of polymethyl methacrylate or polyurethane (such as methyl methacrylate (MMA) for PMMA, or isocyanate and polyol for PU) with monomers containing fluorinated groups to improve compatibility with perfluorooctyl ethyl methacrylate to form a more stable coating layer.
[0110] It should be noted that the composite cross-linking monomer of allyl methacrylate phosphate, itaconic acid epoxy acrylic resin and acrylic melamine has a significant contribution to the improvement of oil-proof effect:
[0111] 1. Enhance surface tension:
[0112] Fluorinated monomers themselves have extremely low surface energy, which can effectively reduce the surface tension of the coating, making the coating have excellent oil-repellent properties.
[0113] The phosphate groups in allyl methacrylate phosphate may enhance the interaction with the fluorinated monomer, further improving the surface tension regulating ability of the coating, making the coating surface smoother and less likely to be wetted by oil stains.
[0114] 2. Enhance coating cross-linking density:
[0115] The use of three cross-linking monomers together can form a more complex cross-linking structure in the polymer network and increase the cross-linking density of the coating. This helps to form a denser and stronger coating to prevent oil penetration.
[0116] Itaconic acid epoxy acrylate resin has excellent cross-linking ability and weather resistance, which can increase the hardness and wear resistance of the coating, while acrylic melamine has excellent heat resistance and chemical resistance due to its triazine ring structure. The two work together with allyl methacrylate phosphate to make the coating more resistant to oil stains.
[0117] 3. Improve coating stability:
[0118] The synergistic effect of multiple cross-linking monomers can improve the chemical stability and thermal stability of the coating, prevent the coating performance from degrading under high temperature or harsh environment, and thus maintain a lasting oil-proof effect.
[0119] Synergistic Mechanism
[0120] Complementarity: The three cross-linking monomers have their own structural characteristics, and through common cross-linking, they can form complementary advantages at the molecular level. For example, itaconic acid epoxy acrylate resin and acrylic melamine have excellent physical and chemical properties respectively, while allyl methacrylate phosphate may enhance the interaction with fluorinated monomers. The three work together to comprehensively improve the coating performance.
[0121] Network structure: A variety of cross-linked monomers form a complex network structure during the polymerization process. This network structure not only enhances the cross-linking density and hardness of the coating, but also improves the density and anti-permeability of the coating, thereby effectively preventing the invasion of oil stains.
[0122] Synergistic effect: During the formation of the coating, the three cross-linking monomers may promote each other's polymerization reaction, improve the polymerization efficiency and conversion rate, and thus improve the overall performance of the coating.
[0123] In addition, it has the following effects:
[0124] 1. Improve cross-linking density:
[0125] These three cross-linking monomers can form a complex cross-linking network during the polymerization process, significantly increasing the cross-linking density of the polymer. High cross-linking density helps to enhance the physical properties of the polymer, such as hardness, wear resistance and solvent resistance.
[0126] 2. Improve weather resistance:
[0127] Both itaconic acid epoxy acrylate and acrylic melamine have good weather resistance and are able to resist UV radiation and oxidative degradation, thereby extending the service life of the product.
[0128] 3. Enhance adhesion:
[0129] The phosphate group in allyl methacrylate phosphate can form a chemical bond with the surface of the substrate, enhancing the adhesion between the coating and the substrate. This is especially important for the application of oil repellent on substrates such as fabrics and leather.
[0130] Synergistic Mechanism
[0131] Complementary effects:
[0132] The three crosslinking monomers have their own characteristics in chemical structure and properties, and they can complement each other. For example, the phosphate group of allyl methacrylate phosphate provides excellent adhesion, while itaconic acid epoxy acrylate resin and melamine acrylate contribute weather resistance and high crosslinking density.
[0133] Synergy Effect:
[0134] During the polymerization process, these cross-linking monomers participate in the cross-linking reaction together to form a more dense and stable cross-linking network. This synergistic effect makes the performance of the final product better than that of a single cross-linking monomer.
[0135] Experimental Example 1:
[0136] The stability test of the fluorinated oil-proofing agent for paper was conducted by testing the stability of the fluorinated oil-proofing agent for each paper in Examples 1-8 according to the following method:
[0137] A. Test of stability at room temperature: centrifuge the fluorinated oil-proofing agent for paper in a centrifuge at 1500r / min for 15min, let it stand for 15min, filter it with a 400-mesh filter cloth, and calculate the proportion of insoluble matter in the oil-proofing agent;
[0138] B Freeze-thaw stability test: Take 50g of paper and store it with fluorinated oil-proof agent at -15℃ for 2h, then put it in a 35℃ water bath to thaw it completely, filter it with a 400-mesh filter cloth, and calculate the proportion of insoluble matter in the oil-proof agent.
[0139] The test results are shown in Table 1
[0140] Table 1. Test results of stability of fluorinated oil-proofing agent for paper
[0141] Example Room temperature stability / % Freeze-thaw stability / % 1 0 0 2 0 0 3 0 0 4 0 0 5 0 0 6 0 0 7 0 0 8 0 0
[0142] As can be seen from Table 1, the fluorinated oil-proofing agents for paper obtained in Examples 1-8 of the present application have excellent room temperature stability and freeze-thaw stability, and the oil-proofing agent dispersion has high stability, which is conducive to its application in the field of paper products.
[0143] Experimental Example 2:
[0144] Oil-proof paper is obtained by using the pulp addition method, the specific methods include:
[0145] 1) diluting the PAE papermaking wet strength agent purchased from Xinquan Papermaking Auxiliary Agent Factory, Taishan District, Tai'an City to 1% to obtain a wet strength agent solution;
[0146] 2) preparing a starch dispersion having a solid content of 1% by using cationic starch purchased from Jinan Xinhong Chemical Co., Ltd.;
[0147] 3) Beat the bleached softwood pulp, cut it into appropriate sections after sufficient debonding, beat it to 85°SR at a pulp concentration of 25%, and adjust the pulp concentration to 10%;
[0148] 4) 50g of the above slurry, 3.2g of starch dispersion, 1.4g of wet strength agent solution and 2.0g of the fluorine-containing oil-proofing agent obtained in Example 1-8 were added to 100g of deionized water and mixed to obtain a raw slurry with a dry pulp content of 3.2%;
[0149] 5) Step 4) The slurry is placed in a sheet making machine and vacuum dehydrated to 3.5 g / m 2 The wet paper was pressed between filter paper sheets under pressure and then aged at 110°C for 90 seconds to obtain a 70 g / m 2 Greaseproof paper.
[0150] The water-proof and oil-proof properties of the oil-proof papers containing the fluorinated oil-proof agents obtained in Examples 1-8 were measured respectively:
[0151] The waterproof performance is determined by the Cobb test method, that is, the water resistance of a 100 cm 2 The weight of water absorbed by a paper product with a surface area that supports 1 cm of water, converted to g / m 2 ;
[0152] The oil resistance performance was measured according to the international general test method OilKitTest-TAPPI557. The statistical results are shown in Table 2.
[0153] Table 2. Waterproof and oilproof properties of oil-proof paper
[0154] Example <![CDATA[Waterproof performance (g / m 2 )]]> Oil resistance 1 8.1 11 2 7.6 11 3 7.6 12 4 7.2 12 5 7.9 12 6 7.5 11 7 7.2 11 8 8.3 11
[0155] As can be seen from the above table, the preferred embodiments of the present application all have a waterproof performance not higher than 8.5 g / m2 and an oil-proof performance not lower than level 11, and have excellent waterproof and oil-proof effects. The present application has a positive significance in improving waterproof and oil-proof properties.
[0156] Those skilled in the art should understand that the embodiments of the present invention shown in the above description are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functions and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.
Claims
1. A fluorine-containing oil-proofing agent, characterized in that: Contains the following raw materials in parts by weight: Fluorine-containing monomer: 60-70 parts by weight; Acrylate monomer: 10-15 parts by weight; Composite cross-linking monomer: 3-6 parts by weight, including 20-40% allyl methacrylate phosphate, 30-50% itaconic acid epoxy acrylic resin, and 20-40% acrylic melamine; Solvent: 100-150 parts by weight; Initiator: 0.3-0.5 parts by weight; Molecular weight regulator: 0.01-0.03 parts by weight; Neutralizer: content 1-3% (based on the weight of emulsion); Antifreeze: 3-5 parts by weight.
2. A fluorine-containing oil-proofing agent according to claim 1, characterized in that: The fluorine-containing monomer is one of CH2=CH-C(=O)-O-CH2CH2-C_6F13 or CH2=C(CH3)-C(=O)-O-CH2CH2-C6F13.
3. A fluorine-containing oil-proofing agent according to claim 2, characterized in that: The solvent is at least one of acetone, butanone, ethanol or isopropanol; the initiator is azobisisobutyronitrile; the molecular weight regulator is 3-mercaptopropionate; the neutralizer is phosphoric acid solution; and the antifreeze agent is methanol, ethylene glycol or propylene glycol.
4. A fluorine-containing oil-proofing agent according to claim 3, characterized in that: It also contains 5-10 parts by weight of an antibacterial monomer, which is pre-treated by coating to improve its durability and stability.
5. A fluorine-containing oil-proofing agent according to claim 4, characterized in that: The coating pretreatment step includes mixing the antibacterial monomer with the coating material monomer to form antibacterial agent microcapsules or nanoparticles through a prepolymerization reaction.
6. A fluorine-containing oil-proofing agent according to claim 5, characterized in that: The antibacterial monomer is a quaternary ammonium salt monomer, and the coating material monomer is polymethyl methacrylate or polyurethane.
7. A fluorine-containing oil-proofing agent according to claim 6, characterized in that: The coating material is modified by copolymerization of precursor monomers of polymethyl methacrylate or polyurethane and monomers containing fluorinated groups, thereby introducing fluorinated groups into the polymer chain to improve compatibility with fluorinated monomers.
8. A method for preparing the fluorine-containing oil-proofing agent according to any one of claims 1 to 7, characterized in that: The following steps are involved: Pre-reaction: Mix the solvent, fluorinated monomer, acrylate monomer, hydrophilic monomer, initiator and part of deionized water at 70-75°C and stir for at least 1.5 hours; Accelerating the reaction: heating the mixture to 80-85°C, adding the composite cross-linking monomer, molecular weight regulator and the remaining deionized water under accelerated stirring, continuing the reaction for 8-10 hours, and then heating to 90°C to evaporate the solvent to obtain an emulsion; Neutralization: Add 1-3% neutralizer to the emulsion, mix well, and convert the emulsion into a solution; Mixing aids: Add antifreeze agent and retention aid into the solution and mix well. Stir at a rate of 60-600r / min for at least 30 minutes during the mixing process.
Citation Information
Cited By
Preparation method of oil-proofing agent based on polymerization of acrylic acid and organic silicon
CN119505245A
Preparation method for oil-proofing agent based on polymerization of acrylic acid and organosilicon
WO2026152556A1