Wide damping temperature range polyurethane material and preparation method thereof
The wide-dampening temperature-domain polyurethane material prepared by one-step mixing and curing is adjusted to form a cross-linking network structure by adjusting the ratio of isocyanate and polytriol, which solves the problem of the existing materials decreasing function when temperature changes, and achieves the wide-ranging The high damping performance and mechanical strength in the temperature domain meet the vibration and noise reduction requirements at various temperatures in the construction field.
Patent Information
- Application Number
- CN202411222318.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing polyurethane materials have reduced or brittle functions when temperature changes, and cannot effectively meet the vibration and noise reduction needs in various temperatures in the construction field.
A wide-dampening and temperature-defying polyurethane material was prepared by one-step mixed curing. By adjusting the ratio of isocyanate and polytriol, the R value was controlled between 3-5, forming a complete cross-linking network structure to ensure that the material was at a wide temperature. Maintain damping performance in the domain.
The high energy absorption and dissipation effect of polyurethane materials in high temperature to low temperature zones is achieved, the damping performance and mechanical strength of the materials are improved, and the needs of industrial mass production are met.
Smart Images

Figure CN118930791A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane material with a wide damping temperature range and a preparation method thereof, belonging to the technical field of polyurethane preparation. Background Art
[0002] Noise pollution is known as one of the four major public hazards of environmental protection. Vibration and noise permeate people's lives, seriously affecting people's physical and mental health, and threatening the safe operation of equipment and facilities. my country's noise pollution prevention and control regulations are also constantly improving, and higher requirements are put forward for vibration reduction and noise reduction. Damping materials can effectively improve the harm caused by vibration and noise due to their special structural characteristics. Among them, the molecular structure of polyurethane is mainly composed of hard segments and soft segments. The hard segment is usually formed by the reaction of isocyanate and polyol or chain extender, while the soft segment is mainly composed of polyether or polyester long chain. The polyurethane molecules are cross-linked through hydrogen bonds, van der Waals forces and other interactions between the hard segment and the soft segment to form a polymer with a network structure. At the same time, polyurethane molecules show a certain arrangement law at the microscopic level. The unique network structure, cross-linking method and microscopic arrangement make polyurethane have good mechanical and damping properties. At present, the vibration and noise reduction materials commonly used in the construction field are rubber vibration pads. The effective damping temperature range of such materials can only meet the needs of low or high temperature areas unilaterally, and the change of seasonal temperature can easily cause the function of the material to decrease or become brittle, which makes the material have certain limitations in solving the problem of vibration and noise reduction. Therefore, it is an urgent problem to prepare polyurethane materials with a wide damping temperature range to meet the requirements of vibration and noise reduction at various temperatures. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a polyurethane material with a wide damping temperature range and a preparation method thereof. A polyurethane material with a wide damping temperature range is designed and prepared. Compared with conventional formulas, the designed formula not only has damping performance in a variety of environments, but also can meet the needs of industrial mass production. This method can obtain a polyurethane damping material that meets the wide temperature range vibration reduction needs at a low cost.
[0004] To achieve the above objectives, the technical solution of the present invention is as follows.
[0005] A polyurethane material with a wide damping temperature range, the polyurethane material is obtained by mixing and curing in a one-step process;
[0006] Taking the total mass of raw materials required to prepare the polyurethane material as 100%, the raw material components and their mass fractions are as follows:
[0007] Isocyanate 80%~85%
[0008] Polytriol 15%~20%
[0009] Among them, the R value of the system is 3-5, and the R value is the molar ratio of isocyanate to hydroxyl;
[0010] Preferably, the isocyanate in the raw material is at least one of diphenylmethane diisocyanate (MDI), toluene diisocyanate (HDI), and isophorone diisocyanate (IPDI);
[0011] Preferably, the polytriol in the raw material is at least one of polycaprolactone triol and polyoxypropylene triol, and the molecular weight of the polytriol is 4500-5000.
[0012] A method for preparing a polyurethane material with a wide damping temperature range, comprising the steps of:
[0013] (1) In a three-necked flask, the polytriol in the raw material is subjected to vacuum dehydration treatment;
[0014] (2) under a protective gas atmosphere, adding the isocyanate in the raw material into the flask described in (1), and mixing and reacting with the polytriol at high temperature;
[0015] (3) curing the product obtained in (2) at high temperature to obtain the polyurethane material with a wide damping temperature range;
[0016] Preferably, in step (1), the temperature during the dehydration treatment is 110-120°C, the vacuum degree during the dehydration treatment is -0.1MPa, and the dehydration treatment time is 2-4h;
[0017] Preferably, in step (2), the protective gas is N 2 , the reaction temperature is 80-90°C, and the reaction time is 4-8h;
[0018] Preferably, in step (3), the curing temperature is 80-90° C. and the curing time is 36-48 h.
[0019] Beneficial Effects
[0020] The invention provides a wide damping temperature range polyurethane material, wherein the polyurethane is a new type of polyurethane damping material, which can meet the use requirements of wide temperature range damping materials, and the polyether triol used in the material has good processability and weather resistance. The long-chain polytriol forms a loose cross-linked network structure with isocyanate, which has a weak inhibitory effect on the movement of molecular chain segments, and the excess isocyanate reacts with water in the air to generate a series of molecular chains with different molecular weights, wherein the part with higher molecular weight serves as a material skeleton network to maintain the basic structure and mechanical properties of the material, and the part with relatively lower molecular weight acts as a plasticizer to increase the overall activity of the molecular chain, so that the material exhibits a higher energy absorption and dissipation effect in both high temperature and low temperature zones, thereby improving the damping performance of the material.
[0021] The present invention provides a polyurethane material with a wide damping temperature range. The polyurethane material is obtained by mixing and curing two raw materials, isocyanate and polytriol, in a certain ratio. The selection and dosage of the two can ensure that a complete and neat cross-linked network exists in the prepared polyurethane material, thereby further improving the mechanical strength and damping performance of the polyurethane material.
[0022] The present invention provides a polyurethane material with a wide damping temperature range. It is necessary to control the ratio of the polytriol component to the isocyanate component in the raw material. If the ratio is too high or too low, the damping temperature range of the material will be limited to the low temperature region. When the R value is between 3 and 5, the cross-linking degree of the material meets the application conditions of a wide temperature range, so that the effective damping of the material can achieve a wide temperature range coverage.
[0023] The invention provides a polyurethane material with a wide damping temperature range. In the preparation of the polyurethane material, both ends of isocyanate contain -NCO groups, and polytriol contains -OH groups. Finished products with different effects can be obtained by adjusting the ratio of the raw materials. The method is simple in steps, and the experimental formula can be changed according to production needs, so that industrial production can be carried out.
[0024] The invention provides a polyurethane material with a wide damping temperature range. In the preparation of the polyurethane material, the R value needs to be controlled. If the R value content is too low, the viscosity of the polyurethane will increase, the chain will not be easy to extend, the structure will be difficult to shape, and polyurethane that can be used in practice cannot be obtained; if the R value content is too high, the reaction activity will surge, and it will be difficult to regulate the molding and processing of the polyurethane. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 1 is a loss factor-temperature curve diagram of the polyurethane material described in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0026] The present invention will be further described in detail below in conjunction with specific embodiments.
[0027] Example 1
[0028] In this example, the molecular weight of diphenylmethane diisocyanate is 250, and the molecular weight of polycaprolactone triol is 4950. The R value of the system is 3.
[0029] (1) In a three-necked flask, 163 g of polycaprolactone triol was dehydrated at 110° C. and -0.1 MPa vacuum for 4 h;
[0030] (2) Add 37 g of diphenylmethane diisocyanate into the flask described in (1) under a protective gas of N 2 The temperature was raised to 80°C in the atmosphere, and the raw materials were stirred at a rate of 200 r / min to make them uniformly mixed, and reacted with polycaprolactone triol for 4 hours;
[0031] (3) The product obtained in (2) was placed in an environment of 80° C. and cured for 36 hours to obtain a polyurethane material with a wide damping temperature range.
[0032] Example 2
[0033] In this example, the molecular weight of isophorone diisocyanate is 222, and the molecular weight of polycaprolactone triol is 4750. The R value of the system is 4.
[0034] (1) In a three-necked flask, 156 g of polycaprolactone triol was dehydrated at 110° C. and -0.1 MPa vacuum for 4 h;
[0035] (2) Add 44 g of isophorone diisocyanate to the flask described in (1) under a protective gas of N 2 The temperature was raised to 80°C in the atmosphere, and the raw materials were stirred at a rate of 200 r / min to make them uniformly mixed, and reacted with polycaprolactone triol for 4 hours;
[0036] (3) The product obtained in (2) was placed in an environment of 80° C. and cured for 36 hours to obtain a polyurethane material with a wide damping temperature range.
[0037] Example 3
[0038] In this example, the molecular weight of toluene diisocyanate is 174, and the molecular weight of polyoxypropylene triol is 4500. The R value of the system is 5.
[0039] (1) In a three-necked flask, dehydrate 155 g of polyoxypropylene triol at 110° C. and -0.1 MPa vacuum for 4 h;
[0040] (2) Add 45 g of toluene diisocyanate into the flask described in (1) and place under a protective gas of N 2 The temperature was raised to 80°C in the atmosphere, and the raw materials were stirred at a rate of 200 r / min to make them uniformly mixed, and reacted with polyoxypropylene triol for 4 hours;
[0041] (3) The product obtained in (2) was placed in an environment of 80° C. and cured for 36 hours to obtain a polyurethane material with a wide damping temperature range.
[0042] Comparative Example 1
[0043] In this comparative example 1, the molecular weight of diphenylmethane diisocyanate is 250, and the molecular weight of polyether diol is 2000. The R value of the system is 3.
[0044] (1) In a three-necked flask, 96 g of polyether diol was dehydrated at 110° C. and -0.1 MPa vacuum for 4 h;
[0045] (2) Add 144 g of toluene diisocyanate into the flask described in (1) under a protective gas of N 2The temperature was raised to 80°C in the atmosphere, and the raw materials were stirred at a rate of 200 r / min to make them uniformly mixed, and reacted with the polyether diol for 4 hours;
[0046] (3) The product obtained in (2) was placed in an environment of 80° C. and cured for 24 hours to obtain a polyurethane material.
[0047] Comparative Example 2
[0048] In this example, the molecular weight of diphenylmethane diisocyanate is 250, and the molecular weight of polycaprolactone triol is 4950. The R value of the system is 1.05.
[0049] Steps (1) to (3) are the same as those in Comparative Example 1.
[0050] Comparative Example 3
[0051] In this example, the molecular weight of diphenylmethane diisocyanate is 250, and the molecular weight of polycaprolactone triol is 4950. The R value of the system is 6.
[0052] Steps (1) to (3) are the same as those in Comparative Example 1.
[0053] The final products prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to DMA test. The test conditions were compression mode. A circular sample with a diameter of 8 mm and a thickness of 2 mm was used to perform a fixed-frequency variable temperature test at 10 Hz. The test temperature range was -100°C to 100°C.
[0054] The results of Example 1 and Comparative Example 1 are as follows Figure 1 As shown;
[0055] Example 1 exhibits a loss factor peak shape and phenomenon that is significantly different from that of Comparative Example 1;
[0056] Embodiments 2 to 3 have similar damping temperature range effects as embodiment 1;
[0057] When the R value is between 1 and 3 or higher than 5, Comparative Examples 2 and 3 all exhibit a damping temperature range effect similar to that of Comparative Example 1;
[0058] Examples 1 to 3 form a cross-linked network, which not only has a higher loss factor in the low temperature region than that of Comparative Examples 1 to 3, but also exhibits a higher damping than that of Comparative Examples 1 to 3 in the high temperature region, and has a tendency to move to higher temperatures, thus broadening the use temperature range of polyurethane materials as damping materials. At the same time, the damping temperature range of the material can be adjusted by changing the triol and isocyanate components used in the material, thereby achieving targeted design.
[0059] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyurethane material with a wide damping temperature range, characterized in that: Taking the total mass of raw materials required to prepare the polyurethane material as 100%, the raw material components and their mass fractions are as follows: Isocyanate 80%~85% Polytriol 15%~20% Wherein, the ratio R of the total number of isocyanate groups in the isocyanate to the total number of hydroxyl groups in the polytriol is 3-5; The molecular weight of the polytriol is 4500-5000.
2. The wide damping temperature range polyurethane material according to claim 1, characterized in that: The isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate and isophorone diisocyanate.
3. A wide damping temperature range polyurethane material according to claim 1 or 2, characterized in that: The polytriol is at least one of polycaprolactone triol and polyoxypropylene triol.
4. A method for preparing a polyurethane material with a wide damping temperature range, characterized in that the steps include: (1) subjecting the polytriol to vacuum dehydration treatment; (2) under a protective gas atmosphere, adding isocyanate to the polytriol after vacuum dehydration in step (1), so that the isocyanate reacts with the polytriol; (3) Curing the product obtained in (2) at high temperature to obtain a polyurethane material with a wide damping temperature range.
5. The method for preparing a polyurethane material with a wide damping temperature range according to claim 4, characterized in that: In the step (1), the temperature during the dehydration treatment is 110-120° C., the vacuum degree during the dehydration treatment is -0.1 MPa, and the dehydration treatment time is 2-4 hours.
6. The method for preparing a polyurethane material with a wide damping temperature range according to claim 4 or 5, characterized in that: In the step (2), the protective gas is N2, the reaction temperature is 80-90°C, and the reaction time is 4-8h.
7. The method for preparing a polyurethane material with a wide damping temperature range according to claim 6, characterized in that: In the step (3), the curing temperature is 80-90° C. and the curing time is 36-48 hours.
Citation Information
Patent Citations
Preparation method for polyurethane damping material containing suspension chain structure
CN101220132A
Bio-based polyurethane damping material and preparation method and application thereof
CN113896859A
Laminated damping type polyurethane elastomer and preparation method thereof
CN118404880A
Polyurethane
JP1995292061A
Frothed energy absorbing polyurethane materials and process of manufacture
US20030229154A1
Cited By
Wide-temperature-range polyurethane material with excellent adhesive property and preparation method of wide-temperature-range polyurethane material
CN120923715A
A wide-temperature-range polyurethane material with excellent adhesion properties and its preparation method
CN120923715B