Preparation method of high-molecular-weight polyoxamide resin and obtained high-molecular-weight polyoxamide resin

By using the combination of quinoline solvents and metal compounds in the preparation of polyoxalamide resin, the problems of thermal decomposition and molecular weight limitation in traditional methods were solved. High molecular weight polyoxalamide resin was successfully prepared, with an intrinsic viscosity of more than 2dL/g, which was significantly Improved performance.

CN118930843AActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310538146.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

It is difficult to effectively prepare high molecular weight polyoxalamide resins in the prior art. Traditional methods have thermal decomposition problems and molecular weight limitations. The existing catalysts are highly toxic or costly, resulting in limited molecular weight of the prepared polyoxalamide.

Method used

The high molecular weight polyoxalamide resin is prepared by combining quinoline solvents with metal compounds through gradually heating prepolymerization reaction and solid phase polycondensation. The polymerization reaction is promoted by using quinoline solvents and metal compounds, and the reaction conditions are controlled to avoid thermal decomposition. Increase molecular weight.

Benefits of technology

The high molecular weight polyoxalamide resin was successfully prepared under mild conditions, with an intrinsic viscosity greater than 2dL/g, which significantly improved the molecular weight and performance of polyoxalamide and avoided the thermal decomposition and toxicity problems in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004227142910000021
    Figure BDA0004227142910000021
  • Figure HDA0004227142930000011
    Figure HDA0004227142930000011
  • Figure HDA0004227142930000021
    Figure HDA0004227142930000021
Patent Text Reader

Abstract

The invention discloses a preparation method of high-molecular-weight polyoxamide resin and the obtained high-molecular-weight polyoxamide resin, and the preparation method comprises the following steps: (1) carrying out prepolymerization reaction on a diamine compound and oxalic acid and / or oxalic acid diester in the presence of a quinoline solvent and a metal compound by gradually heating, and filtering to obtain a polyoxamide prepolymer; and (2) carrying out solid-phase polycondensation reaction on the polyoxamide prepolymer to obtain the high-molecular-weight polyoxamide resin. According to the present invention, with the preparation method, the high molecular weight polyoxamide can be obtained, and the intrinsic viscosity of the high molecular weight polyoxamide is more than 2 dL / g, preferably 2.1-3 dL / g, and more preferably 2.3-2.5 dL / g;
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a preparation method of a high molecular weight polyoxamide resin and the obtained high molecular weight polyoxamide resin. Background Art

[0002] Polyamide resin (ie nylon) is a thermoplastic material with a wide variety of types, mainly nylon 6, nylon 66, nylon 1010, nylon 11, nylon 12 and nylon 56. Nylon products are widely used in textile, aviation, automobile, electronics and other fields. Polyamide resin and modified polyamide have a wide operating temperature, good physical properties and wear resistance, high softening point, self-lubrication, oil resistance and general chemical non-toxicity, good electrical insulation, easy processing, and are a promising polymer material.

[0003] Oxalic acid (oxalic acid) is the dibasic acid with the shortest carbon chain. The preparation of polyoxamide resin (oxalic acid nylon) with oxalic acid as the raw material can form dense hydrogen bonds. The two back-to-back amide structures make nylon resin have both the toughness of polyamide and the strength of polyurea. It has excellent barrier performance under high humidity conditions, high temperature resistance, chemical corrosion resistance, high strength and high modulus, and can be used in food packaging sealing, thermoplastic material strength, thermoplastic elastomers and other fields. Compared with general polyamides, polyoxamide has obvious differences in the arrangement, structure and performance of macromolecular chains. Taking advantage of the high melting point and acid and alkali resistance of polyoxamide, it can be used as a component of packaging materials, suitable for rigid packaging applications and multi-level structures. Because polyoxamide has significant resistance to chemical degradation, it can be developed into seawater desalination membrane materials.

[0004] There are dense intermolecular hydrogen bonds inside the polyoxamide polymer (as shown in the figure below), the cohesive energy within the polyoxamide molecule is extremely large, the melting point is high, and the solubility is poor. All of these limit the molecular weight growth of polyoxamide and the processing of polyoxamide molecules.

[0005]

[0006] Higher molecular weight polyoxamides cannot be easily prepared by the conventional Carothers route from diamine oxalates by melt polycondensation because the raw oxalic acid and oligomers are susceptible to thermal decomposition. Similarly, when cyclic oxalamides are used as monomer raw materials, they will also undergo slow thermal decomposition during ring-opening polymerization.

[0007] The early synthesis method of polyoxamide mainly relied on the interfacial polycondensation method. The conditions of interfacial polycondensation are very mild, operating at room temperature and in a short time. The raw material used for interfacial polymerization is oxalyl chloride, which is obtained by reacting with diamine in aqueous solution (LB Sokolov. Synthesis of High Molecular Polyoxamides at a Liquid-Gas Interface, Journal of Polymer Science, 1962, 58 (166): 1253-1261). Some people have also proposed the aminolysis polymerization method of oxalate. The viscosity of the product of the aminolysis polymerization method may be increased by 2 to 3 times, which is suitable for industrial spinning (Dong Jian. Progress in the synthesis and properties of polyoxamide resins [J]. New Chemical Materials, 2011, 39 (11): 16-20).

[0008] Patent CN106220845 A and Cong Cheng et al. (Cong Cheng, Fredrick Nzioka Mutua, Yusheng Dong, Bo Zhu, Yong, He. Bio-based poly (pentamethylene oxamide) synthesized by spray / solid-state polycondensation [J], Polym. Bull. (2018) 75: 121-134) introduced a method for preparing polyoxamide prepolymer by spray drying, in which the catalyst used for spray prepolymerization is potassium iodide, and after the prepolymer is obtained, solid phase polycondensation is performed to obtain polyoxamide. This method of preparing polyoxamide prepolymer by spraying has a low molecular weight because the prepolymer particles are quickly precipitated and separated from the reaction raw materials (oxalic acid diester, diamine), and the molecular weight increases during the subsequent solid phase polycondensation (SSP), and the final prepared PA52 has a relative viscosity of 3.2 and a number average molecular weight of 43000.

[0009] Gaymans et al. introduced a method for synthesizing polyoxamide 42 (RJ Gaymans, VS Venkatraman, J. Schuijer. Preparation and Some Properties of Nylon-4,2 [J]. Journal of Polymer Science: Polymer Chemistry Edition, 1984, 22: 1373-1382). The characteristic viscosity of the polyoxamide 42 synthesized by them is 1.9 (0.5% concentration measured in 96% concentrated sulfuric acid). Its preparation process is to prepare a prepolymer by aminolysis of diethyl oxalate and dibutyleneamine in a mixed solvent of phenol and trichlorobenzene, and then solid condensation at 270°C.

[0010] L. Franco reported a method for polyoxamide 92. (L. Franco, JA Subirana, J. Structure and Morphology of Odd Polyoxamides [Nylon 9,2]. A New Example of Hydrogen-Bonding Interactions in Two Different Directions [J]. Macromolecules 1998, 31, 3912-3924), which uses trifluoroethanol as a solvent to prepare oxalamide 92 prepolymer, and then heats it at 250°C for solid-state polycondensation. The intrinsic viscosity of the final prepared polymer PA92 is 0.10 dL / g. Trifluoroethanol is highly toxic and expensive, and the molecular weight of the final prepared polyoxalamide is limited.

[0011] Japanese patent JP2016121217A introduces a method for preparing polyoxamide, which is prepared by a simple programmed temperature method.

[0012] US Patent No. 2977340 of the United States introduces a method for preparing polyoxamide, which uses a substance containing arsenic, antimony, bismuth and other elements as a catalyst. Patent No. 2704282 introduces a method for preparing polyoxamide, which is to polymerize oxalic acid diester and diamine under the catalysis of phosphoric acid, and the characteristic viscosity of the polyoxamide finally obtained is between 0.25 and 0.5. Summary of the invention

[0013] In order to overcome the problems existing in the prior art, the present invention provides a method for preparing a high molecular weight polyoxamide resin and the obtained high molecular weight polyoxamide resin. The preparation method adopts quinoline solvent and cooperates with the action of metal compounds to achieve the preparation of high molecular weight polyoxamide.

[0014] One of the purposes of the present invention is to provide a method for preparing a high molecular weight polyoxamide resin, comprising: (1) performing a prepolymerization reaction of a diamine compound and oxalic acid and / or an oxalic acid diester in the presence of a quinoline solvent and a metal compound by gradually increasing the temperature, and obtaining a polyoxamide prepolymer by filtering; and (2) performing a solid phase polycondensation reaction of the polyoxamide prepolymer to obtain a high molecular weight polyoxamide resin.

[0015] In a preferred embodiment, the diamine compound is selected from aliphatic diamines, preferably C2-C20 aliphatic diamines, and more preferably at least one selected from 1,5-pentanediamine, 1,4-butanediamine, 1,6-hexanediamine, 2-methylpentanediamine, 1,10-decanediamine, and 1,11-undecanediamine.

[0016] In a further preferred embodiment, based on 100wt% of the quinoline solvent, the amount of the diamine compound is 0.5-20wt%, preferably 1-10wt%, for example, 0.5wt%, 1wt%, 2wt%, 4wt%, 6wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%.

[0017] In a preferred embodiment, the oxalic acid diester is selected from dialkyl oxalate, preferably at least one selected from dimethyl oxalate, diethyl oxalate, dipropyl oxalate, diisopropyl oxalate, and dibutyl oxalate.

[0018] In a preferred embodiment, the molar ratio of the oxalic acid and / or oxalic acid diester to the diamine compound is 1:1.

[0019] In a preferred embodiment, the quinoline solvent is selected from at least one of quinoline and 2-methylquinoline.

[0020] Among them, the inventors have found through a large number of experimental studies that, compared with other polar solvents such as NMP, DMF, DMAc, DMI, etc., when the quinoline solvent is used to prepare polyoxamide, a polyoxamide with a higher molecular weight can be obtained. Preferably, the quinoline solvent is an anhydrous quinoline solvent.

[0021] In a preferred embodiment, based on 100wt% of the quinoline solvent, the amount of the metal compound is 0.5-5wt%, preferably 1-3wt%, for example 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%.

[0022] In a further preferred embodiment, the metal compound is selected from at least one of anhydrous metal chlorides and anhydrous metal nitrate compounds, and / or the metal in the metal compound is selected from at least one of alkali metals, alkaline earth metals and transition metals, preferably transition metals.

[0023] Wherein, the alkali metal is selected from at least one of potassium and lithium, and / or the alkaline earth metal is selected from at least one of calcium, magnesium and barium, and / or the transition metal is selected from zinc.

[0024] In a further preferred embodiment, the metal compound is selected from at least one of anhydrous CaCl2, anhydrous LiCl, and anhydrous ZnCl2, preferably ZnCl2.

[0025] In a preferred embodiment, in step (1), the temperature is gradually increased to 220-280°C, preferably 230-260°C, more preferably 238-248°C, for example 220°C, 230°C, 240°C, 250°C, 260°C, 270°C or 280°C.

[0026] Wherein, the prepolymerization reaction is carried out at a high temperature and the alcohol compound generated by the reaction can be removed at any time.

[0027] In a further preferred embodiment, the prepolymerization reaction time is 5 to 30 h, preferably 10 to 24 h, for example 5 h, 8 h, 10 h, 12 h, 15 h, 18 h, 20 h, 22 h, 25 h, 28 h or 30 h.

[0028] In a preferred embodiment, the filtration is performed as follows: first cooling to room temperature, and then filtering in a dry funnel to prevent the prepolymer from contacting moisture.

[0029] In a preferred embodiment, the prepolymerization reaction in step (1) is carried out as follows: the metal compound is added to the quinoline solvent, and then the diamine compound is added to obtain dispersion liquid 1, and oxalic acid and / or oxalic acid diester is added to the dispersion liquid 1 to carry out the prepolymerization reaction.

[0030] In a further preferred embodiment, the metal compound is added to the quinoline solvent while stirring; and / or oxalic acid and / or oxalic acid diester is added to the dispersion by dropwise addition.

[0031] Among them, oxalic acid diester reacts directly with diamine compound. If they are directly mixed, the reaction will be intensive, and the reaction speed is too fast and may cause explosion.

[0032] In a preferred embodiment, the solid phase polycondensation reaction is carried out under a protective atmosphere, preferably while stirring while introducing a protective gas, and more preferably the protective gas is selected from at least one of nitrogen and an inert gas.

[0033] In a further preferred embodiment, the introduction rate of the protective gas is 20-200 ml / min, preferably 50-150 ml / min, for example 20 ml / min, 50 ml / min, 80 ml / min, 100 ml / min, 120 ml / min, 150 ml / min, 180 ml / min or 200 ml / min.

[0034] In a preferred embodiment, in step (2), the temperature of the solid phase polycondensation reaction is 200-300° C., and the time of the solid phase polycondensation reaction is 30-120 h.

[0035] In a further preferred embodiment, in step (2), the temperature of the solid phase polycondensation reaction is 220-260° C., and the time of the solid phase polycondensation reaction is 48-96 h.

[0036] For example, the temperature of the solid phase polycondensation reaction is 200°C, 220°C, 240°C, 260°C, 280°C or 300°C, and the time of the solid phase polycondensation reaction is 30h, 40h, 50h, 60h, 70h, 80h, 90h, 100h, 110h or 120h.

[0037] In a preferred embodiment, the intrinsic viscosity of the high molecular weight polyoxamide resin is greater than 2 dL / g, preferably 2.1-3 dL / g, more preferably 2.3-2.5 dL / g, for example, 2.1 dL / g, 2.2 dL / g, 2.3 dL / g, 2.4 dL / g, 2.5 dL / g, 2.6 dL / g, 2.7 dL / g, 2.8 dL / g, 2.9 dL / g or 3 dL / g.

[0038] The method of the present invention can be used to obtain high molecular weight polyoxamide resin under mild conditions.

[0039] The second object of the present invention is to provide a high molecular weight polyoxamide resin obtained by the preparation method described in one of the objects of the present invention.

[0040] In a preferred embodiment, the intrinsic viscosity of the high molecular weight polyoxamide resin is greater than 2 dL / g, preferably 2.1-3 dL / g, more preferably 2.3-2.5 dL / g, for example, 2.1 dL / g, 2.2 dL / g, 2.3 dL / g, 2.4 dL / g, 2.5 dL / g, 2.6 dL / g, 2.7 dL / g, 2.8 dL / g, 2.9 dL / g or 3 dL / g.

[0041] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0042] Compared with the prior art, the present invention has the following beneficial effects: the preparation method of the present invention can be used to obtain a high molecular weight polyoxamide resin, the intrinsic viscosity of which is greater than 2dL / g, preferably 2.1-3dL / g, and more preferably 2.3-2.5dL / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The TG graph of PA52 obtained in Example 1 is shown;

[0044] Figure 2 The infrared spectrum of PA52 obtained in Example 1 is shown;

[0045] Figure 3 The infrared spectrum of PA42 obtained in Example 2 is shown;

[0046] Figure 4 The infrared spectrum of PA112 obtained in Example 3 is shown. DETAILED DESCRIPTION

[0047] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0048] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0049] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0050] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0051] [Example 1]

[0052] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 1000g of anhydrous quinoline and stir while adding anhydrous 30.93g of LiCl, then add 10.10g (0.099mol) of refined 1,5-pentanediamine, continue stirring, and then add 14.46g (0.099mol) of diethyl oxalate using a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 222°C. The ethanol generated by the reaction is removed. After reacting for 24 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact moisture to obtain a polyoxamide PA52 prepolymer;

[0053] The polyoxamide PA52 prepolymer was placed in a 0.5L solid phase polycondensation reactor, and nitrogen (50ml / min) was slowly blown in while stirring. The reactor temperature was raised to 220°C, and the solid phase polycondensation was performed for 96 hours. The prepolymer was cooled and discharged to obtain the polyoxamide PA52 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh Thermogravimetric analysis of the product PA52 is 2.4dL / g. Figure 1 .

[0054] Depend on Figure 1 It can be seen that the PA52 obtained in Example 1 has good heat resistance.

[0055] [Example 2]

[0056] In a 5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous 2-methylquinoline and add 35.35g of anhydrous ZnCl2, then add 35.35g (0.401mol) of refined 1,4-butanediamine, continue stirring, and then add 47.38g (0.401mol) of dimethyl oxalate with a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 248°C. The methanol generated by the reaction is removed. After reacting for 36 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact with water to obtain a polyoxamide PA42 prepolymer;

[0057] The polyoxamide PA42 prepolymer was placed in a 0.5L solid phase polycondensation reactor, and nitrogen (100ml / min) was slowly blown in while stirring, and the reactor temperature was raised to 260°C, and solid phase polycondensation was performed for 96 hours, cooled, and discharged to obtain polyoxamide PA42 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 2.4dL / g.

[0058] [Example 3]

[0059] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous 2-methylquinoline and stir while adding 100g of anhydrous CaCl2, then add 184.21g of 1,11-undecanediamine, continue stirring, then add 144.5g (0.989mol) of diethyl oxalate with a dropping funnel, a large number of bubbles are generated in the system, gradually heat up to 248°C, remove the ethanol generated by the reaction, react for 24 hours, cool to room temperature, filter in an anhydrous funnel, control the prepolymer not to contact with water, and obtain polyoxamide PA112 prepolymer;

[0060] The polyoxamide PA112 prepolymer was placed in a 1L solid phase polycondensation reactor, and nitrogen (100 ml / min) was slowly blown in while stirring, and the reactor temperature was raised to 260°C. The solid phase polycondensation was carried out for 90 hours, cooled, and discharged to obtain the polyoxamide PA112 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 2.5dL / g.

[0061] [Example 4]

[0062] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous quinoline and add 89.74g of anhydrous ZnCl2, then add 184.21g (1.804mol) of refined 1,5-pentanediamine, continue stirring, and then add 263.62g (1.804mol) of diethyl oxalate using a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 238°C. The ethanol generated by the reaction is removed. After reacting for 10 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact moisture to obtain a polyoxamide PA52 prepolymer;

[0063] The polyoxamide PA52 prepolymer was placed in a 0.5L solid phase polycondensation reactor, nitrogen was slowly blown in (50ml / min) while stirring, the reactor temperature was raised to 260°C, solid phase polycondensation was performed for 96h, cooled, and discharged to obtain polyoxamide PA52 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 2.2dL / g.

[0064] [Example 5]

[0065] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous methylquinoline and add 53.3g of anhydrous CaCl2, then add 184.21g (1.804mol) of refined 1,0-decanediamine, continue stirring, and then add 213.03g (1.804mol) of dimethyl oxalate using a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 245°C. The methanol generated by the reaction is removed. After reacting for 24 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact with moisture to obtain a polyoxamide PA102 prepolymer;

[0066] The polyoxamide PA102 prepolymer was placed in a 0.5L solid phase polycondensation reactor, and nitrogen (100ml / min) was slowly blown in while stirring, and the reactor temperature was raised to 240°C, and solid phase polycondensation was performed for 96 hours, cooled, and discharged to obtain polyoxamide PA102 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 2.2dL / g.

[0067] [Example 6]

[0068] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous methylquinoline and add 46.1g of anhydrous ZnCl2, then add 184.21g (0.989mol) of 1,11-undecanediamine, continue stirring, and then add 144.5g (0.989mol) of diethyl oxalate with a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 245°C. The ethanol generated by the reaction is removed. After reacting for 28 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact with moisture to obtain a polyoxamide PA112 prepolymer;

[0069] The polyoxamide PA112 prepolymer was placed in a 1L solid phase polycondensation reactor, and nitrogen (100 ml / min) was slowly blown in while stirring, and the reactor temperature was raised to 230°C, and solid phase polycondensation was performed for 96 hours, cooled, and discharged to obtain polyoxamide PA112 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 2.3dL / g.

[0070] [Comparative Example 1]

[0071] In a 5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous NMP and stir while adding anhydrous 108.25g of CaCl2, then add 38.89g (0.335mol) of 2-methyl-1,5-pentanediamine, continue stirring, and then add 48.94g (0.335mol) of diethyl oxalate with a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 202°C. The ethanol generated by the reaction is removed. After reacting for 24 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact moisture to obtain a polyoxamide PAM52 prepolymer;

[0072] The polyoxamide PAM52 prepolymer was placed in a 1L solid phase polycondensation reactor, and nitrogen was slowly blown in (100 / min) while stirring, and the reactor temperature was raised to 220°C. The solid phase polycondensation was performed for 48 hours, cooled, and discharged to obtain the polyoxamide PAM52 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 1.3dL / g.

[0073] [Comparative Example 2]

[0074] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, 1000g of anhydrous DMAc was added, and 20.41g of anhydrous LiCl was added while stirring, and then 52.3g (0.306mol) of 10-decanediamine was added, and stirring was continued. Then, 36.1g (0.306mol) of dimethyl oxalate was added with a dropping funnel, and a large number of bubbles were generated in the system. The temperature was gradually raised to 165°C, and the methanol generated by the reaction was removed. After reacting for 36 hours, the system was cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact with water, thereby obtaining a polyoxamide PA102 prepolymer;

[0075] The polyoxamide PA102 prepolymer was placed in a 0.5L solid phase polycondensation reactor, and nitrogen was slowly blown in (150 / min) while stirring. The reactor temperature was raised to 255°C, and the solid phase polycondensation was performed for 48 hours. The prepolymer was cooled and discharged to obtain the polyoxamide PA102 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 1.1dL / g.

[0076] [Comparative Example 3]

[0077] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous DMF and stir while adding anhydrous 46.1g of ZnCl2, then add 184.21g (0.989mol) of 1,11-undecanediamine, continue stirring, then add 144.5g (0.989mol) of diethyl oxalate with a dropping funnel, a large number of bubbles are generated in the system, gradually heat up to 140°C, remove the ethanol generated by the reaction, react for 28 hours, cool to room temperature, filter in an anhydrous funnel, control the prepolymer not to contact with water, and obtain polyoxamide PA112 prepolymer;

[0078] The polyoxamide PA112 prepolymer was placed in a 1L solid phase polycondensation reactor, and nitrogen was slowly blown in (100 / min) while stirring. The reactor temperature was raised to 230°C, and solid phase polycondensation was performed for 96 hours. The prepolymer was cooled and discharged to obtain the polyoxamide PA112 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 0.8dL / g.

[0079] [Comparative Example 4]

[0080] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 1000g of anhydrous DMAc, then add 26.98g (0.306mol) of 1,4-diamine, continue stirring, and then add 36.1g (0.306mol) of dimethyl oxalate using a dropping funnel. A large number of bubbles are generated in the system, and the temperature is gradually raised to 165°C. The methanol generated by the reaction is removed. After reacting for 36 hours, it is cooled to room temperature and filtered in a dry funnel to control the prepolymer not to contact with moisture to obtain a polyoxamide PA42 prepolymer;

[0081] The polyoxamide PA42 prepolymer was placed in a 0.5L solid phase polycondensation reactor, nitrogen was slowly blown in (150 / min) while stirring, the reactor temperature was raised to 255°C, solid phase polycondensation was performed for 48 hours, cooled, and discharged to obtain polyoxamide PA102 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 0.5dL / g.

[0082] [Comparative Example 5]

[0083] In a 2.5L dry and anhydrous four-necked flask equipped with an air condenser, add 3500g of anhydrous DMF, then add 184.21g (0.989mol) of 1,11-undecanediamine, continue stirring, then add 144.5g (0.989mol) of diethyl oxalate using a dropping funnel, a large number of bubbles are generated in the system, gradually heat up to 145°C, remove the ethanol generated by the reaction, react for 28 hours, cool to room temperature, filter in a dry funnel, control the prepolymer not to contact with water, and obtain polyoxamide PA112 prepolymer;

[0084] The polyoxamide PA112 prepolymer was placed in a 1L solid phase polycondensation reactor, and nitrogen was slowly blown in (100 / min) while stirring. The reactor temperature was raised to 230°C, and solid phase polycondensation was performed for 96 hours. The prepolymer was cooled and discharged to obtain the polyoxamide PA112 resin. The intrinsic viscosity η of the polymer was measured at 25°C using an Ubbelohde viscometer. inh It is 0.4dL / g.

[0085] It can be seen from the above Examples 1 to 6 and Comparative Examples 1 to 5 that the polyoxamide resin with a higher molecular weight can be obtained by adopting the technical solution of the present invention (under the combined action of quinoline solvent and metal compound).

[0086] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a high molecular weight polyoxamide resin, comprising: (1) a diamine compound and oxalic acid and / or oxalic acid diester are prepolymerized by gradually increasing the temperature in the presence of a quinoline solvent and a metal compound, and a polyoxamide prepolymer is obtained by filtration; and (2) the polyoxamide prepolymer is subjected to a solid phase polycondensation reaction to obtain a high molecular weight polyoxamide resin.

2. The preparation method according to claim 1, characterized in that: The diamine compound is selected from aliphatic diamines, preferably C2-C20 aliphatic diamines, more preferably at least one selected from 1,5-pentanediamine, 1,4-butanediamine, 1,6-hexanediamine, 2-methylpentanediamine, 1,10-decanediamine, and 1,11-undecanediamine; Preferably, based on 100 wt % of the quinoline solvent, the amount of the diamine compound is 0.5 to 20 wt %, preferably 1 to 10 wt %.

3. The preparation method according to claim 1, characterized in that: The oxalic acid diester is selected from dialkyl oxalate, preferably at least one selected from dimethyl oxalate, diethyl oxalate, dipropyl oxalate, diisopropyl oxalate, and dibutyl oxalate; preferably, the molar ratio of the oxalic acid and / or oxalic acid diester to the diamine compound is 1:

1.

4. The preparation method according to claim 1, characterized in that: The quinoline solvent is selected from at least one of quinoline and 2-methylquinoline.

5. The preparation method according to claim 1, characterized in that: The metal compound is selected from at least one of anhydrous metal chloride and anhydrous metal nitrate; and / or, The metal in the metal compound is selected from at least one of alkali metals, alkaline earth metals and transition metals; preferably, the alkali metal is selected from at least one of potassium and lithium, and / or the alkaline earth metal is selected from at least one of calcium, magnesium and barium, and / or the transition metal is selected from zinc.

6. The preparation method according to claim 1, characterized in that: In step (1), gradually raising the temperature to 220-280°C, preferably to 230-260°C, more preferably to 238-248°C; and / or, The prepolymerization reaction time is 5 to 30 hours, preferably 10 to 24 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The prepolymerization reaction in step (1) is carried out as follows: the metal compound is added to the quinoline solvent, and then the diamine compound is added to obtain a dispersion liquid 1, and oxalic acid and / or oxalic acid diester is added to the dispersion liquid 1 to carry out the prepolymerization reaction.

8. The preparation method according to claim 7, characterized in that: The solid phase polycondensation reaction in step (2) is carried out under a protective atmosphere, preferably while stirring while introducing a protective gas, more preferably the protective gas is selected from at least one of nitrogen and an inert gas.

9. The preparation method according to claim 8, characterized in that: In step (2), The temperature of the solid phase polycondensation reaction is 200-300°C, preferably 220-260°C; and / or, The solid phase polycondensation reaction time is 30-120 hours, preferably 48-96 hours.

10. A high molecular weight polyoxamide resin obtained by the preparation method according to any one of claims 1 to 9.

11. The high molecular weight polyoxamide resin according to claim 10, characterized in that: The intrinsic viscosity of the high molecular weight polyoxamide resin is greater than 2 dL / g, preferably 2.1 to 3 dL / g, and more preferably 2.3 to 2.5 dL / g.

Citation Information

Patent Citations

  • Preparation method of soluble, colorless, transparent and low-thermal-expansion-coefficient polyamide imide film

    CN105017534A

  • Semi-aromatic polyamide resin and preparation method thereof

    CN112646173A

  • Colorless transparent polyimide film, preparation method thereof and polyimide hardened film

    CN113061269A

  • Improvements in or relating to synthetic linear polyamides

    GB584561A

  • Production of polyamide

    JP1992311723A