Polishing pad detection window and preparation method thereof
By directly mixing a variety of raw materials and vacuum defoaming and vulcanizing treatment, the polishing pad detection window is prepared, and the problems of insufficient light transmittance and complex preparation process in the prior art are solved, thus achieving efficient polishing pad window preparation and excellent light transmittance rate and anti-aging properties.
Patent Information
- Application Number
- CN202411027614.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The light transmittance of the existing polishing pad windows is insufficient, resulting in low sensitivity and accuracy of polishing endpoint detection, and complex preparation process and low efficiency.
The raw materials such as polyether glycol, aromatic isocyanates, aliphatic isocyanates, amine chain extenders and phenolic antioxidants are directly mixed, and the polishing pad detection window is prepared after vacuum defoaming and vulcanization treatment, and the prepolymer synthesis is discarded to increase Antioxidants to extend window life and improve light transmittance.
The light transmittance and anti-aging properties of the polishing pad window are significantly improved, the preparation process is simplified, and the adhesion effect and service life of the detection window and the polishing pad are improved.
Smart Images

Figure CN118930799A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polishing pads, and in particular to a polishing pad detection window and a preparation method thereof. Background Art
[0002] Chemical Mechanical Ploshing (CMP) is the mainstream polishing process used in the semiconductor industry. Chemical Mechanical Polishing can achieve high-quality polishing on the wafer surface and meet the flatness requirements required by the wafer. The CMP process includes a variety of equipment and consumables, and the polishing pad is one of the most important consumables. The polishing pad and the wafer are continuously rotated and rubbed to achieve a smooth surface.
[0003] In the process of polishing wafers with polishing pads, monitoring the polishing endpoint is a very important process, which is used to terminate the polishing process in time to avoid over-polishing or incomplete polishing of the wafer. Optical in-situ monitoring of the wafer polishing endpoint is commonly used. This technology uses a light beam to pass through the polishing pad window to reach the wafer surface. After reflection, the wafer surface passes through the window in the opposite direction to reach the detector. The detector determines whether polishing is completed by analyzing the roughness and polishing thickness of the wafer surface. However, the sensitivity and accuracy of optical in-situ monitoring mainly depend on the light transmittance of the window.
[0004] The invention patent with application number CN117396308A discloses a method for manufacturing a polishing pad window and a polishing pad manufactured thereby. The polishing pad window is made by mixing a polyurethane prepolymer and a curing agent (MOCA, 4,4′-methylenebis(2-chloroaniline)), and the light transmittance of the window is 5%-12%.
[0005] The invention patent with application number CN116218200A discloses a polyurethane composition and a chemical mechanical polishing pad window made of the composition, using toluene diisocyanate (TDI), dicyclohexylmethane diisocyanate (HMDI) and polytetramethylene ether glycol as raw materials, and continuously stirring at a reaction temperature of 40-100°C for 4-12 hours to obtain a prepolymer. The reaction product prepolymer is then mixed with an aromatic diamine chain extender and polysiloxane microspheres for reaction, and then degassed and vulcanized to finally prepare a window sample with a light transmittance of 30%-70%.
[0006] Therefore, the light transmittance of the existing polishing pad window still cannot meet the requirements of high-precision detection, there may be deviations in capturing the polishing end point, and the preparation process is cumbersome, requiring the synthesis of prepolymers or the purchase of prepolymers, and then reacting with chain extenders, resulting in low preparation efficiency. Summary of the invention
[0007] The purpose of the present invention is to provide a polishing pad detection window and a preparation method thereof in order to overcome the defects of the prior art.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] A method for preparing a polishing pad detection window comprises the following steps:
[0010] (a) preparing a raw material mixture, wherein the weight ratio of the components in the raw material mixture is: 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol, and 0.1-0.7 parts of phenolic antioxidant;
[0011] (b) subjecting the raw material mixture to vacuum degassing to obtain a degassed mixture;
[0012] (c) curing and vulcanizing the deaerated mixture to obtain a vulcanized sample;
[0013] (d) Slicing the sulfurized sample to obtain a detection window.
[0014] In one embodiment, the weight ratio of the components in the raw material mixture is: 46.2 parts of polyether diol, 10.5 parts of aromatic isocyanate, 27.3 parts of aliphatic isocyanate, 9.7 parts of amine chain extender, 5.8 parts of diol, and 0.5 parts of phenolic antioxidant.
[0015] In one embodiment, the polyether diol is polytetramethylene ether diol with an average molecular weight of 600 to 2000.
[0016] In one embodiment, the aromatic isocyanate is one or more of toluene diisocyanate, diphenyl diisocyanate, and naphthalene 1,5-diisocyanate;
[0017] The aliphatic isocyanate is one or more of hexamethylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane diisocyanate;
[0018] The amine chain extender is one or more of 4,4'-methylenebis(2-chloroaniline), diethyltoluenediamine, and m-phenylenediamine;
[0019] The diol is one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol and diethylene glycol.
[0020] In one embodiment, the phenolic antioxidant is 2,6-di-tert-butyl-p-cresol.
[0021] In one embodiment, in the step (a), the following steps are included:
[0022] Weigh 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol and 0.1-0.7 parts of phenolic antioxidant respectively according to the weight ratio;
[0023] The weighed polyether diol is heated to 55° C. to 60° C.;
[0024] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0025] In one embodiment, in the step (b), the following steps are included: using a vacuum degassing machine to vacuum degas the raw material mixture, the vacuum degree of the vacuum degassing machine is 90-110 kPa, the rotation speed is 750-950 rpm, and the processing time is 1-3 min.
[0026] In one embodiment, in the step (c), the following steps are included: placing the degassing mixture into a molding mold; placing the molding mold into a vulcanizer, the treatment temperature is 100-105°C, the treatment time is 12-14h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0027] In one embodiment, in step (d), the thickness of the detection window is 1.5-2.5 mm.
[0028] A polishing pad detection window is obtained by the preparation method of the polishing pad detection window.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] 1. Compared with the traditional polishing pad window production formula, the above polishing pad detection window preparation method does not use polyurethane prepolymer, but directly mixes and degasses a variety of raw materials, abandons the synthesis or procurement of prepolymers, greatly improves efficiency, shortens the process flow, and adds phenolic antioxidants to the raw materials, which not only has a degassing effect, but also can inhibit and delay the oxidative degradation of the window, thereby extending the service life of the window and effectively improving the light transmittance and anti-aging properties of the window.
[0031] 2. Using isophorone diisocyanate (IPDI) as the raw material can significantly improve the light transmittance of the window and has good chemical resistance, which can prevent the polishing liquid from corroding the detection window during polishing.
[0032] 3. Diethyltoluenediamine (DETDA) is used as a chain extender. Since diethyltoluenediamine (DETDA) has low reactivity, it will not form gel immediately when in contact with isocyanate. This can prevent the raw material mixture from generating gel before degassing is completed during the preparation process, thereby effectively extending the degassing time.
[0033] 4. Antioxidant 264 is used to fully degas the raw material mixture, so that there are no bubbles in the detection window. At the same time, the bonding effect between the detection window and the polishing pad is significantly improved to avoid falling off between the detection window and the polishing pad. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The figure is a flow chart of the method for preparing the polishing pad detection window of the present invention. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0036] The polishing pad detection window and the preparation method thereof are described in detail below with reference to the accompanying drawings.
[0037] like Figure 1 As shown, in one embodiment, a method for preparing a polishing pad detection window is provided, comprising the following steps:
[0038] (a) preparing a raw material mixture, wherein the weight ratio of the components in the raw material mixture is: 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol, and 0.1-0.7 parts of phenolic antioxidant;
[0039] (b) subjecting the raw material mixture to vacuum degassing to obtain a degassed mixture;
[0040] (c) curing and vulcanizing the deaerated mixture to obtain a vulcanized sample;
[0041] (d) Slicing the sulfurized sample to obtain a detection window.
[0042] Among them, polyether diol, aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenol antioxidant are all commercially available.
[0043] Specifically, in one embodiment, the weight ratio of each component in the raw material mixture is: 46.2 parts of polyether diol, 10.5 parts of aromatic isocyanate, 27.3 parts of aliphatic isocyanate, 9.7 parts of amine chain extender, 5.8 parts of diol, and 0.5 parts of phenolic antioxidant.
[0044] Furthermore, in one embodiment, the weight ratio of each component in the raw material mixture is: 44 parts of polyether diol, 9 parts of aromatic isocyanate, 25 parts of aliphatic isocyanate, 8 parts of amine chain extender, 4 parts of diol, and 0.1 parts of phenolic antioxidant.
[0045] Furthermore, in one embodiment, the weight ratio of each component in the raw material mixture is: 47 parts of polyether diol, 11 parts of aromatic isocyanate, 28 parts of aliphatic isocyanate, 11 parts of amine chain extender, 6 parts of diol, and 0.7 parts of phenolic antioxidant.
[0046] Specifically, in one embodiment, the polyether diol is polytetramethylene ether diol (PTMG) having an average molecular weight of 600 to 2000. Preferably, the average molecular weight of polytetramethylene ether diol is 1000.
[0047] Specifically, in one embodiment, the aromatic isocyanate is one or more of toluene diisocyanate (TDI), diphenyl diisocyanate (MDI), and naphthalene 1,5-diisocyanate (NDI). Preferably, the aromatic isocyanate is diphenyl diisocyanate (MDI), which has low toxicity and good moldability of the manufactured window.
[0048] Specifically, in one embodiment, the aliphatic isocyanate is one or more of hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and dicyclohexylmethane diisocyanate (HMDI). Preferably, the aliphatic isocyanate is isophorone diisocyanate (IPDI). Since the reactivity of aliphatic isocyanates is lower than that of aromatic isocyanates, the produced detection window has excellent light stability and chemical resistance, and good light transmittance.
[0049] Specifically, in one embodiment, the amine chain extender is one or more of 4,4'-methylenebis(2-chloroaniline) (MOCA), diethyltoluenediamine (DETDA), and metaphenylenediamine. Preferably, the amine chain extender is diethyltoluenediamine (DETDA), which has low toxicity, is liquid at room temperature, and has low reactivity. It will not form a gel immediately after contacting with aromatic isocyanate, which is conducive to the full and uniform mixing of the raw material mixture.
[0050] Specifically, in one embodiment, the diol is one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, and diethylene glycol (DEG). More preferably, the diol is diethylene glycol (DEG), which is a colorless transparent liquid and is widely used in polyurethane high-resilience foam, microporous foam, elastomer, and high-density rigid foam, which can improve the resilience of foam plastic products and produce a dense epidermis.
[0051] Specifically, in one embodiment, the phenolic antioxidant is 2,6-di-tert-butyl-p-cresol (antioxidant 264). 2,6-di-tert-butyl-p-cresol is non-toxic, non-corrosive, has good storage stability, can inhibit or delay the oxidative degradation of plastics and extend the service life, thereby effectively improving the light stability, processing stability, mechanical strength, color stability and transparency of the detection window, and also has a defoaming effect, further reducing the production of bubbles in the detection window and improving the light transmittance of the detection window.
[0052] Specifically, in one embodiment, in the step (a), the following steps are included:
[0053] Weigh 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol and 0.1-0.7 parts of phenolic antioxidant respectively according to weight percentage;
[0054] The weighed polyether diol is heated to 55° C. to 60° C.;
[0055] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0056] Specifically, in one embodiment, in the step (b), the following steps are included: using a vacuum degassing machine to vacuum degas the raw material mixture, the vacuum degree of the vacuum degassing machine is 90-110 kPa, the rotation speed is 750-950 rpm, and the processing time is 1-3 min.
[0057] Specifically, in one embodiment, in the step (c), the following steps are included: placing the degassing mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 100 to 105° C. and a treatment time of 12 to 14 hours, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0058] Specifically, in one embodiment, in the step (d), the thickness of the detection window is 1.5-2.5 mm.
[0059] In one embodiment, a polishing pad detection window is provided, and the polishing pad detection window is obtained by the above-mentioned preparation method:
[0060] (a) preparing a raw material mixture according to the components, wherein the raw material mixture includes 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol, and 0.1-0.7 parts of phenolic antioxidant;
[0061] (b) subjecting the raw material mixture to vacuum degassing to obtain a degassed mixture;
[0062] (c) curing and vulcanizing the deaerated mixture to obtain a vulcanized sample;
[0063] (d) Slicing the sulfurized sample to obtain a detection window.
[0064] The present invention is further described below with reference to the examples. The raw material proportions of Examples 1 to 4 are shown in Table 1.
[0065] Example 1
[0066] The polishing pad detection window is prepared by the following method and steps:
[0067] (a) 47 parts of polytetramethylene glycol (PTMG), 10.1 parts of diphenyl diisocyanate (MDI), 27.3 parts of isophorone diisocyanate (IPDI), 10 parts of diethyltoluenediamine (DETDA), 5.1 parts of diethylene glycol (DEG) and 0.5 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0068] The weighed polyether glycol is heated to 60° C.;
[0069] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0070] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0071] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0072] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0073] Example 2
[0074] Compared with Example 1, Example 2 has the same process conditions except for the different ratio of the raw material mixture. The polishing pad detection window is prepared by the following method steps:
[0075] (a) 45.3 parts of polytetramethylene glycol (PTMG), 10.9 parts of diphenyl diisocyanate (MDI), 27.9 parts of isophorone diisocyanate (IPDI), 10.1 parts of diethyltoluenediamine (DETDA), 5.2 parts of diethylene glycol (DEG) and 0.6 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0076] The weighed polyether glycol is heated to 60° C.;
[0077] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0078] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0079] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0080] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0081] Example 3
[0082] Compared with Example 1, Example 3 has the same process conditions except for the different ratio of the raw material mixture. The polishing pad detection window is prepared by the following method steps:
[0083] (a) 46.9 parts of polytetramethylene glycol (PTMG), 10.0 parts of diphenyl diisocyanate (MDI), 26.8 parts of isophorone diisocyanate (IPDI), 11 parts of diethyltoluenediamine (DETDA), 5.0 parts of diethylene glycol (DEG) and 0.3 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0084] The weighed polyether glycol is heated to 60° C.;
[0085] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0086] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0087] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0088] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0089] Example 4
[0090] Compared with Example 1, except for the different ratio of the raw material mixture, all process conditions are the same, and the polishing pad detection window is prepared by the following method steps:
[0091] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of diphenyl diisocyanate (MDI), 28 parts of isophorone diisocyanate (IPDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0092] The weighed polyether glycol is heated to 60° C.;
[0093] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0094] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0095] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0096] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0097] Table 2 shows the different raw material components of Examples 5 to 8.
[0098] Example 5
[0099] Example 5 Compared with Example 4, hexamethylene diisocyanate (HDI) is used to replace isophorone diisocyanate (IPDI) as the aliphatic isocyanate component. In addition, the ratio and process conditions of all raw material mixtures are the same. The polishing pad detection window is prepared by the following method steps:
[0100] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of diphenyl diisocyanate (MDI), 28 parts of hexamethylene diisocyanate (HDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0101] The weighed polyether glycol is heated to 60° C.;
[0102] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0103] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0104] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0105] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0106] Example 6
[0107] Example 6 Compared with Example 4, dicyclohexylmethane diisocyanate (HMDI) is used to replace isophorone diisocyanate (IPDI) as the aliphatic isocyanate component. In addition, the ratio and process conditions of all raw material mixtures are the same. The polishing pad detection window is prepared by the following method steps:
[0108] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of diphenyl diisocyanate (MDI), 28 parts of dicyclohexylmethane diisocyanate (HMDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0109] The weighed polyether glycol is heated to 60° C.;
[0110] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0111] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0112] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0113] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0114] Example 7
[0115] Compared with Example 4, toluene diisocyanate (TDI) is used to replace diphenyl diisocyanate (MDI) as the aromatic isocyanate component. In addition, the proportions and process conditions of all raw material mixtures are the same. The polishing pad detection window is prepared by the following method steps:
[0116] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of toluene diisocyanate (TDI), 28 parts of isophorone diisocyanate (IPDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0117] The weighed polyether glycol is heated to 60° C.;
[0118] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0119] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0120] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0121] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0122] Example 8
[0123] Example 8 Compared with Example 4, naphthalene 1,5-diisocyanate (NDI) is used to replace diphenyl diisocyanate (MDI) as the aromatic isocyanate component. In addition, the ratio and process conditions of all raw material mixtures are the same. The polishing pad detection window is prepared by the following method steps:
[0124] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of naphthalene 1,5-diisocyanate (NDI), 28 parts of isophorone diisocyanate (IPDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 part of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0125] The weighed polyether glycol is heated to 60° C.;
[0126] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0127] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 100 kPa, the rotation speed is 850 rpm, and the processing time is 2 min.
[0128] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0129] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0130] As shown in Table 5, Example 4 and Examples 9 to 10 have different vacuum release treatment processes.
[0131] Example 9
[0132] Compared with Example 4, Example 9 changed the process conditions of vacuum degassing during the preparation process, and the polishing pad detection window was prepared by the following method steps:
[0133] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of diphenyl diisocyanate (MDI), 27.328 parts of isophorone diisocyanate (IPDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0134] The weighed polyether glycol is heated to 60° C.;
[0135] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0136] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 90 kPa, the rotation speed is 750 rpm, and the processing time is 1 min.
[0137] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0138] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0139] Example 10
[0140] Compared with Example 4, Example 10 changes the process conditions of vacuum degassing during the preparation process, and adopts the following method steps to prepare the polishing pad detection window:
[0141] (a) 46.2 parts of polytetramethylene glycol (PTMG), 10.5 parts of diphenyl diisocyanate (MDI), 27.328 parts of isophorone diisocyanate (IPDI), 9.7 parts of diethyltoluenediamine (DETDA), 5.6 parts of diethylene glycol (DEG) and 0.7 parts of 2,6-di-tert-butyl-p-cresol (antioxidant 264) were weighed respectively according to weight percentage;
[0142] The weighed polyether glycol is heated to 60° C.;
[0143] The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
[0144] (b) The raw material mixture is subjected to vacuum degassing treatment by using a vacuum degassing machine, wherein the vacuum degree of the vacuum degassing machine is 110 kPa, the rotation speed is 950 rpm, and the processing time is 3 min.
[0145] (c) placing the deaerated mixture into a molding mold; placing the molding mold into a vulcanizer, with a treatment temperature of 103° C. and a treatment time of 13 h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
[0146] (d) Slicing the vulcanized sample to obtain a detection window, wherein the thickness of the detection window is 2.0 mm.
[0147] The polishing pad inspection windows obtained in Examples 1 to 10 were tested for light transmittance, heat aging and adhesion.
[0148] The light transmittance test is carried out in accordance with GB2410-2008 “Test method for light transmittance and haze of transparent plastics”.
[0149] Thermal aging test: The time required for the polishing pad detection window to change from white to yellow is measured when the detection window is placed in a 160°C environment.
[0150] Adhesion test: After the detection window and the polishing pad are installed and combined, the adhesion between the window and the polishing pad is tested using a universal material testing machine.
[0151] From the test results in Table 2, it can be seen that the light transmittance of the polishing pad detection window obtained in Examples 1 to 4 can reach about 80%, the light transmittance is effectively improved, and the heat aging resistance is also improved. And as the content of antioxidant 264 gradually increases, the light transmittance can reach up to 83%, and the color change after aging treatment is minimal. Therefore, under the raw material ratio and process conditions of Example 4, the obtained detection window has the best light transmittance, the strongest anti-aging ability, and the largest window adhesion.
[0152] From the test results in Table 4, it can be seen that the light transmittance of the polishing pad detection window obtained in Examples 5 to 9 can reach about 80%, and the light transmittance is effectively improved. Since IPDI has a positive effect on the light transmittance, the light transmittance of Examples 7 to 8 is higher than that of Examples 5 and 6. Due to the presence of antioxidant 264 and the consistent addition amount in Examples 5 to 9, the heat aging resistance is basically the same and relatively excellent. And due to the presence of antioxidant 264 and the consistent addition amount in Examples 5 to 9, the window adhesion is also relatively consistent and relatively excellent. Therefore, under the raw material composition, ratio and process conditions of Example 4, the obtained detection window has the best light transmittance, the strongest anti-aging ability and the largest window adhesion.
[0153] From the test results in Table 6, it can be seen that in Example 9, due to low vacuum degree, low rotation speed and short time, the mixture has a small amount of bubbles, resulting in lower window transmittance than in Example 4 and Example 10. In Example 10, due to high vacuum degree, high rotation speed and long time, the heat aging resistance and bonding force of the window are lower than those of Example 9 and Example 4. Therefore, the polishing pad obtained in Example 4 has the best window transmittance, the strongest anti-aging ability and the largest window bonding force.
[0154] Table 1: Raw material ratios in Examples 1 to 4.
[0155] Raw material name Example 1 Example 2 Example 3 Example 4 PTMG 47.0 45.3 46.9 46.2 MDI 10.1 10.9 10.0 10.5 IPDI 27.3 27.9 26.8 28.0 DETDA 10.0 10.1 11 9.7 DEG 5.1 5.2 5.0 5.6 Antioxidant 264 0.5 0.6 0.3 0.7
[0156] Table 2: Test results of Examples 1 to 4
[0157] Detection parameters Example 1 Example 2 Example 3 Example 4 Transmittance % 80 81 76 83 Heat aging resistance (min / 160℃) 15 30 16 36 Adhesion force of window N 19 33 20 35
[0158] Table 3: Raw material composition in Examples 5 to 8
[0159]
[0160]
[0161] Table 4: Test results of Examples 5 to 8
[0162] Detection parameters Example 5 Example 6 Example 7 Example 8 Transmittance % 80 80 82 83 Heat aging resistance (min / 160℃) 35 36 34 35 Adhesion force of window N 35 35 34 35
[0163] Table 5: Process conditions for vacuum degassing in Examples 9 to 11
[0164] Process conditions Example 9 Example 10 Embodiment 11 Vacuum degree KPa 90 100 110 Speed rpm 750 850 950 Time min 1 2 3
[0165] Table 6: Test results of Examples 4, 9-10
[0166] Detection parameters Example 9 Example 4 Example 10 Transmittance % 80 83 82 Heat aging resistance (min / 160℃) 35 36 34 Adhesion force of window N 35 35 34
[0167] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0168] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a polishing pad detection window, It is characterized in that The steps include: (a) preparing a raw material mixture, wherein the weight ratio of the components in the raw material mixture is: 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol, and 0.1-0.7 parts of phenolic antioxidant; (b) subjecting the raw material mixture to vacuum degassing to obtain a degassed mixture; (c) curing and vulcanizing the deaerated mixture to obtain a vulcanized sample; (d) Slicing the sulfurized sample to obtain a detection window.
2. A method for preparing a polishing pad detection window according to claim 1, It is characterized in that The weight ratio of each component in the raw material mixture is: 46.2 parts of polyether diol, 10.5 parts of aromatic isocyanate, 27.3 parts of aliphatic isocyanate, 9.7 parts of amine chain extender, 5.8 parts of diol, and 0.5 parts of phenolic antioxidant.
3. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that The polyether diol is polytetrahydrofuran ether diol with an average molecular weight of 600-2000.
4. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that The aromatic isocyanate is one or more of toluene diisocyanate, diphenyl diisocyanate, and naphthalene 1,5-diisocyanate; The aliphatic isocyanate is one or more of hexamethylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane diisocyanate; The amine chain extender is one or more of 4,4'-methylenebis(2-chloroaniline), diethyltoluenediamine, and m-phenylenediamine; The diol is one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol and diethylene glycol.
5. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that The phenolic antioxidant is 2,6-di-tert-butyl-p-cresol.
6. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that In the step (a), the following steps are included: Weigh 44-47 parts of polyether diol, 9-11 parts of aromatic isocyanate, 25-28 parts of aliphatic isocyanate, 8-11 parts of amine chain extender, 4-6 parts of diol and 0.1-0.7 parts of phenolic antioxidant respectively according to the weight ratio; The weighed polyether diol is heated to 55-60° C.; The weighed aromatic isocyanate, aliphatic isocyanate, amine chain extender, diol and phenolic antioxidant are sequentially added to the polyether diol, and mixed evenly to obtain a raw material mixture.
7. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that In the step (b), the following steps are included: using a vacuum degassing machine to vacuum degas the raw material mixture, the vacuum degree of the vacuum degassing machine is 90-110 kPa, the rotation speed is 750-950 rpm, and the processing time is 1-3 minutes.
8. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that In the step (c), the following steps are included: placing the degassing mixture into a molding mold; placing the molding mold into a vulcanizer, the treatment temperature is 100-105°C, the treatment time is 12-14h, completing the curing molding and vulcanization treatment to obtain a vulcanized sample.
9. The method for preparing a polishing pad detection window according to claim 1, It is characterized in that In the step (d), the thickness of the detection window is 1.5 to 2.5 mm.
10. A polishing pad detection window, It is characterized in that The polishing pad detection window is obtained by the preparation method of any one of claims 1-9.
Citation Information
Cited By
Polishing pad end point inspection window as well as preparation method and application thereof
CN120923724A