Mortar admixture as well as preparation method and application thereof

The mortar admixture prepared by the esterification reaction of modified amino acids and polyglycerols has solved the problems of poor stability and short working time in the prior art, achieved high stability and long working time of the mortar, and simplified the compounding process , and improves the overall state of the mortar.

CN118930841APending Publication Date: 2024-11-12BOTE NEW MATERIALS TAIZHOU JIANGYAN CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410992873.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the compounding process of existing mortar admixtures, due to the large variety and mutual influence, the mortar is poor in stability, short working time, and compatibility problems affecting the overall state.

Method used

By esterifying the amino acid and hydrolyzing it with ethylene oxide, forming a modified amino acid, and then esterifying with polyglycerol, a mortar admixture containing dipolyether chains and polyglycerol structure is obtained to improve the mortar stability and working hours.

Benefits of technology

This mortar admixture has the effect of retaining water and gas extraction in a cement alkaline environment, enhancing the stability and working time of the mortar, simplifying the compounding process, avoiding the problem of uneven solution, and significantly improving the overall state of the mortar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959342620000031
    Figure BDA0004959342620000031
  • Figure BDA0004959342620000032
    Figure BDA0004959342620000032
  • Figure BDA0004959342620000033
    Figure BDA0004959342620000033
Patent Text Reader

Abstract

The invention provides a mortar admixture as well as a preparation method and application thereof, and the mortar admixture is prepared by the following steps: firstly carrying out esterification reaction on amino acid, then reacting an esterification product with ethylene oxide, finally hydrolyzing and reducing carboxyl functional groups in an amino acid structure, and then carrying out esterification reaction on the modified amino acid and polyglycerol. Finally, the cement mortar admixture with a novel structure is obtained. When in use, the mortar admixture can be prepared into solid powder and can also be dissolved in water to be prepared into a mortar admixture solution with the mass concentration not higher than 20%. The novel mortar admixture has the effects of water retention, delayed coagulation and air entraining in a cement alkaline environment, the delayed coagulation time is prolonged, the water retention performance of mortar is enhanced, the stability of the mortar can be improved, the working time of the mortar can be prolonged, and the novel mortar admixture has a very good effect when being applied to the mortar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a mortar admixture and a preparation method and application thereof. Background Art

[0002] With the rapid development of Chinese cities, the increase in infrastructure and the number of houses has led to a gradual increase in the proportion of building energy consumption. As a major building material second only to wall materials and concrete, building mortar is used in an annual amount of hundreds of millions of tons. Mortar admixtures are a series of materials, divided into masonry mortar and plastering mortar. It is an additive added to cement and sand to improve the performance of cement mortar. In cement wet mortar without mortar admixtures, there are often rapid losses, poor workability and poor workability.

[0003] After searching, Chinese patent CN 114656189 A discloses a two-group early-strength wet-mix masonry mortar admixture, which is mainly compounded with water reducer, air entraining agent, water retaining agent, early strength agent, emulsifier, and retarder. The mortar has good workability and construction properties, increases the early compressive strength and bonding strength of the mortar, and solves the problem of short storage time of mortar admixtures. However, we know that the retarder inhibits the hydration rate of cement and prolongs the initial setting time of cement, while the early strength agent has the opposite effect, which is to increase the hydration rate and facilitate the early improvement of concrete strength. Mixing the two will inevitably affect their respective effects.

[0004] Chinese patent CN 115321872 A discloses a method for preparing a mortar admixture, the main components of which are synthetic end-functionalized polycarboxylic acid and dispersant, which are compounded with polyether viscosity regulator, thickener, retarder, air entraining agent, and reinforcing agent, and can improve the fluidity and anti-separation of the mortar, so that it has excellent working performance and mortar strength. Chinese patent CN 114853386A discloses a machine-made sand mortar admixture, which is mainly compounded with polycarboxylic acid water reducer, polycarboxylic acid collapse retainer, organic retarder, air entraining agent, organosilicon defoamer, water retainer, and mud inhibitor, which improves the water-locking, water-retaining and collapse-retaining performance of wet-mixed mortar and inhibits the influence of machine-made sand on the working performance of the admixture, while not affecting the working performance of the wet-mixed mortar, and achieves the purpose of improving the stability of the wet-mixed mortar and avoiding water seepage and stratification of the wet-mixed mortar. Summary of the invention

[0005] In view of the prior art, the mortar admixtures currently used in the market are mainly obtained by compounding and dissolving several products. During use, because there are many varieties added, not only may the products directly affect each other's effects, but they may also have compatibility problems directly in the aqueous solution, thereby affecting a series of problems such as the overall state of the mixed mortar. The present application proposes a mortar admixture and its preparation method and application. The admixture is first esterified with an amino acid, and then the esterified product is reacted with ethylene oxide, and finally the carboxyl functional group in the amino acid structure is hydrolyzed and reduced, and the modified amino acid is esterified with polyglycerol to finally obtain a cement mortar admixture containing a dipolyether chain and a polyglycerol structure. It can improve the stability of the mortar, extend the working time of the mortar, and has a very good effect when used in the mortar.

[0006] A mortar admixture, which is obtained by reacting polyglycerol with modified amino acid under catalyst conditions;

[0007] The molar ratio of the polyglycerol, modified amino acid and catalyst is 1:(4-22):(0.1-0.5);

[0008] The general structural formula of the polyglycerol is shown in the following formula (A):

[0009] Among them, n=3-20; polyglycerol contains a large number of hydroxyl groups. Under the premise of good solubility, the higher the degree of polymerization, the better the water retention effect.

[0010] The general structural formula of the modified amino acid is shown in the following formula (B):

[0011] Among them, R is H, CH3, CH2-CH(CH3)2, CH(CH3)2, CH2-C6H5, CH2-CH2-S-CH3, and m=5~7.

[0012] The structure of the mortar admixture of the present application conforms to the following general formula (R):

[0013] Among them, R is H, CH3, CH2-CH(CH3)2, CH(CH3)2, CH2-C6H5, CH2-CH2-S-CH3, n=3~20; m=5~7.

[0014] The modified amino acid is prepared by the following steps: (a) subjecting an amino acid to an esterification reaction with a halogenated benzene under acidic conditions to obtain an amino acid esterification product; (b) subjecting the esterification product obtained in step (a) to an addition reaction with ethylene oxide under alkaline catalyst conditions to obtain an amino acid addition product; (c) subjecting the addition product obtained in step (b) to hydrolysis under alkaline conditions and acid treatment to obtain a product with a carboxyl group, namely, the modified amino acid.

[0015] The preparation steps of the modified amino acid are as follows: the first step is to place the amino acid and the halogenated benzene in a reaction kettle, and react at room temperature for 2 to 5 hours under acidic conditions to obtain an amino acid esterification product; the second step is to place the amino acid esterification product and the catalyst in a reaction kettle, and when the reaction kettle is sealed, nitrogen is introduced to remove the air in the kettle, and then the temperature is raised to 130 to 155° C., and ethylene oxide is slowly introduced into the reaction kettle under the condition that the reaction pressure is less than 0.6 MPa, and the reaction kettle is aged for 1 to 3 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the third step is to hydrolyze the amino acid addition product under alkaline conditions and reflux for 20 to 24 hours, and then subject it to acidic treatment to obtain a product with a carboxyl group, namely the modified amino acid.

[0016] The reaction structure of the first step of preparing the modified amino acid is shown in the following formula (1):

[0017]

[0018] The reaction structure of the second step of the preparation of modified amino acids is shown in the following formula (2):

[0019]

[0020] The reaction structure of the third step of the preparation of modified amino acids is shown in the following formula (3):

[0021]

[0022] The molar ratio of the amino acid, halogenated benzene, ethylene oxide and alkaline catalyst is 1:1:(10-14):(0.01-0.1).

[0023] The amino acid in the above step (a) is any one of glycine, alanine, leucine, valine, phenylalanine and methionine, or a mixture of two or more of them in any proportion.

[0024] It should be noted that products containing both carboxyl and amino groups in their molecular structures can also undergo the reaction shown in formula (1) and can also be used to prepare subsequent mortar admixtures.

[0025] In the above step (a), the halogenated benzene is any one of iodobenzene and bromobenzene.

[0026] In the above step (b), the alkaline catalyst is any one of potassium hydroxide, sodium hydroxide, potassium alcoholate, sodium alcoholate and metallic sodium.

[0027] The catalyst is a mixture of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, and the mixing mass ratio is (1-25):5.

[0028] A method for preparing a mortar admixture specifically comprises the following steps: (1) preparing a modified amino acid; (2) dissolving the modified amino acid prepared in step (1) in water, adding polyglycerol and a catalyst, and stirring at room temperature for 4 to 8 hours to obtain the mortar admixture.

[0029] The reaction structure of the mortar admixture preparation is shown in the following formula (4):

[0030]

[0031] A method for applying a mortar admixture. The mortar admixture can be prepared into a solid powder when used, or dissolved in water to form a mortar admixture solution with a mass concentration of no more than 20%; the solid dosage of the mortar admixture when used is 0.1%-5% of the amount of cementitious material used.

[0032] Compared with the prior art, this application has the following advantages:

[0033] (1) Currently, mortar admixtures on the market are basically compounded, while the new mortar admixture of the present application has the effect of retaining water and entraining air in the cement alkaline environment, thereby enhancing the water retention performance of the mortar. The new mortar admixture can improve the stability of the mortar and extend the working time of the mortar, and its application in the mortar has a very good effect.

[0034] (2) The mortar admixture of the present application is a material, and therefore, is easier to use. It can also reduce the risk of errors in the compounding of traditional mortar admixtures, and avoid the occurrence of problems such as precipitation due to immiscible substances during compounding, thereby making the prepared solution uneven. The mortar admixture of the present application has multiple functions to improve the state of the mortar, such as air entrainment and water retention, and has a much better effect on improving the overall state of the mortar. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The raw materials used in the following examples and comparative examples were all purchased commercially. The catalyst EDC / NHS ratio in Example 1 and Example 2 was 1:5, the catalyst EDC / NHS ratio in Example 3 and Example 4 was 1:1, and the catalyst EDC / NHS ratio in Example 5 and Example 6 was 5:1.

[0037] Example 1

[0038] The modified amino acid synthesis steps are as follows: 1 mol of alanine and 1.05 mol of iodobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 2 hours, and an amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of sodium methoxide are placed in a reactor, sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 140°C, and 10 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 2 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105°C, the hydrolysis is refluxed for 20 hours, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0039] 5 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of triglycerol and 0.15 mol of catalyst EDC / NHS were added into the reactor. The mixture was stirred at room temperature for 4 hours to obtain a mortar admixture.

[0040] Example 2

[0041] The modified amino acid synthesis steps are as follows: 1 mol of glycine and 1.05 mol of iodobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 3 hours, and an amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of sodium methoxide are placed in a reactor, sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 130° C., and 12 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 2 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105° C., the hydrolysis is refluxed for 20 hours, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0042] 6 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of tetraglycerol and 0.15 mol of catalyst EDC / NHS were added into the reactor, and the mixture was stirred at room temperature for 4 hours to obtain a mortar admixture.

[0043] Example 3

[0044] The modified amino acid synthesis steps are as follows: 1 mol of leucine and 1.05 mol of iodobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 2 hours, and an amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of sodium methoxide are placed in a reactor, sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 140°C, and 10 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 2 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105°C, the hydrolysis is refluxed for 20 hours, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0045] 8 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of hexaglycerol and 0.2 mol of catalyst EDC / NHS were added into the reactor, and the mixture was stirred at room temperature for 6 hours to obtain a mortar admixture.

[0046] Example 4

[0047] The modified amino acid synthesis steps are as follows: 1 mol of phenylalanine and 1.05 mol of bromobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 2 hours, and an amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of potassium hydroxide are placed in a reactor, which is sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 130° C., and 14 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 1 hour, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105° C., the hydrolysis is refluxed for 20 hours by stirring, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0048] 5 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of triglycerol and 0.2 mol of catalyst EDC / NHS were added into the reactor. The mixture was stirred at room temperature for 4 hours to obtain a mortar admixture.

[0049] Example 5

[0050] The modified amino acid synthesis steps are as follows: 1 mol of glycine and 1.05 mol of bromobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 2 hours, and the amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of sodium methoxide are placed in a reactor, sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 140°C, and 10 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 2 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105°C, the hydrolysis reflux is stirred for 22 hours, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0051] 12 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of decaglycerol and 0.4 mol of catalyst EDC / NHS were added into the reactor, and the mixture was stirred at room temperature for 6 h to obtain a mortar admixture.

[0052] Example 6

[0053] The modified amino acid synthesis steps are as follows: 1 mol of methionine and 1.05 mol of bromobenzene are placed in a reactor, the pH of the solution is adjusted to between 5.0 and 6.0, the reaction is carried out at room temperature, the stirring rate is adjusted to 150 r / min, the reaction time is 5 hours, and the amino acid esterification product is obtained; the 1 mol of amino acid esterification product and 0.1 mol of sodium hydroxide are placed in a reactor, sealed, and then nitrogen is introduced into the sealed reactor to remove the air in the reactor. The temperature is raised to 150°C, and 10 mol of ethylene oxide is slowly introduced into the reactor under the condition of a reaction pressure of 0.5 MPa, and the reaction is aged for 3 hours, and then the temperature is lowered to degas and discharge the material to obtain an amino acid addition product; the 1 mol of amino acid addition product is placed in a reactor, sodium hydroxide solution is added, the pH is adjusted to 8.0-9.0, the reaction temperature is 105°C, the hydrolysis reflux is stirred for 24 hours, and then dilute sulfuric acid is added for treatment to finally obtain a modified amino acid.

[0054] 22 mol of modified amino acid was placed in a reactor, and water was added to dissolve it. Then 1.05 mol of polyglycerol and 0.5 mol of catalyst EDC / NHS were added to the reactor, and the mixture was stirred at room temperature for 8 h to obtain a mortar admixture.

[0055] Comparative Example 1

[0056] Thickening powder, Shanghai Research Institute of Building Science Co., Ltd.

[0057] Comparative Example 2

[0058] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, only modified amino acids are prepared, and no further esterification reaction is carried out between the modified amino acids and polyglycerol. The other reaction conditions are the same as those in Example 1.

[0059] Comparative Example 3

[0060] The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, the amino acid is directly esterified with polyglycerol without reacting with ethylene oxide, and the other reaction conditions are the same as those in Example 1.

[0061] Comparative Example 4

[0062] 5 mol of the modified amino acid obtained in Example 1 and 1.05 mol of triglycerol were uniformly mixed to form an additive.

[0063] Test Example 1: Performance Test:

[0064] In each embodiment and comparative example, the cement used is Conch Cement PO 42.5, the sand is natural sand with a fineness modulus of Mx=2.6, and the fly ash is Grade II. The consistency, water retention rate, and bulk density of the mortar are measured and calculated according to the method described in JGJ / T70-2009 "Standard for Basic Performance Test Methods of Building Mortar". In each embodiment and comparative example, the dosage of admixtures and water consumption are adjusted to maintain the initial consistency of the mortar at 90±5mm and the initial bulk density of the mortar at 1800±50kg / m 3 .

[0065] The performance was compared through mortar tests, and the wet mix mortar ratio is shown in Table 1:

[0066] Table 1

[0067] Conch Cement PO 42.5 / g Fly ash grade II / g Natural sand (Mx = 2.6) / g 220 50 1350

[0068] The performance test results of each embodiment and comparative example are shown in Table 2 below:

[0069] Table 2

[0070]

[0071] It can be seen from the data in Table 2 above that the wet-mixed mortar to which the mortar admixture having a novel structure having multiple functional components (Examples 1 to 6) is added has a 24-hour bulk density loss rate of less than 4.5%, a 32-hour bulk density loss rate of less than 6.5%, and a 48-hour bulk density loss rate of less than 9.5%; the consistency loss is significantly smaller, with an initial consistency of 90±5 mm, a 24-hour consistency loss rate of less than 9.5%, a 32-hour consistency loss rate of less than 17%, and a 48-hour consistency loss rate of less than 22%, and the initial water retention rate can reach more than 91%, and those with better performance can reach more than 95%. Therefore, it can effectively meet the long-term construction requirements of the wet-mixed mortar.

[0072] Comparative Example 1 is a commercially available mortar admixture. Through data comparison, it can be found that its mortar bulk density loss rate and consistency loss rate are significantly higher than those of the new mortar admixture synthesized by the present invention.

[0073] In Comparative Example 2, polyglycerol was not added during the synthesis process, so its water retention was much worse, which also shows that polyglycerol has a good water retention effect in mortar.

[0074] In Comparative Example 3, although polyglycerol was reacted during the synthesis process, the amino acid was not modified by epoxy addition. Therefore, the air entrainment effect of Comparative Example 3 was poor.

[0075] In comparative example 4, pure physical compounding, we can find that its water retention rate is not high, and the bulk density loss and consistency loss are both large, indicating that pure physical compounding cannot achieve the effect of the synthetic product well.

[0076] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A mortar admixture, characterized in that: The mortar admixture is obtained by reacting polyglycerol with modified amino acid under catalyst conditions; The molar ratio of the polyglycerol, the modified amino acid and the catalyst is 1:(4-22):(0.1-0.5); The general structure of the polyglycerol is shown in the following formula (A): Wherein, n=3 to 20; The general structural formula of the modified amino acid is shown in the following formula (B): Wherein, R is H, CH3, CH2-CH(CH3)2, CH(CH3)2, CH2-C6H5, CH2-CH2-S-CH3, and m=5~7.

2. A mortar admixture according to claim 1, characterized in that: The modified amino acid is prepared by the following steps: (a) reacting an amino acid with a halogenated benzene under acidic conditions to obtain an amino acid esterification product; (b) reacting the esterification product obtained in step (a) with ethylene oxide under alkaline catalyst conditions to obtain an amino acid addition product; (c) hydrolyzing the addition product obtained in step (b) under alkaline conditions and subjecting it to acidic treatment to obtain a product with a carboxyl group, namely, a modified amino acid.

3. A mortar admixture according to claim 2, characterized in that: The molar ratio of the amino acid, halogenated benzene, ethylene oxide and alkaline catalyst is 1:1:(10-14):(0.01-0.1).

4. A mortar admixture according to claim 2, characterized in that: The amino acid in step (a) is any one of glycine, alanine, leucine, valine, phenylalanine and methionine, or a mixture of two or more of them in any proportion.

5. A mortar admixture according to claim 2, characterized in that: In the step (a), the halogenated benzene is any one of iodobenzene and bromobenzene.

6. A mortar admixture according to claim 2, characterized in that: In the step (b), the alkaline catalyst is any one of potassium hydroxide, sodium hydroxide, potassium alcoholate, sodium alcoholate and metallic sodium.

7. A mortar admixture according to claim 1, characterized in that: The catalyst is a mixture of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, and the mixing mass ratio is (1-25):

5.

8. The method for preparing a mortar admixture according to any one of claims 1 to 7, characterized in that: The specific steps include: (1) Preparation of modified amino acids; (2) Dissolving the modified amino acids prepared in step (1) in water, adding polyglycerol and a catalyst, and stirring at room temperature for 4 to 8 hours to obtain a mortar admixture.

9. The method for applying the mortar admixture according to any one of claims 1 to 7, characterized in that: The mortar admixture can be prepared into solid powder when used, or dissolved in water to form a mortar admixture solution with a mass concentration of less than 20%; when the mortar admixture is used, its solid content is 0.1%-5% of the amount of the cementitious material.

Citation Information

Patent Citations

  • Two-component early-strength wet-mixed masonry mortar admixture and preparation method thereof

    CN114656189A

  • Machine-made sand wet-mixed mortar admixture

    CN114853386A

  • Wet-mixed mortar admixture as well as preparation method and application thereof

    CN115321872A